Nickel-zinc ferrite material and preparation method thereof
By adjusting the proportions of Fe2O3, NiO, ZnO and Co2O3 and controlling the sintering process, the problem of difficulty in balancing high saturation magnetic induction intensity and anti-magnetization performance of nickel-zinc ferrite materials is solved, and the balance of high saturation magnetic induction intensity and anti-magnetization performance is achieved. Ensure the performance stability of electronic devices under external magnetic field interference.
Patent Information
- Application Number
- CN202410792752.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-19
AI Technical Summary
It is difficult for existing nickel-zinc ferrite materials to achieve both high saturation magnetic induction intensity and good anti-magnetization properties, which leads to the problem that electronic devices are susceptible to interference from external magnetic fields, leading to reduced performance.
By adjusting the proportions of Fe2O3, NiO, ZnO and Co2O3, nickel-zinc ferrite materials are prepared. Traditional grinding methods and sintering processes are used to control pre-sintering and sintering temperatures to ensure both high saturation magnetic induction intensity and anti-magnetization properties of the material.
It has achieved significant improvement in anti-magnetization performance on the basis of maintaining high saturation magnetic induction intensity. The change rate of magnetic permeability before and after magnetization is less than 4%, which can effectively resist external magnetic field interference. Bs is greater than 460mT, and the material performance is stable.
Smart Images

Figure BDA0004900571630000091 
Figure BDA0004900571630000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ferrite preparation, and in particular to a nickel-zinc ferrite material and a preparation method thereof. Background Art
[0002] With the development of electronic power technology, it is an inevitable trend for electronic devices to develop in the direction of miniaturization, high frequency and high current. Therefore, the performance requirements for soft magnetic materials in electronic devices are increasing. Nickel zinc ferrite (NiZn ferrite) has the advantages of excellent high frequency characteristics, good temperature stability, diverse formulas, large nonlinearity, simple process, etc. It is widely used in television, communication, instrumentation, automatic control, electronic countermeasures and other fields.
[0003] At present, NiZn ferrite materials can be divided into three categories according to their uses and characteristics: high frequency, high saturation magnetic induction intensity and high initial magnetic permeability. However, there are always inevitable disadvantages. For example, materials with high saturation magnetic induction intensity and low conductivity have good superposition performance, but due to their low anti-magnetic performance, they can only be used in low-amplitude alternating magnetic fields. If used in electronic devices, external magnetic field interference may cause the device performance to be greatly reduced. It is difficult for existing manufacturers to produce nickel-zinc ferrites that have both high saturation magnetic induction intensity and anti-magnetic performance.
[0004] For example, CN104030669A discloses a filter-pressing molding preparation method for NiZn ferrite. The main components are Fe2O3: 48-54 mol%, ZnO: 30-32 mol%, NiO: 3.5-10 mol%, CuO: 8-15 mol% in molar percentage; the dopant is V2O5: 0-3 wt%. The saturation magnetic induction intensity of the NiZn ferrite is low. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defect of the nickel-zinc ferrite material in the prior art that both high saturation magnetic induction intensity and good anti-magnetization performance cannot be taken into account, thereby providing a nickel-zinc ferrite material and a preparation method thereof.
[0006] To this end, in the first aspect, the present invention provides a nickel-zinc ferrite material, which includes a main component and an auxiliary component. Taking the total weight of the main component as 100wt%, the main component contains the following components, and the weight percentage of each component is: Fe2O3 is 68.34~68.76wt%, NiO is 19.12~19.54wt%, and the remainder is ZnO; based on the total weight of the main component, the auxiliary component includes 0.1wt%~0.2wt% of Co2O3.
[0007] In a second aspect, the present invention also provides a method for preparing the above-mentioned nickel-zinc ferrite material, comprising mixing Fe2O3, NiO, and ZnO in a weight ratio, grinding the mixture for a first time, pre-burning the mixture to obtain a pre-burned material, mixing the pre-burned material with auxiliary components, grinding the mixture for a second time, granulating, molding, and sintering the mixture to obtain the nickel-zinc ferrite material.
[0008] Furthermore, the first grinding and / or the second grinding is ball milling.
[0009] Furthermore, the ball milling time is 2-3h; and / or the ball milling speed is 350-450rpm, and the material-ball ratio is 2-3:1.
[0010] The ball-to-material ratio is the mass ratio of the material to be ground to the ball-milling medium.
[0011] Water is also added before ball milling, and the material-water ratio is 3:4-5. The ball-water ratio is the mass ratio of the material to be ground to water.
[0012] Furthermore, the pre-sintering temperature is 900-950° C. and the time is 2-3 hours.
[0013] Furthermore, in the pre-firing process, before reaching the pre-firing temperature, it also includes a first heating stage of heating from room temperature to 280-320°C at a heating rate of 80-100°C / h, and a second heating stage of heating from 280-320°C to 900-950°C at a heating rate of 120-140°C / h.
[0014] Furthermore, the granulation process includes the steps of mixing a binder and screening and crushing;
[0015] Preferably, the quality of the adhesive comprises PVA adhesive;
[0016] Preferably, the binder accounts for 8-12 wt % of the total mass of the pre-sintered material.
[0017] Furthermore, the sintering temperature is 1100-1200°C and the time is 2-3 hours; preferably, before reaching the sintering temperature, it also includes the process of heating from room temperature to 190-210°C at a heating rate of 85-95°C / h, heating from 190-210°C to 440-460°C at a heating rate of 60-65°C / h, and heating from 440-460°C to 1100-1200°C at a heating rate of 140-160°C / h.
[0018] Furthermore, after the first grinding or the second grinding, a step of drying and screening is also included.
[0019] Furthermore, the preparation method comprises the following steps:
[0020] (1) Main component mixing and first grinding: Fe2O3, NiO and ZnO are mixed according to weight ratio, and the mixture is ball milled and dried; the ball milling time is 2-3 hours, the rotation speed is 350-450 rpm, and the material-ball ratio is 2-3:1;
[0021] (2) Pre-calcining: the dried material of step (1) is sieved and heated from room temperature to 280-320°C at a heating rate of 80-100°C / h, and then heated from 280-320°C to 900-950°C at a heating rate of 120-140°C / h, and then kept at 900-950°C for 2-3h to obtain a pre-calcined material;
[0022] (3) Doping and second grinding: the pre-sintered material is sieved and mixed with the auxiliary components, and the mixture is ball-milled and dried; the ball-milling time is 2-3 hours and the rotation speed is 350-450 rpm;
[0023] (4) Granulation: the dried material from step (3) is sieved and mixed with a binder, and then sieved and crushed;
[0024] (5) Molding: Pressing the material crushed in step (4) into a mold;
[0025] (6) Sintering: The material formed in step (5) is sintered in an air atmosphere, and the sintering process is as follows: heating from room temperature to 190-210°C at a heating rate of 85-95°C / h, heating from 190-210°C to 440-460°C at a heating rate of 60-65°C / h, heating from 440-460°C to 1100-1200°C at a heating rate of 140-160°C / h, and then sintering at 1100-1200°C for 2-3 hours to obtain a nickel-zinc ferrite material.
[0026] The technical solution of the present invention has the following advantages:
[0027] 1. The nickel-zinc ferrite material provided by the present invention comprises a main component and an auxiliary component. Taking the total weight of the main component as 100wt%, the main component comprises the following components, and the weight percentage of each component is: Fe2O3 is 68.34-68.76wt%, NiO is 19.12-19.54wt%, and the balance is ZnO; the auxiliary component comprises 0.1wt%-0.2wt% of Co2O3 according to the total weight of the main component. By controlling the contents of Fe2O3, NiO, ZnO and Co2O3 in the formula within the above range, the nickel-zinc ferrite material significantly improves the anti-magnetic performance (anti-electromagnetic interference ability) on the basis of maintaining high saturation magnetic induction intensity. The prepared material has good anti-magnetic performance, and the change rate of magnetic permeability before and after magnetization is less than 4%, which can prevent the performance from being greatly reduced due to external magnetic field interference. And Bs is greater than 460mT.
[0028] 2. The preparation method of the nickel-zinc ferrite material provided by the present invention comprises mixing Fe2O3, NiO and ZnO in proportion, grinding the mixture for the first time, pre-firing to obtain a pre-firing material, mixing the pre-firing material with auxiliary components, grinding the mixture for the second time, granulating, molding and sintering to obtain the nickel-zinc ferrite material. The present invention adopts a traditional grinding method (such as mechanical ball milling) for preparation, and the production process is simple and easy to produce.
[0029] 3. The preparation method of the nickel-zinc ferrite material provided by the present invention, during the pre-burning process, by controlling the pre-burning temperature to 900-950°C, the time to 2-3h and also including a first heating stage of heating from room temperature to 280-320°C at a heating rate of 80-100°C / h before reaching the pre-burning temperature, and a second heating stage of heating from 280-320°C to 900-950°C at a heating rate of 120-140°C / h, the experimental efficiency can be improved.
[0030] During the sintering process, the sintering temperature is controlled to be 1100-1200°C for 2-3 hours; and before reaching the sintering temperature, the temperature is increased from room temperature to 190-210°C at a heating rate of 85-95°C / h, from 190-210°C to 440-460°C at a heating rate of 60-65°C / h, and from 440-460°C to 1100-1200°C at a heating rate of 140-160°C / h. This can further improve the shrinkage rate of the sample ring, improve the density, and help to improve Bs and magnetic permeability. DETAILED DESCRIPTION
[0031] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0032] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0033] Example 1
[0034] This embodiment provides a nickel-zinc ferrite material and a preparation method thereof, comprising the following steps:
[0035] (1) Mixing and first grinding of main components: Fe2O3, NiO and ZnO were weighed and mixed according to the weight ratio of Fe2O3: 68.55wt%, NiO: 19.33wt%, and the balance ZnO to form the main component. 300g of the prepared main component was added to a ball mill, 100g of zirconium oxide balls were added as the ball milling medium, 450g of deionized water was added, and the slurry was dried after ball milling for two and a half hours at a speed of 391 rpm using a planetary ball mill.
[0036] (2) Pre-burning: The dried slurry is sieved with a 30-mesh screen and then pre-burned to cause a curing reaction to obtain a pre-burned material. The pre-burning process is as follows: heating from room temperature to 300°C at a heating rate of 90°C / h, heating from 300°C to 950°C at a heating rate of 130°C / h, keeping at 950°C for 2h, and cooling naturally in the furnace.
[0037] (3) Doping and secondary grinding: After the pre-sintered material cools to room temperature, it is sieved with a 30-mesh sieve and doped with 0.1 wt% Co2O3, which accounts for the mass of the main component, and placed in a ball mill. 100 g of zirconia balls are added as the ball milling medium, and 450 g of deionized water are added. The slurry is ball milled at a speed of 391 rpm for two and a half hours using a planetary ball mill and then dried.
[0038] (4) Granulation: The dried slurry was sieved with a 30-mesh sieve to obtain a powder, into which 10 wt% of the mass of the powder was added PVA glue (solid content of 36%), stirred and granulated, and then crushed with a 30-mesh sieve.
[0039] (5) Molding: Use a mold with an outer diameter of 20 mm and an inner diameter of 10 mm at a pressure of 6 MPa to form a sample ring.
[0040] (6) Sintering: The sample ring was placed in a muffle furnace and sintered in an air atmosphere. The sintering process was as follows: heating from room temperature to 200 °C at a heating rate of 90 °C / h, heating from 200 °C to 450 °C at a heating rate of 62.5 °C / h, and heating from 450 °C to 1200 °C at a heating rate of 150 °C / h; finally, sintering at 1200 °C for 2 h.
[0041] Example 2
[0042] This embodiment provides a nickel-zinc ferrite material and a preparation method thereof, which is basically the same as that of Embodiment 1, except that the amount of Co2O3 added in step (3) is adjusted to 0.2% of the mass of the main component.
[0043] Example 3
[0044] This embodiment provides a nickel-zinc ferrite material and a preparation method thereof, comprising the following steps:
[0045] (1) Main component mixing and first grinding: Fe2O3, NiO and ZnO were weighed and mixed according to the weight ratio of Fe2O3: 68.76wt%, NiO: 19.12wt%, and the balance ZnO to form the main component. 300g of the prepared main component was added to a ball mill, 150g of zirconium oxide balls were added as the ball milling medium, 450g of deionized water was added, and the slurry was dried after ball milling for 2h at a speed of 350rpm using a planetary ball mill.
[0046] (2) Pre-burning: The dried slurry is sieved with a 30-mesh screen and then pre-burned to cause a curing reaction to obtain a pre-burned material. The pre-burning process is as follows: heating from room temperature to 280°C at a heating rate of 100°C / h, heating from 280°C to 900°C at a heating rate of 140°C / h, keeping at 900°C for 3 hours, and cooling naturally in the furnace.
[0047] (3) Doping and secondary grinding: After the pre-sintered material cools to room temperature, it is sieved with a 30-mesh sieve and doped with 0.1 wt% Co2O3, which accounts for the mass of the main component, and placed in a ball mill. 100 g of zirconia balls are added as the ball milling medium, and 450 g of deionized water are added. The slurry is ball milled at a speed of 391 rpm for two and a half hours using a planetary ball mill and then dried.
[0048] (4) Granulation: The dried slurry was sieved with a 50-mesh sieve to obtain a powder, into which 8 wt% of the mass of the powder was dropped PVA glue (solid content of 36%), stirred and granulated, and then crushed with a 30-mesh sieve.
[0049] (5) Molding: Use a mold with an outer diameter of 20 mm and an inner diameter of 10 mm at a pressure of 6 MPa to form a sample ring.
[0050] (6) Sintering: The sample ring was placed in a muffle furnace and sintered in an air atmosphere. The sintering process was as follows: heating from room temperature to 210°C at a heating rate of 95°C / h, heating from 210°C to 460°C at a heating rate of 60°C / h, and heating from 460°C to 1100°C at a heating rate of 150°C / h; finally, sintering was performed at 1100°C for 3 h.
[0051] Example 4
[0052] The present embodiment provides a nickel-zinc ferrite material and a preparation method thereof, which is basically the same as Example 1, except that the weight ratio of each component in the main component is different. The weight ratio of each component in the main component in this embodiment is as follows: Fe2O3: 68.34wt%, NiO: 19.54wt%, and the balance is ZnO.
[0053] Comparative Example 1
[0054] This comparative example provides a nickel-zinc ferrite material and a preparation method thereof, which are basically the same as those of Example 1, except that the amount of Co2O3 added in step (3) is adjusted to 0.3% of the mass of the main component.
[0055] Comparative Example 2
[0056] This comparative example provides a nickel-zinc ferrite material and a preparation method thereof, which are basically the same as those of Example 1, except that the amount of Co2O3 added in step (3) is adjusted to 0.4% of the mass of the main component.
[0057] Comparative Example 3
[0058] This comparative example provides a nickel-zinc ferrite material and a preparation method thereof, which are basically the same as Example 1, except that Co2O3 is not added in step (3).
[0059] Comparative Example 4
[0060] This comparative example provides a nickel-zinc ferrite material and a preparation method thereof, which are basically the same as Example 1, except that the components are weighed as the main components according to the weight ratio of Fe2O3: 67.3wt%, NiO: 19.33wt%, and the balance ZnO.
[0061] Comparative Example 5
[0062] This comparative example provides a nickel-zinc ferrite material and a preparation method thereof, which are basically the same as Example 2, except that the components are weighed as the main components according to the weight ratio of Fe2O3: 67.3wt%, NiO: 19.33wt%, and the balance ZnO.
[0063] Comparative Example 6
[0064] This comparative example provides a nickel-zinc ferrite material and a preparation method thereof, which are basically the same as Example 1, except that the components are weighed as the main components according to the weight ratio of Fe2O3: 68.55wt%, NiO: 18.34wt%, and the balance ZnO.
[0065] Comparative Example 7
[0066] This comparative example provides a nickel-zinc ferrite material and a preparation method thereof, which are basically the same as Example 1, except that the components are weighed as the main components according to the weight ratio of Fe2O3: 68.55wt%, NiO: 20.15wt%, and the balance ZnO.
[0067] Core magnetic properties test:
[0068] (1) Magnetic permeability test: The nickel-zinc ferrite materials (ie, magnetic rings) prepared in the examples and comparative examples were tested for the real part μ1 of the magnetic permeability (ie, initial magnetic permeability μ') at 1 MHz using an Agilent E4991A analyzer. The results are shown in Table 1.
[0069] (2) Anti-magnetization performance test: The magnetic rings prepared in the embodiments and comparative examples were magnetized clockwise along the axial direction of the sample ring and around the center of the circle using a magnet with a surface magnetic induction intensity of 320 mT. The real part μ2 of the magnetic permeability of the sample ring after magnetization at 1 MHz was then tested using an Agilent E4991A analyzer, and the change rate of the magnetic permeability before and after was calculated using the formula (μ1-μ2) / μ1. The results are shown in Table 1.
[0070] (3) Bs test: The magnetic rings prepared in each embodiment and comparative example were uniformly wound with 25 turns of copper wire with a diameter of 0.4 mm. The test conditions were 50 Hz, 1 V, 25° C., and the maximum value of the applied magnetic field was 4000 A / m. The results are shown in Table 2.
[0071] Table 1 Anti-magnetic performance test results
[0072] Initial magnetic permeability μ' Magnetic permeability change rate before and after Example 1 104.3 0.48% Example 2 99.8 3.76% Example 3 105.6 0.44% Example 4 103.9 0.43% Comparative Example 1 92.8 8.56% Comparative Example 2 74.6 13.56% Comparative Example 3 126.8 9.65% Comparative Example 4 93.6 6.77% Comparative Example 5 90.8 8.69% Comparative Example 6 134.6 8.77% Comparative Example 7 50.8 1.33%
[0073] Table 2 Saturation magnetic induction intensity test results
[0074]
[0075]
[0076] From the results in the above table, it can be seen that the magnetic permeability of Examples 1-4 is appropriate (between 90 and 110), and the anti-magnetization performance is excellent (the change rate of the magnetic permeability is less than 4%), and Bs>460mT. The smaller the absolute value of the magnetocrystalline anisotropy constant K1 of the material, the more difficult it is to produce irreversible magnetization in the material. The K1 of NiZn ferrite is negative, while that of Fe 2+ With Co 2+ The K1 of the NiZn ferrite is a large positive value, and the K1 of the NiZn ferrite can be corrected to make its absolute value close to 0. Therefore, the absolute value of K1 of Examples 1-4 may be small, so that it has excellent anti-magnetization performance.
[0077] By comparing Example 1 with Comparative Examples 1-3, it can be seen that if too much or too little Co2O3 is added, the absolute value of K1 will increase, the rate of change of magnetic permeability before and after magnetization will increase, and the sub-Co ions have the effect of freezing the magnetic domain, and adding too much will also cause the magnetic permeability to decrease. In summary, Co2O3 also needs to be controlled at about 0.1wt% to 0.2wt%.
[0078] By comparing Example 1 with Comparative Examples 4-7, it can be seen that the amounts of Fe2O3, NiO and ZnO need to be strictly controlled within the range required by the present invention. If not strictly controlled (the content is too high or too low), the rate of change of magnetic permeability before and after magnetization will increase. In Comparative Example 6, the Bs of the nickel-zinc ferrite material is significantly reduced due to the low NiO content. In Comparative Example 7, the magnetic permeability of the nickel-zinc ferrite material is significantly reduced due to the high NiO content.
[0079] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A nickel-zinc ferrite material, characterized in that: The nickel-zinc ferrite material includes a main component and an auxiliary component. Taking the total weight of the main component as 100wt%, the main component contains the following components, and the weight percentage of each component is: Fe2O3 is 68.34~68.76wt%, NiO is 19.12~19.54wt%, and the balance is ZnO; based on the total weight of the main component, the auxiliary component includes 0.1wt%~0.2wt% of Co2O3.
2. A method for preparing the nickel-zinc ferrite material according to claim 1, characterized in that: The method comprises the steps of mixing Fe2O3, NiO and ZnO according to a weight ratio, grinding the mixture for the first time, pre-firing the mixture to obtain a pre-firing material, mixing the pre-firing material with auxiliary components, grinding the mixture for the second time, granulating, molding and sintering the mixture to obtain a nickel-zinc ferrite material.
3. The method for preparing the nickel-zinc ferrite material according to claim 2, characterized in that: The first grinding and / or the second grinding is ball milling.
4. The method for preparing the nickel-zinc ferrite material according to claim 3, characterized in that: The ball milling time is 2-3h, the ball milling speed is 350-450rpm, and the material-to-ball ratio of the ball mill is 2-3:
1.
5. The method for preparing the nickel-zinc ferrite material according to claim 2, characterized in that: The pre-sintering temperature is 900-950° C. and the pre-sintering time is 2-3 hours.
6. The method for preparing the nickel-zinc ferrite material according to claim 5, characterized in that: In the pre-firing process, before reaching the pre-firing temperature, it also includes a first heating stage of heating from room temperature to 280-320°C at a heating rate of 80-100°C / h, and a second heating stage of heating from 280-320°C to 900-950°C at a heating rate of 120-140°C / h.
7. The method for preparing the nickel-zinc ferrite material according to claim 2, characterized in that: The granulation process includes the steps of mixing a binder and screening and crushing; Preferably, the adhesive comprises PVA adhesive; Preferably, the mass of the binder accounts for 8-12wt% of the total mass of the pre-sintered material.
8. The method for preparing the nickel-zinc ferrite material according to claim 2, characterized in that: The sintering temperature is 1100-1200°C and the time is 2-3 hours; preferably, before reaching the sintering temperature, it also includes the process of heating from room temperature to 190-210°C at a heating rate of 85-95°C / h, heating from 190-210°C to 440-460°C at a heating rate of 60-65°C / h, and heating from 440-460°C to 1100-1200°C at a heating rate of 140-160°C / h.
9. The method for preparing the nickel-zinc ferrite material according to any one of claims 2 to 8, characterized in that: After the first grinding or the second grinding, a step of drying and screening is also included.
10. The method for preparing the nickel-zinc ferrite material according to claim 2, characterized in that: The preparation method comprises the following steps: (1) Main component mixing and first grinding: Fe2O3, NiO and ZnO are mixed according to weight ratio, and the mixture is ball milled and dried; the ball milling time is 2-3 hours, the rotation speed is 350-450 rpm, and the material-ball ratio is 2-3:1; (2) Pre-calcining: the dried material of step (1) is sieved and heated from room temperature to 280-320°C at a heating rate of 80-100°C / h, and then heated from 280-320°C to 900-950°C at a heating rate of 120-140°C / h, and then kept at 900-950°C for 2-3h to obtain a pre-calcined material; (3) Doping and second grinding: the pre-sintered material is sieved and mixed with the auxiliary components, and the mixture is ball-milled and dried; the ball-milling time is 2-3 hours and the rotation speed is 350-450 rpm; (4) Granulation: the dried material from step (3) is sieved and mixed with a binder, and then sieved and crushed; (5) Molding: Pressing the material crushed in step (4) into a mold; (6) Sintering: The material formed in step (5) is sintered in an air atmosphere, and the sintering process is as follows: heating from room temperature to 190-210°C at a heating rate of 85-95°C / h, heating from 190-210°C to 440-460°C at a heating rate of 60-65°C / h, heating from 440-460°C to 1100-1200°C at a heating rate of 140-160°C / h, and then sintering at 1100-1200°C for 2-3 hours to obtain a nickel-zinc ferrite material.
Citation Information
Patent Citations
Ni-Zn soft-magnetic ferrite material, Ni-Zn ferrite, preparation method thereof and electrical inductance
CN105985103A
Nickel-zinc soft magnetic ferrite material and preparation method thereof
CN107382300A
Nickel-zinc-copper ferrite material suitable for wide-temperature loading and preparation method of nickel-zinc-copper ferrite material
CN115417664A
High-frequency low-temperature-coefficient low-loss nickel-zinc ferrite and preparation method thereof
CN117902888A
Low temperature sintering radio frequency soft ferrite material, and method for manufacturing a wire coiling inductor core using such material
US5853608A