Method for preparing high-hardness hydrophobic SiO2 antireflection film by mixing acid catalysis sol and base catalysis sol

High-hardness hydrophobic SiO2 antireflective films were prepared by mixing acid-catalyzed and alkali-catalyzed sols, which solved the problems of insufficient hardness, adhesion and transmittance in the existing technology and achieved film effects with high transmittance, strong adhesion and high hardness.

CN118724475AActive Publication Date: 2024-10-01TIANJIN POLYTECHNIC UNIV

Patent Information

Application Number
CN202310318110.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01
Estimated Expiration
2043-03-29

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a preparation method for preparing a high-hardness hydrophobic SiO2 antireflection film by mixing acid catalysis and base catalysis sol. Tetraethyl orthosilicate (TEOS) and methyltriethoxysilane (MTES) are used as precursors, absolute ethyl alcohol is used as a solvent, fatty alcohol-polyoxyethylene ether (AEO) is used as a pore-foaming agent, hydrochloric acid and ammonia water are respectively used as catalysts to prepare acid-catalyzed silica sol and base-catalyzed silica sol, the two kinds of silica sol are mixed in proportion, glass is coated with the mixed sol through a dipping-pulling method and the like, and the silica sol-coated glass is prepared. And drying and annealing to form the porous nano film. The average transmittance (coated glass transmittance) of the antireflection film in the range of 400-1100nm is 92.51%, which is improved by 5.17% compared with that of blank glass; the water contact angle of the film is 91 degrees, the hardness of a pencil method reaches 7H, and the adhesive force of an adhesive tape method reaches the highest level of 0; and after 100 hours of ultraviolet irradiation, the transmittance change is only 1.1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anti-reflection film materials, and in particular relates to a method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing acid-catalyzed and base-catalyzed sols. Background Art

[0002] Anti-reflection films are widely used in the field of solar cells. Most solar panels serve outdoors or in the wild in relatively harsh environments. In addition to light transmittance, anti-reflection films must also have high mechanical properties (adhesion, hardness, etc.), good weather resistance (anti-ultraviolet radiation, etc.) and certain self-cleaning capabilities.

[0003] Using tetraethyl orthosilicate as a precursor, silica sol can be prepared by base catalysis or acid catalysis, and then coated on the glass surface by dip-coating to obtain an anti-reflection film. The base-catalyzed SiO2 film has excellent anti-reflection performance due to its high porosity, but the bonding force between its particles and between the particles and the substrate is very weak, and it is easy to break or fall off the substrate. The acid-catalyzed SiO2 has a linear chain structure, and chemical bonds can be formed between the particles and between the particles and the substrate, and it has strong adhesion, but its porosity is low and the anti-reflection performance is poor.

[0004] In order to make the sol-gel anti-reflection film obtain high mechanical properties and self-cleaning properties, some explorations have been carried out. Wang et al. [Chemical Physics Letters.2020, 747:137331] mixed alkaline sols of different particle sizes to prepare a SiO2 film with a concave-convex structure. The average transmittance at 380-1100nm was 97.55%, and the contact angle was 141.38°, but its hardness and adhesion were not studied. Zhi et al. [Applied surface science.2018, 454:239-248] synthesized a high anti-reflection super-hydrophobic film with a dual-scale structure by introducing SiO2 nanoparticles into the nanoporous structure. The transmittance was increased by 7 percentage points, the contact angle was 157.9°, and the surface pencil hardness was 4H, but the adhesion was not characterized. Yuan et al. [Solar energy. 2017, 155: 1366-1372] used ammonia to catalyze TEOS in the early stage of spherical SiO2 growth. After a period of time, hydrochloric acid was used as a catalyst to change the environment to acidic. As a result, the pencil hardness of the coating was 2B, and the average transmittance increased by 6.3 percentage points. Then, polymethylhydrogensiloxane (PMHS) was used for surface treatment, and the pencil hardness was further increased to 5H. Adhesion and wettability were not characterized. Ye et al. [Solar energy materials and solar cells. 2011, 95 (8): 2347-2351] used tetraethyl silicate as a precursor and an acid / base two-step catalytic sol-gel method to prepare an antireflection film with high transmittance and high wear resistance. Then, hexamethyldisilazane was used for surface modification. When the acid / base catalytic sol molar ratio was 0.5, the contact angle was 72.51°, and the maximum transmittance at 630nm increased by 6.5 percentage points. The hardness and adhesion of the film were not characterized.

[0005] Chinese patent CN 107863393 A discloses a method for preparing solar photovoltaic glass with a micro / nano anti-reflection layer. The solar photovoltaic glass with a micro / nano anti-reflection layer is prepared by plasma etching and nanoimprinting, and the transmittance is increased by 3 percentage points, and the contact angle is 119°. This method requires the use of photoresist and vacuum imprinting equipment. Chinese patent CN112442669 A discloses a method for preparing a self-cleaning anti-reflection film. First, a film is plated on the glass surface by magnetron sputtering, and then a SiO2 film is obtained by etching with a specific solution. The refractive index of the silicon dioxide crystalline film is 1.21-1.32, and the water contact angle is 137-141°, but the hardness and adhesion of the film are not characterized, and this method is complex. Chinese patent CN 112661415 A discloses an anti-reflection film for photovoltaic glass and its preparation method. The anti-reflection film is composed of an anti-reflection main layer close to the glass substrate and an anti-reflection auxiliary layer arranged on the anti-reflection main layer. The transmittance of the anti-reflection film is increased by 3%, and the pencil hardness is 5H. The adhesion and contact angle are not characterized. Chinese patent CN 113387597 B discloses a super-hydrophobic anti-reflection film and photovoltaic glass. A layer of base-catalyzed nano-SiO2 sol is coated on the surface of K9 photovoltaic glass by an immersion-pulling method. The transmittance of the anti-reflection film is 94.7% and the contact angle is 156.7°, but the hardness and adhesion of the film are not studied. Chinese patent CN 109502987 B discloses a method for preparing a high-hardness anti-reflection film based on hollow silicon oxide. The method uses tetraethyl orthosilicate as a raw material, polyacrylic acid as a template agent, 2-isopropoxyethanol and methanol as solvents, and ammonia water as a catalyst. The hollow SiO2 sol is prepared by a template method, and the coating is plated on a glass substrate by an immersion-pulling method. After calcination at 550°C, the obtained film has an average transmittance of more than 98% in the wavelength range of 400-800nm, but the hardness is only 4H, and the adhesion and wettability of the film are not characterized. Chinese patent CN 105399340 A discloses a super-hydrophobic high-transmittance anti-reflection film and a preparation method thereof. A hybrid sol doped with trimethylchlorosilane is prepared, and a coating is formed on the surface of a glass slide by an immersion-pulling method. After drying, a super-hydrophobic high-transmittance anti-reflection film is obtained, and the transmittance is increased by 5.56 percentage points, and the contact angle is 106°. The hardness and adhesion of the film are not tested. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing acid-catalyzed and base-catalyzed sols. The anti-reflection film prepared by the present invention has high transmittance, high hardness, high adhesion and hydrophobicity. The average transmittance in the wavelength range of 400 to 1100 nm is 92.51%, which is 5.17 percentage points higher than the average transmittance of blank glass. The water contact angle of the anti-reflection film can reach 91°, the adhesion of the film is the highest level 0 of the tape method, the surface hardness reaches 7H of the pencil method, and the transmittance changes to 1.1% after 100 hours of ultraviolet irradiation.

[0007] In order to solve the technical problem of the present invention, the technical solution adopted is a method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing acid-catalyzed and base-catalyzed sols. The specific operation steps are as follows:

[0008] S1. Preparation of acid-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and concentrated hydrochloric acid are added to a pre-cleaned beaker in a volume ratio of 1: (0.1-3.0): 10: 0.3: (0.1-0.5) in sequence, stirred at room temperature for 1-5 hours at a speed of 200-1000 r / min, transferred to a conical flask and placed in a water bath at 50-100° C. for 1-5 hours, and AEO is added to the sol and mixed, wherein the volume ratio of AEO to silane (tetraethyl silicate + methyltriethoxysilane) is 0.1-45%, aged for 1-5 days, and the desired acid-catalyzed silica sol is obtained;

[0009] S2. Preparation of base-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol and ammonia water are added into a pre-cleaned beaker in a volume ratio of 1:(0.1-3.0):15:(0.1-0.7) in sequence, stirred at room temperature for 0.5-12h at a speed of 200-1000r / min, aged for 1-5 days, and the desired base-catalyzed silica sol is obtained;

[0010] S3. Preparation of mixed sol: reflux the base-catalyzed silica sol in a water bath at 50-100° C. for 6-24 hours, cool to room temperature, mix the acid-catalyzed silica sol with the base-catalyzed silica sol at a volume ratio of 5-95%, stir at room temperature for 1-5 hours, and age for 12-72 hours to obtain the desired mixed sol.

[0011] S4. Preparation of anti-reflection film: Use immersion-pulling method for coating, with a pulling speed of 100-3000 μm / s, move the coated glass substrate into an oven at 50-80°C for drying for 1-5 hours, then move it into a muffle furnace and keep it at 300-500°C for 1-5 hours, then cool it naturally to obtain a mixture of acid-catalyzed and base-catalyzed sols to prepare a high-hardness hydrophobic SiO2 anti-reflection film. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 The transmittance spectrum (a) and average transmittance (b) of a high-hardness hydrophobic SiO2 anti-reflection film prepared by mixing acid-catalyzed and base-catalyzed sols provided in an embodiment of the present invention are shown.

[0013] Figure 2 The contact angle of the high-hardness hydrophobic SiO2 anti-reflection film prepared by mixing the acid-catalyzed and base-catalyzed sols provided in the embodiment of the present invention varies with the volume ratio of the acid-catalyzed silica sol to the base-catalyzed silica sol.

[0014] Figure 3 This is an adhesion diagram of a high-hardness hydrophobic SiO2 anti-reflection film prepared by mixing the acid-catalyzed and base-catalyzed sols provided in the embodiments of the present invention; the volume ratios of the acid-catalyzed silica sol to the base-catalyzed silica sol are (a) 0%, (b) 10%, (c) 20%, (d) 30%, and (e) 40%, respectively; the adhesion of the film was tested according to "GB / T 6379-2006", and the figure shows scratches made by a hundred-grid knife, from which it can be judged that the adhesion of the second to fifth embodiments reaches level 0.

[0015] Figure 4 This is a surface hardness diagram of a high-hardness hydrophobic SiO2 anti-reflection film prepared by mixing the acid-catalyzed and base-catalyzed sols provided in an embodiment of the present invention; the volume ratios of the acid-catalyzed silica sol and the base-catalyzed silica sol are (a) and (b) 0, (c) and (d) 30%, respectively; the surface hardness of the film is tested according to "GB / T 33049-2016", and the figure shows the scratches of an 8H pencil, from which it can be judged that the hardness of the second and fifth embodiments reaches 7H. DETAILED DESCRIPTION

[0016] The invention discloses a method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing acid-catalyzed and base-catalyzed sols. The SiO2 anti-reflection film is prepared by mixing acid-catalyzed silica sol and base-catalyzed silica sol.

[0017] The present invention is described in further detail below in conjunction with embodiments:

[0018] Embodiment 1:

[0019] In order to compare the modification effect of acid-catalyzed silica sol, a base-catalyzed SiO2 anti-reflection film was first prepared, and the preparation method thereof included the following steps:

[0020] 1. Preparation of base-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and ammonia water are added into a pre-cleaned beaker in a volume ratio of 1:1:15:0.5 in sequence, stirred at room temperature for 0.5-12h at a speed of 200-1000r / min, aged for 1-5 days, and the desired base-catalyzed silica sol is obtained;

[0021] 2. Preparation of anti-reflection film: Use the immersion-pulling method for coating, with a pulling speed of 100-3000 μm / s. Move the coated glass substrate into an oven at a temperature of 50-80°C for drying for 1-5 hours, then move it into a muffle furnace and keep it at 300-500°C for 1-5 hours, then cool it naturally to obtain an alkali-catalyzed SiO2 anti-reflection film.

[0022] Embodiment 2:

[0023] A method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing acid-catalyzed and base-catalyzed sols comprises the following steps:

[0024] 1. Preparation of acid-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and concentrated hydrochloric acid are added to a pre-cleaned beaker in a volume ratio of 1:1:10:0.3:0.3 in sequence, stirred at a speed of 200-1000r / min for 1-5h, transferred to a conical flask and placed in a water bath at 50-100°C for 1-5h, AEO is added to the sol and mixed, wherein the volume ratio of AEO to Si (TEOS+MTES) is 45%, aged for 1-5 days, and the desired acid-catalyzed silica sol is obtained;

[0025] 2. Preparation of base-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol and ammonia water are added into a pre-cleaned beaker in a volume ratio of 1:1:15:0.5, stirred at a speed of 200-1000r / min for 0.5-12h, aged for 1-5 days, and the desired base-catalyzed silica sol is obtained;

[0026] 3. Preparation of mixed sol: reflux the base-catalyzed silica sol in a water bath at 50-100°C for 6-24h, cool to room temperature, mix the acid-catalyzed silica sol with the base-catalyzed silica sol at a volume ratio of 10%, stir at room temperature for 1-5h, and age for 12-72h to obtain the desired mixed sol.

[0027] 4. Preparation of anti-reflection film: Use the immersion-pulling method for coating, with a pulling speed of 100-3000 μm / s. Move the coated glass substrate into an oven at a temperature of 50-80°C and dry it for 1-5 hours. Then move it into a muffle furnace and keep it at 300-500°C for 1-5 hours. Then cool it naturally to obtain a mixture of acid-catalyzed and base-catalyzed sols to prepare a high-hardness hydrophobic SiO2 anti-reflection film.

[0028] Embodiment three:

[0029] A method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing acid-catalyzed and base-catalyzed sols comprises the following steps:

[0030] 1. Preparation of acid-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and concentrated hydrochloric acid are added to a pre-cleaned beaker in a volume ratio of 1:1:10:0.3:0.3 in sequence, stirred at a speed of 200-1000r / min for 1-5h, transferred to a conical flask and placed in a water bath at 50-100°C for 1-5h, AEO is added to the sol and mixed, wherein the volume ratio of AEO to Si (TEOS+MTES) is 45%, aged for 1-5 days, and the desired acid-catalyzed silica sol is obtained;

[0031] 2. Preparation of base-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol and ammonia water are added into a pre-cleaned beaker in a volume ratio of 1:1:15:0.5, stirred at a speed of 200-1000r / min for 0.5-12h, aged for 1-5 days, and the desired base-catalyzed silica sol is obtained;

[0032] 3. Preparation of mixed sol: reflux the base-catalyzed silica sol in a water bath at 50-100°C for 6-24h, cool to room temperature, mix the acid-catalyzed silica sol with the base-catalyzed silica sol at a volume ratio of 20%, stir at room temperature for 1-5h, and age for 12-72h to obtain the desired mixed sol.

[0033] 4. Preparation of anti-reflection film: Use the immersion-pulling method for coating, with a pulling speed of 100-3000 μm / s. Move the coated glass substrate into an oven at a temperature of 50-80°C and dry it for 1-5 hours. Then move it into a muffle furnace and keep it at 300-500°C for 1-5 hours. Then cool it naturally to obtain a mixture of acid-catalyzed and base-catalyzed sols to prepare a high-hardness hydrophobic SiO2 anti-reflection film.

[0034] Embodiment 4:

[0035] A method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing acid-catalyzed and base-catalyzed sols comprises the following steps:

[0036] 1. Preparation of acid-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and concentrated hydrochloric acid are added to a pre-cleaned beaker in a volume ratio of 1:1:10:0.3:0.3 in sequence, stirred at a speed of 200-1000r / min for 1-5h, transferred to a conical flask and placed in a water bath at 50-100°C for 1-5h, AEO is added to the sol and mixed, wherein the volume ratio of AEO to Si (TEOS+MTES) is 45%, aged for 1-5 days, and the desired acid-catalyzed silica sol is obtained;

[0037] 2. Preparation of base-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol and ammonia water are added into a pre-cleaned beaker in a volume ratio of 1:1:15:0.5, stirred at a speed of 200-1000r / min for 0.5-12h, aged for 1-5 days, and the desired base-catalyzed silica sol is obtained;

[0038] 3. Preparation of mixed sol: reflux the base-catalyzed silica sol in a water bath at 50-100°C for 1-5 hours, cool to room temperature, mix the acid-catalyzed silica sol with the base-catalyzed silica sol at a volume ratio of 30%, stir at room temperature for 1-5 hours, and age for 12-72 hours to obtain the desired mixed sol.

[0039] 4. Preparation of anti-reflection film: Use the immersion-pulling method for coating, with a pulling speed of 100-3000 μm / s. Move the coated glass substrate into an oven at a temperature of 50-80°C and dry it for 1-5 hours. Then move it into a muffle furnace and keep it at 300-500°C for 1-5 hours. Then cool it naturally to obtain a mixture of acid-catalyzed and base-catalyzed sols to prepare a high-hardness hydrophobic SiO2 anti-reflection film.

[0040] Embodiment five:

[0041] A method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing acid-catalyzed and base-catalyzed sols comprises the following steps:

[0042] 1. Preparation of acid-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and concentrated hydrochloric acid are added to a pre-cleaned beaker in a volume ratio of 1:1:10:0.3:0.3 in sequence, stirred at a speed of 200-1000r / min for 1-5h, transferred to a conical flask and placed in a water bath at 50-100°C for 1-5h, AEO is added to the sol and mixed, wherein the volume ratio of AEO to Si (TEOS+MTES) is 45%, aged for 1-5 days, and the desired acid-catalyzed silica sol is obtained;

[0043] 2. Preparation of base-catalyzed silica sol: tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol and ammonia water are added into a pre-cleaned beaker in a volume ratio of 1:1:15:0.5, stirred at a speed of 200-1000r / min for 0.5-12h, aged for 1-5 days, and the desired base-catalyzed silica sol is obtained;

[0044] 3. Preparation of mixed sol: reflux the base-catalyzed silica sol in a water bath at 50-100°C for 1-5 hours, cool to room temperature, mix the acid-catalyzed silica sol with the base-catalyzed silica sol at a volume ratio of 40%, stir at room temperature for 1-5 hours, and age for 12-72 hours to obtain the desired mixed sol.

[0045] 4. Preparation of anti-reflection film: Use the immersion-pulling method for coating, with a pulling speed of 100-3000 μm / s. Move the coated glass substrate into an oven at a temperature of 50-80°C and dry it for 1-5 hours. Then move it into a muffle furnace and keep it at 300-500°C for 1-5 hours. Then cool it naturally to obtain a mixture of acid-catalyzed and base-catalyzed sols to prepare a high-hardness hydrophobic SiO2 anti-reflection film.

[0046] Acid-catalyzed silica sol changes the transmittance of SiO2 film. As the amount of acid-catalyzed silica sol increases, more pores can be formed after annealing, and the transmittance gradually increases. Figure 1 -The transmittance spectrum of the film is shown in the figure.

[0047] Acid-catalyzed silica sol changes the wettability of SiO2 film. With the increase of acid-catalyzed silica sol, the roughness of the film increases and the contact angle increases. When there is too much acid-catalyzed silica sol, the particles of the film are occupied by acid-catalyzed SiO2 particles, the roughness decreases, and the contact angle decreases. Figure 2 -Schematic diagram of the contact angle of the film.

[0048] Acid-catalyzed silica sol changes the adhesion and hardness of SiO2 film. With the increase of acid-catalyzed silica sol, the chemical bonds between particles increase, and the adhesion and hardness are improved. Figure 3 and Figure 4 .

[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing acid-catalyzed and base-catalyzed sols, characterized in that: Acid-catalyzed silica sol and base-catalyzed silica sol were prepared using tetraethyl silicate (TEOS) and methyltriethoxysilane (MTES) as precursors and anhydrous ethanol as solvent, and hydrochloric acid and ammonia water as catalysts respectively. Fatty alcohol polyoxyethylene ether (AEO) was added to the acid-catalyzed silica sol as a porogen. The acid-catalyzed silica sol and the base-catalyzed silica sol were mixed in a volume ratio of 5 to 95% to prepare a mixed sol, which was then coated on glass by a dip-pulling method. During annealing, the AEO inside the coating volatilized to form a micro-nano pore structure, and a high-hardness hydrophobic SiO2 anti-reflection film was obtained after annealing.

2. A method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing an acid-catalyzed and a base-catalyzed sol according to claim 1, characterized in that: The preparation method of the acid-catalyzed and base-catalyzed mixed sol is as follows: S1. Preparation of acid-catalyzed silica sol: TEOS, MTES, anhydrous ethanol, deionized water and concentrated hydrochloric acid are added to a pre-cleaned beaker in a volume ratio of 1: (0.1-3.0): 10: 0.3: (0.1-0.5) in sequence, stirred at a speed of 200-1000 r / min for 1-5 hours, then transferred to a conical flask and placed in a water bath at 50-100° C. for 1-5 hours, AEO is added to the sol and mixed, wherein the volume ratio of AEO to silane (TEOS+MTES) is 0.1-45%, aged for 1-5 days, and the desired acid-catalyzed silica sol is obtained; S2. Preparation of base-catalyzed silica sol: TEOS, MTES, anhydrous ethanol and ammonia water are added into a pre-cleaned beaker in a volume ratio of 1:(0.1-3.0):15:(0.1-0.7) in sequence, stirred at a speed of 200-1000 r / min for 0.5-12 h, aged for 1-5 days, and the desired base-catalyzed silica sol is obtained; S3. Preparation of mixed sol: reflux the base-catalyzed silica sol in a water bath at 50-100° C. for 6-24 hours and cool to room temperature, then mix the acid-catalyzed silica sol and the base-catalyzed silica sol in a volume ratio of 5-95%, stir at room temperature for 1-5 hours, and age for 12-72 hours to obtain the desired mixed sol.

3. A method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing an acid-catalyzed and a base-catalyzed sol according to claim 2, characterized in that: The mixed sol is coated on the glass by the dipping-pulling method, and the pulling speed is 10-3000 μm / s. The coated glass substrate is moved into an oven with a temperature of 50-80°C, dried for 1-5 hours, and then moved into a muffle furnace and annealed at 200-500°C for 1-5 hours to obtain a high-hardness hydrophobic SiO2 anti-reflection film prepared by mixing acid-catalyzed and base-catalyzed sols.

4. A method for preparing a high-hardness hydrophobic SiO2 anti-reflection film by mixing an acid-catalyzed and a base-catalyzed sol according to claim 3, characterized in that: The film exhibits excellent anti-reflection effect in the visible light range (400-1100nm), with an average transmittance of 92.51% in the wavelength range of 400-1100nm, which is 5.17 percentage points higher than that of blank glass; the anti-reflection film has a certain hydrophobic self-cleaning function, and the water contact angle reaches 91°; it has good mechanical properties, the adhesion is the highest level 0 by the tape method, and the surface hardness reaches 7H by the pencil method; the transmittance changes by 1.1% after 100h of strong ultraviolet irradiation; the method for preparing the film is simple, low-cost, suitable for large-area coating, and easy to promote industrialization.

Citation Information

Patent Citations

  • Method for preparing porous silicon dioxide antireflective film with controllable refractive index

    CN101531468A

  • Preparation of disordered porous silicon dioxide material and application of fatty alcohol-polyoxyethylene ether to preparation of disordered porous silicon dioxide material

    CN102807225A

  • Method for preparing antireflection film from doped silica (SiO2) sol

    CN103613279A

  • Preparation method of modified porous silicon dioxide anti-reflection coating

    CN104230178A

  • Preparation method of damp and heat-resistant anti-reflection coating with high strength

    CN106291779A

Cited By

  • Photovoltaic glass surface hydrophobic treatment process

    CN120887655A

  • Photovoltaic glass surface hydrophobic treatment process

    CN120887655B

  • Low-reflection anti-dazzle high-transmission conductive glass and preparation method thereof

    CN122145046A