Manganese slag treatment method, application thereof and magnesium oxide board

Through the wet mixing of manganese slag, magnesium salt and magnesium oxide, a mixed gel is formed, which solves the pollution problem in the treatment of manganese slag, realizes the harmlessness and resource utilization of manganese slag, and prepares glassware that meets environmental protection requirements. Magnesium sheet.

CN118724487AInactive Publication Date: 2024-10-01GUANGZHOU GUANGHE LIGHT STEEL PRODUCTS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410801377.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Manganese slag treatment involves dust pollution, leakage risks and heavy metal pollution, and it is difficult to achieve harmlessness and resource utilization with existing technology.

Method used

By wet mixing manganese slag, magnesium salt and magnesium oxide to form a mixed gel, the magnesium oxide converts ammonium sulfate into magnesium sulfate and ammonia gas, and converts the soluble manganese source into manganese oxide to form a gel suitable for preparing glass magnesium sheets. Mix the gel.

Benefits of technology

The harmless treatment and resource utilization of manganese slag are achieved. The prepared glass magnesium plates meet environmental protection and quality requirements and reduce the migration and diffusion of pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724487A_ABST
    Figure CN118724487A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of industrial waste residue treatment, and provides a manganese residue treatment method and application thereof and a glass magnesium planes.The manganese residue treatment method comprises the steps that a mixed solution containing manganese residues, magnesium salt, magnesium oxide and water is stirred, the magnesium oxide reacts to remove ammonium sulfate in the manganese residues, and a soluble manganese source contained in the manganese residues is converted into manganese oxide; the mixed gel comprises magnesium salt, magnesium oxide, magnesium sulfate and a manganese-containing compound, and the manganese-containing compound comprises manganese oxide. The magnesium oxide and the magnesium salt are utilized to form a gel system, the magnesium oxide can convert ammonium sulfate in the manganese slag into magnesium sulfate and ammonia gas, and the magnesium sulfate can be used as the magnesium salt; and a gel environment formed by magnesium oxide and magnesium salt can react and convert a soluble manganese source in the manganese slag into manganese oxide, so that harmless treatment of the manganese slag is realized. In addition, the formed mixed gel can be used as a preparation raw material of the magnesium oxide board, and the prepared magnesium oxide board meets environmental protection requirements and quality requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of industrial waste slag treatment, and in particular to a manganese slag treatment method and application thereof and a glass magnesium plate. Background Art

[0002] Manganese is an important raw material for metallurgical and chemical production, and is widely used in new energy and new materials. Since most manganese production adopts wet electrolysis process, the amount of slag discharged for every ton of electrolytic manganese is 7t~9t, which is the main industrial solid waste in the electrolytic manganese industry. The main treatment method for electrolytic manganese slag is to build a special slag warehouse for storage and treatment, which not only occupies a large amount of land area, but also easily causes dust pollution. Most importantly, the slag warehouse is prone to leakage and lateral seepage. The acidic manganese slag containing heavy metal ions leaks through rainwater leaching and surface runoff infiltration, polluting the surrounding surface water, groundwater and soil. Therefore, it is extremely important to harmlessly treat and recycle manganese slag. Summary of the invention

[0003] Based on this, an embodiment of the present application provides a harmless and resource-based manganese slag treatment method and its application and a glass magnesium plate.

[0004] In a first aspect, the present application provides a method for treating manganese slag, the method comprising:

[0005] Stirring a mixed solution containing manganese slag, magnesium salt, magnesium oxide and water, wherein the magnesium oxide reacts to remove ammonium sulfate in the manganese slag and converts a soluble manganese source contained in the manganese slag into manganese oxide;

[0006] A mixed gel including magnesium salt, magnesium oxide, magnesium sulfate and a manganese-containing compound is obtained, and the manganese-containing compound contained in the mixed gel includes manganese oxide.

[0007] In some embodiments, the mass percentage of the manganese source contained in the manganese slag is 10% to 20%.

[0008] In some embodiments, the soluble manganese source includes at least one of manganese sulfate and manganese carbonate.

[0009] In some embodiments, the mass ratio of the manganese slag to the magnesium oxide is (0.3~0.5):1.

[0010] In some embodiments, the mass ratio of the magnesium salt to the magnesium oxide is (0.4-0.6):1.

[0011] In some embodiments, the manganese slag treatment method further includes: recovering ammonia gas generated by the reaction of the magnesium oxide and the ammonium sulfate.

[0012] In some embodiments, the stirring speed is 250 rpm to 1500 rpm, the temperature is 30° C. to 40° C., and the time is 5 min to 10 min.

[0013] In some embodiments, the manganese slag includes electrolytic manganese slag.

[0014] In some embodiments, the magnesium salt includes at least one of magnesium sulfate and magnesium chloride.

[0015] In some embodiments, the mixed solution further contains a modifier.

[0016] Optionally, the ratio of the amount of the modifier added to the mass of the magnesium oxide is (0.001~0.01):1.

[0017] Optionally, the modifying agent comprises a surfactant.

[0018] In a second aspect, the present application provides an application of the manganese slag treatment method as described in the first aspect, wherein the mixed gel produced by the manganese slag treatment method is used to prepare a glass magnesium board.

[0019] In a third aspect, the present application provides a glass-magnesium board material, wherein the preparation method of the glass-magnesium board material comprises the step of preparing a mixed gel by the manganese slag treatment method as described in the first aspect.

[0020] Compared with the traditional technology, this application has at least the following beneficial effects:

[0021] The present application forms a mixed gel by wet mixing manganese slag, magnesium salt and magnesium oxide. In the mixed gel, magnesium oxide can convert ammonium sulfate in the manganese slag into magnesium sulfate and ammonia gas, and magnesium sulfate can be used as magnesium salt; and the gel environment formed by magnesium oxide and magnesium salt can react and convert the soluble manganese source in the manganese slag into manganese oxide, thereby achieving harmless treatment of manganese slag. The formed mixed gel can be used as a raw material for preparing glass magnesium board, and the prepared glass magnesium board meets environmental protection requirements and quality requirements. The manganese slag treatment method of the present application can achieve harmless treatment and resource utilization of manganese slag. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic flow chart of a method for treating manganese slag provided in one embodiment of the present application. DETAILED DESCRIPTION

[0023] Below in conjunction with the embodiments and examples, the present application is further described in detail. These embodiments and examples are only used to illustrate the present application and are not used to limit the scope of the present application. The purpose of providing these embodiments and examples is to make the understanding of the disclosure of the present application more thorough and comprehensive. It should also be understood that the present application can be implemented in many different forms, and is not limited to the embodiments and examples described herein. Those skilled in the art can make various changes or modifications without violating the connotation of the present application, and the equivalent form obtained also falls within the protection scope of the present application. In addition, in the description below, a large number of specific details are given in order to provide a more comprehensive understanding of the present application. It should be understood that the present application can be implemented without one or more of these details.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0025] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0026] In this application, the terms "first", "second", etc. in "the first aspect", "the second aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0027] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0028] In the present application, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values ​​in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to an integer in the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical range disclosed in the present application should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows for a broad range of quantitative intervals such as percentage intervals, ratio intervals, and ratio intervals.

[0029] All documents mentioned in this application are cited as references in this application, just as each document is cited as reference separately. Unless they conflict with the application purpose and / or technical solution of this application, the cited documents involved in this application are cited with all contents and all purposes. When the cited documents are involved in this application, the definitions of relevant technical features, terms, nouns, phrases, etc. in the cited documents are also cited. When the cited documents are involved in this application, the examples and preferred methods of the cited relevant technical features can also be incorporated into this application as references, but are limited to the implementation of this application. It should be understood that when the cited content conflicts with the description in this application, the present application shall prevail or be modified adaptively according to the description of this application.

[0030] Among traditional technologies, manganese slag harmless treatment technology can be divided into two categories. One is the pyrometallurgical high-temperature sintering and melting treatment technology, which adopts high-temperature calcination (250℃~850℃) or high-temperature melting (>1200℃) to volatilize ammonia nitrogen and fix the manganese source to achieve harmless treatment of manganese slag. The treatment effect is long-term and stable, and the product resource utilization has a wide range of uses. However, this type of technology has a large one-time fixed asset investment and high treatment cost; the other is solidification / stabilization treatment technology, including dry and wet methods, which uses alkaline materials, phosphate materials, etc. to mix with slag to produce physical and chemical reactions, reduce the migration and diffusion of pollutants such as manganese and ammonia nitrogen, and achieve harmless treatment of manganese slag. This type of technology is simple to operate and has a quick effect. It can use materials such as red mud to treat waste, but the treatment effect is not as stable as pyrometallurgical treatment.

[0031] The first aspect of the present application provides a method for treating manganese slag, such as Figure 1 As shown, the manganese slag treatment method comprises:

[0032] Stirring a mixed solution containing manganese slag, magnesium salt, magnesium oxide and water, wherein the magnesium oxide reacts to remove ammonium sulfate in the manganese slag and converts a soluble manganese source contained in the manganese slag into manganese oxide;

[0033] A mixed gel including magnesium salt, magnesium oxide, magnesium sulfate and a manganese-containing compound is obtained, and the manganese-containing compound contained in the mixed gel includes manganese oxide.

[0034] The present application forms a mixed gel by wet mixing manganese slag, magnesium salt and magnesium oxide. In the mixed gel, magnesium oxide can convert ammonium sulfate in manganese slag into magnesium sulfate and ammonia gas, and magnesium sulfate can be used as magnesium salt; and the gel environment formed by magnesium oxide and magnesium salt can react and convert the soluble manganese source in manganese slag into manganese oxide, reduce the migration and diffusion of pollutants such as manganese and ammonia nitrogen, and achieve harmless treatment of manganese slag. The formed mixed gel can be used as a raw material for preparing glass magnesium board, and the prepared glass magnesium board meets environmental protection requirements and quality requirements. The manganese slag treatment method of the present application can achieve harmless treatment and resource utilization of manganese slag.

[0035] It is understood that the reaction formula of magnesium oxide and ammonium sulfate is MgO+(NH4)2SO4→MgSO4+2NH3+H2O. In addition, magnesium oxide can react with water to form alkaline conditions. Under alkaline conditions, the free manganese dissolved in the soluble manganese source in the manganese source solidifies to form manganese hydroxide, and manganese hydroxide is unstable and easily undergoes disproportionation reaction to form manganese oxide, which forms a eutectic with magnesium oxide and magnesium salt. Optionally, manganese oxide includes at least one of Mn2O3, MnO2 and MnO. It is understood that the manganese slag also includes an insoluble manganese source, such as manganese oxide or an insoluble manganese salt.

[0036] In some embodiments, the mass proportion of the manganese source contained in the manganese slag is 10% to 20%, for example, it can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%. It is understood that the manganese source includes at least one of a manganese salt and a manganese oxide, wherein the manganese salt can be a soluble manganese salt or an insoluble manganese salt, for example, the soluble manganese source includes at least one of manganese sulfate and manganese carbonate.

[0037] In some embodiments, the manganese slag further contains at least one of silicon oxide, iron source, calcium source and magnesium source. Optionally, the mass proportion of silicon oxide in the manganese slag is 10% to 30%; the mass proportion of iron source in the manganese slag is 10% to 20%; the mass proportion of calcium source in the manganese slag is 5% to 15%; the mass proportion of magnesium source in the manganese slag is 1% to 5%. The iron source can be at least one of an iron salt and an iron oxide; the calcium source can be at least one of a calcium salt and a calcium oxide; and the magnesium source can be at least one of a magnesium salt and a magnesium oxide.

[0038] In some embodiments, the mass ratio of the manganese slag to the magnesium oxide is (0.3-0.5): 1, for example, it can be 0.30: 1, 0.32: 1, 0.34: 1, 0.36: 1, 0.38: 1, 0.40: 1, 0.42: 1, 0.44: 1, 0.46: 1, 0.48: 1 or 0.50: 1. The present application selects the mass ratio of manganese slag to magnesium oxide as above, and by adding more magnesium oxide relative to the manganese slag, it effectively ensures that the ammonium sulfate in the manganese slag and the manganese source react fully, avoids residual ammonium sulfate and improves the solidification effect of the manganese source.

[0039] In some embodiments, the mass ratio of the magnesium salt to the magnesium oxide is (0.4-0.6): 1, for example, 0.40: 1, 0.42: 1, 0.44: 1, 0.46: 1, 0.48: 1, 0.50: 1, 0.52: 1, 0.54: 1, 0.56: 1, 0.58: 1 or 0.60: 1. It is understood that the amount of magnesium salt added can be reasonably selected according to the mass of the magnesium salt formed by the reaction of magnesium oxide and ammonium sulfate.

[0040] In some embodiments, the manganese slag treatment method further includes: recovering ammonia generated by the reaction of the magnesium oxide and the ammonium sulfate. In the present application, the magnesium sulfate generated during the reaction of the magnesium oxide and the ammonium sulfate can be used as a raw material for the glassy magnesium board, reducing the amount of magnesium sulfate added, and the generated ammonia is soluble in water and can be used to manufacture fertilizers and synthetic ammonia after recovery.

[0041] In some embodiments, the stirring speed is 250 rpm to 1500 rpm, for example, it can be 250 rpm, 300 rpm, 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm, 1400 rpm or 1500 rpm.

[0042] In some embodiments, the stirring temperature is 30° C. to 40° C., for example, 30° C., 31° C., 32° C., 33° C., 34° C., 35° C., 36° C., 37° C., 38° C., 39° C. or 40° C. It is understood that the stirring temperature can satisfy the reaction of magnesium oxide with the manganese source and ammonium sulfate in the manganese slag.

[0043] In some embodiments, the stirring time is 5 min to 10 min, for example, it can be 5.0 min, 5.5 min, 6.0 min, 6.5 min, 7.0 min, 7.5 min, 8.0 min, 8.5 min, 9.0 min, 9.5 min or 10.0 min.

[0044] In some embodiments, the manganese slag includes electrolytic manganese slag.

[0045] In some embodiments, the magnesium salt includes at least one of magnesium sulfate and magnesium chloride.

[0046] In some embodiments, the mixed solution further contains a modifier.

[0047] Optionally, the ratio of the amount of the modifier added to the mass of the magnesium oxide is (0.001~0.01):1, for example, it can be 0.001:1, 0.002:1, 0.003:1, 0.004:1, 0.005:1, 0.006:1, 0.007:1, 0.008:1, 0.009:1 or 0.010:1.

[0048] Optionally, the modifier includes a surfactant. In the present application, the modifier is added during the manganese slag treatment process to improve the contact reaction between the manganese slag, magnesium oxide and magnesium salt, thereby improving the reaction efficiency.

[0049] In some embodiments, the surfactant includes at least one of an anionic surfactant and a cationic surfactant. The surfactant can be reasonably selected according to the properties of the raw materials. For example, the surfactant can be sodium dodecylbenzene sulfonate.

[0050] It is understood that the amount of water added in the present application is sufficient to allow the raw materials to form a gel and react. Optionally, the mass ratio of the amount of water added to the magnesium oxide is (0.7-0.8):1.

[0051] Exemplarily, a method for treating the manganese slag is provided, comprising:

[0052] Stir magnesium oxide, manganese slag, magnesium salt, modifier and water according to the mass ratio of 1: (0.3-0.5): (0.4-0.6): (0.001-0.01): (0.7-0.8) at a stirring speed of 250 rpm-1500 rpm, a temperature of 30°C-40°C, and a time of 5 min-10 min;

[0053] After the generated ammonia gas is recovered, a mixed gel including magnesium salt, magnesium oxide, magnesium sulfate and a manganese-containing compound containing at least manganese oxide is obtained.

[0054] The second aspect of the present application provides an application of the manganese slag treatment method as described in the first aspect, wherein the mixed gel produced by the manganese slag treatment method is used to prepare a glass magnesium board.

[0055] In the conventional technology, a gel formed by magnesium salt and magnesium oxide is used to prepare a glass magnesium board, while the present application uses a mixed gel treated with manganese slag as a raw material. During the treatment process, magnesium sulfate can be formed to reduce the amount of magnesium salt added, and the manganese source solidified in the mixed gel can further improve the strength and weather resistance of the glass magnesium board. The present application uses a gel formed by magnesium oxide and magnesium salt to perform harmless treatment on manganese slag, and the formed mixed gel can be used as a raw material for glass magnesium boards, thereby realizing the resource utilization of manganese slag.

[0056] In some embodiments, the mixed gel is added with binding fibers and then roll-formed to prepare a glass magnesium board. Optionally, the binding fibers include plant fibers, such as wood fibers. It is understood that adding binding fibers to the mixed gel can improve the strength of the glass magnesium board and reduce the density of the board.

[0057] In some embodiments, the mixed gel is compounded with the reinforcing layer and then roll-formed. The reinforcing layer may be an alkali-resistant glass fiber cloth.

[0058] The embodiments of the present application will be described in detail below in conjunction with examples. It should be understood that these examples are only used to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are preferably referred to the guidance provided in the present application, and can also be based on the experimental manual or normal conditions in this area, can also be based on the conditions recommended by the manufacturer, or refer to experimental methods known in the art.

[0059] In the following examples, the element composition of manganese slag is as follows:

[0060]

[0061] The modifier is sodium dodecylbenzene sulfonate.

[0062] Example 1

[0063] Magnesium oxide, manganese slag, magnesium sulfate, a modifier and water are stirred in a mass ratio of 1:0.4:0.5:0.01:0.75 at a stirring speed of 1000 rpm, a temperature of 35°C and a time of 5 minutes. Magnesium oxide reacts with a soluble manganese source and ammonium sulfate in the manganese slag to form magnesium sulfate, ammonia and manganese oxide. After removing the ammonia formed by the reaction, a mixed gel including magnesium sulfate, magnesium oxide and a manganese-containing compound is obtained.

[0064] Example 2

[0065] Magnesium oxide, manganese slag, magnesium chloride, a modifier and water are stirred and mixed in a mass ratio of 1:0.3:0.6:0.005:0.8 at a stirring speed of 800 rpm, a temperature of 35°C and a time of 8 minutes. Magnesium oxide reacts with a soluble manganese source and ammonium sulfate in the manganese slag to form magnesium sulfate, ammonia and manganese oxide. After removing the ammonia formed by the reaction, a mixed gel including magnesium sulfate, magnesium chloride, magnesium oxide and a manganese-containing compound is obtained.

[0066] Example 3

[0067] Magnesium oxide, manganese slag, magnesium chloride, a modifier and water are stirred in a mass ratio of 1:0.5:0.4:0.001:0.7 at a stirring speed of 1500 rpm, a temperature of 35°C and a time of 5 minutes. Magnesium oxide reacts with a soluble manganese source and ammonium sulfate in the manganese slag to form magnesium sulfate, ammonia and manganese oxide. After removing the ammonia formed by the reaction, a mixed gel including magnesium sulfate, magnesium chloride, magnesium oxide and a manganese-containing compound is obtained.

[0068] The determination of manganese in the glass magnesium board prepared in the above embodiment refers to the nitric acid-hydrogen peroxide digestion method recommended by the U.S. Environmental Protection Agency. After digestion and membrane, the manganese element is determined using an inductively coupled plasma spectrometer (ICP-OES); referring to GB / T39701-2020 "Limits and test methods for ammonium ion content in fly ash", an ammonium ion analyzer (ACA-2021) is used to determine the ammonia nitrogen content in the glass magnesium board, and the leachable heavy metal content is tested in accordance with GB / T 30810-2014. The results show that the glass magnesium board of the embodiment of the present application meets the environmental protection requirements and quality requirements. The test results of the total manganese and ammonia nitrogen content of the glass magnesium board of Example 1 are shown in Table 1, and the heavy metal content test results are shown in Table 2.

[0069] Table 1

[0070]

[0071] Note: NT means that there is no detection line description in the standard, and the ammonia nitrogen limit is from GB / T39701-2020.

[0072] Table 2

[0073]

[0074] Note: ND means not reaching the detection limit, the limit value comes from GB 30760-2024.

[0075] It can be seen from Tables 1 and 2 above that the indicators of this application meet the limit requirements of the "Technical Specifications for Manganese Slag Pollution Control" (HJ1241-2022), and the product has high environmental safety.

[0076] The mixed gel after removing ammonia is used as a raw material, wood fiber and a foaming agent (sodium carbonate can be used as the foaming agent) are added to the mixed gel, and air is introduced to foam and stir and mix, and the ratio of the added amount of wood fiber to the added amount of magnesium oxide is 0.65:1; after mixing evenly, the mixed gel is compounded with an alkali-resistant glass fiber cloth, and a glass magnesium board is obtained after roller forming.

[0077] The performance of the glass magnesium board prepared in the above embodiment was tested according to the industry standard of magnesium cementitious material products for construction - magnesium oxysulfide board. The flexural strength, impact strength, apparent density, moisture content, shrinkage rate, swelling rate, screw holding force, extractable chloride ion content and anti-halogen return of the glass magnesium board prepared in this application all meet the quality requirements for use. Among them, the flexural strength of the glass magnesium board prepared in this application reaches more than 11.0MPa, and the impact strength reaches 3.0kJ / m 2 above.

[0078] In summary, the present application forms a mixed gel by wet mixing manganese slag, magnesium salt and magnesium oxide. In the mixed gel, magnesium oxide can convert ammonium sulfate in manganese slag into magnesium sulfate and ammonia, and magnesium sulfate can be used as magnesium salt; and the gel environment formed by magnesium oxide and magnesium salt can react and convert the soluble manganese source in manganese slag into manganese oxide, thereby achieving harmless treatment of manganese slag. The formed mixed gel can be used as a raw material for preparing glass magnesium board, and the prepared glass magnesium board meets environmental protection requirements and quality requirements. The manganese slag treatment method of the present application can achieve harmless treatment and resource utilization of manganese slag.

[0079] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0080] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the application. It should be noted that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A method for treating manganese slag, characterized in that: The manganese slag treatment method comprises: Stirring a mixed solution containing manganese slag, magnesium salt, magnesium oxide and water, wherein the magnesium oxide reacts to remove ammonium sulfate in the manganese slag and converts a soluble manganese source contained in the manganese slag into manganese oxide; A mixed gel including magnesium salt, magnesium oxide, magnesium sulfate and a manganese-containing compound is obtained, and the manganese-containing compound contained in the mixed gel includes manganese oxide.

2. The method for treating manganese slag according to claim 1, characterized in that: The mass proportion of the manganese source contained in the manganese slag is 10% to 20%.

3. The method for treating manganese slag according to claim 1, characterized in that: The soluble manganese source includes at least one of manganese sulfate and manganese carbonate.

4. The method for treating manganese slag according to claim 1, characterized in that: The manganese slag treatment method meets at least one of the following conditions: (1) The mass ratio of the manganese slag to the magnesium oxide is (0.3-0.5):1; (2) The mass ratio of the magnesium salt to the magnesium oxide is (0.4-0.6):

1.

5. The method for treating manganese slag according to claim 1, characterized in that: The manganese slag treatment method further includes: recovering ammonia gas generated by the reaction of the magnesium oxide and the ammonium sulfate.

6. The method for treating manganese slag according to claim 1, characterized in that: The stirring speed is 250 rpm to 1500 rpm, the temperature is 30° C. to 40° C., and the time is 5 min to 10 min.

7. The method for treating manganese slag according to claim 1, characterized in that: The manganese slag treatment method also satisfies at least one of the following conditions: (1) The manganese slag includes electrolytic manganese slag; (2) The magnesium salt includes at least one of magnesium sulfate and magnesium chloride.

8. The method for treating manganese slag according to any one of claims 1 to 7, characterized in that: The mixed liquid also contains a modifier; Optionally, the ratio of the amount of the modifier added to the mass of the magnesium oxide is (0.001-0.01):1; Optionally, the modifying agent comprises a surfactant.

9. An application of the method for treating manganese slag according to any one of claims 1 to 8, characterized in that: The mixed gel produced by the manganese slag treatment method is used to prepare glass magnesium plates.

10. A glass magnesium plate, characterized in that: The method for preparing the glass magnesium plate comprises the step of preparing a mixed gel by the manganese slag treatment method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for innocent treatment and comprehensive utilization of manganese slag

    CN101691633A

  • Alkaline cementing material produced from electrolytic manganese residue

    CN110642543A

  • Electrolytic manganese residue non-sintered brick and preparation method thereof

    CN110642560A

  • Method for preparing composite modified magnesium oxysulfate cementing material by utilizing electrolytic manganese slag

    CN111689755A