Preparation method and application of 4-cyclohexene-1, 2-dicarboxylic acid

By degrading epoxy resin and ethylene glycol at low temperatures and using NaOH for alkaline hydrolysis, sodium cyclohexene-2-carboxylate is generated. Further acidification and recycling processes solve the problem of difficulty in recycling waste epoxy resin. , realizing efficient and environmentally friendly epoxy resin recycling and reuse, and the obtained product performance is equivalent to that of the original epoxy resin.

CN118724696APending Publication Date: 2024-10-01SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410780933.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to efficiently recycle waste epoxy resin with existing technology, leading to resource waste and environmental pollution. Existing chemical recycling methods have problems such as high energy consumption and the use of corrosive solvents.

Method used

By degrading epoxy resin and ethylene glycol at low temperature to obtain epoxy degradation products, NaOH is used for alkaline hydrolysis to generate sodium cyclohexene-2-carboxylate, which is then acidified and recycled to prepare 4-Cyclohexene-1,2-dicarboxylic acid enables efficient recovery and reuse of epoxy resin.

Benefits of technology

It achieves normal pressure, rapid and complete depolymerization and separation of epoxy resin. The recycled epoxy resin monomer obtained has the same comprehensive properties as the original epoxy resin, reducing resource waste and environmental pollution, and the process conditions are optimized. Improved recovery efficiency and purity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724696A_ABST
    Figure CN118724696A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of 4-cyclohexene-1, 2-dicarboxylic acid, the 4-cyclohexene-1, 2-dicarboxylic acid is prepared by recycling epoxy resin, and the preparation method comprises the following steps: a, degrading the epoxy resin; and b, adding NaOH into the degradation product, removing water, and adding the degradation product into ethanol to obtain a sodium salt precipitate, namely cyclohexene-2-sodium carboxylate R-THA-Na. The invention also provides a preparation method of the epoxy resin. According to the invention, EG and sodium hydroxide are successively used for depolymerizing the polyester epoxy / amine condensate, so that the condensate can be quickly and thoroughly depolymerized and separated under normal pressure, and a new process for recovering the ester epoxy / amine condensate is formed; the acidity value obtained after acidification of sodium salt is 467.3 mg KOH / g, the purity is 99%, an original epoxy resin monomer structure is obtained after epoxidation of the acid, and the comprehensive performance of the epoxy resin is equivalent to that of original epoxy resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing 4-cyclohexene-1,2-dicarboxylic acid. Background Art

[0002] Sodium cyclohexene-2-carboxylate is an organic compound that is often used as an intermediate in organic synthesis. It has a cyclohexene ring and a sodium carboxylate functional group, which makes it very useful in the synthesis of various chemicals and materials. Sodium cyclohexene-2-carboxylate can participate in a variety of chemical reactions, including addition reactions, substitution reactions, and polymerization reactions.

[0003] In recent decades, the application of thermosetting materials in industrial fields has become more and more extensive, and has become an important industrial raw material. Wherein, epoxy resin is one of the most important thermosetting resins, because of its good thermodynamic properties, thermal stability, corrosion resistance and adhesion and other properties, it is widely used in many fields such as coatings, composite materials, vehicles and electronic packaging. However, once epoxy resin is cured and formed, because the rigid three-dimensional network structure cannot be repeatedly processed and formed and is difficult to recycle and reprocess, it has caused great waste of resources, and epoxy resin will produce a large amount of waste scraps after the service life, and the treatment method of composite material waste is mostly physical treatment and burning at present, which not only can cause environmental pollution, but also can produce great waste of resources. Therefore, the present invention has achieved the effective recycling of thermosetting resin by separating glycidyl ester alcoholysis product.

[0004] Separation and recovery of epoxy resin as initial material to form resource recycling is one of the important ways to achieve the sustainable development strategy of epoxy resin industry. The separation methods of thermosetting epoxy resin are mainly divided into mechanical separation method and chemical depolymerization method. Among the epoxy depolymerization chemical depolymerization methods that have been studied or industrially applied, they can be subdivided into hydrolysis method, acid hydrolysis method, alkaline hydrolysis method, alcohol-base combined method, etc. The recycling of fiber-reinforced resin composites is divided into four methods: mechanical recycling, pyrolysis process, fluidized bed process and chemical recycling.

[0005] At present, the current status of epoxy resin separation research is:

[0006] (1) Mechanical separation method: The mechanical separation method is to cut or grind the epoxy resin material, and then recycle it as a filler into a new epoxy resin composite material for reuse. This method is easy to operate and has low cost, but it is only a physical separation during the separation process, which only destroys the original size of the long fiber. The resulting short fibers can only be used as fillers, which loses a lot of use value.

[0007] Jutte et al. physically cut the discarded epoxy resin material and then crushed it into powder. The powder was added to the newly produced epoxy resin as a filler and reinforcement. Although the physical and chemical properties of the newly obtained epoxy resin were reduced, it can still be used in some occasions.

[0008] Kouparitsas et al. used a pulverizer and classification screen to cut and crush the epoxy resin, recovered the part with high chopped fiber content, and then added it back into the new composite material to test its physical properties. There was only slight loss and it could still be reused.

[0009] (2) Hydrolysis: Hydrolysis and oxidation in subcritical and supercritical water have been widely studied as methods for converting organic waste into carbon dioxide and water. In the 1970s, M. Model proposed the properties of water in hydrolysis, hydrothermal and oxidation processes. Water plays a variety of roles in chemical reactions and can act as a reactant, product, catalyst, etc. This technology can be used to destroy epoxy resin, a polymer that is easily used in nuclear power plants. The organic network of epoxy resin is hydrolyzed and oxidized. Conditions such as temperature, pressure and reaction time will affect the hydrolysis. Low molecular weight degradation compounds are characterized by GC / MS technology. Epoxy resin is completely destroyed by oxidation at 410°C and 24MPa. The experimental conditions for the complete separation and recovery of epoxy resin by hydrolysis are relatively harsh, making it difficult to be widely put into industrial production.

[0010] (3) Acid hydrolysis: The acid hydrolysis of epoxy resin is an important series of reactions used in the polymer industry (including coatings and rubbers). Neodecanoic acid glycidyl ester is a green material for environmentally friendly coatings. Yan Zifei et al. synthesized it through the acid hydrolysis reaction of epichlorohydrin (ECH) and neodecanoic acid. A green catalyst called tetramethylammonium neodecanoate (TMAN) was developed. TMAN is completely recyclable and the reaction system can be uniform, thus combining the advantages of tertiary amines and quaternary ammonium salts while eliminating their disadvantages. Compared with the traditional industrial catalyst tetramethylammonium chloride (TMAC), the amount of byproduct dichloropropane can be reduced by more than 50%, the effective utilization rate of ECH and the yield of the main product are increased by 5% and 2% respectively, and the reaction time can be shortened by more than 20%.

[0011] Epoxy resins are considered to be among the top materials in terms of chemical resistance; contrary to the common assumption that acid degradation is a chemical degradation process, the actual mechanism of epoxy resins is a physical degradation process driven by aggressive plasticization of the amine-cured epoxy thermoset matrix as the diffusing ionic species bind to the polar moieties and break the non-covalent bonds within the polymer network. The ensuing non-equilibrium swelling behavior leads to physical erosion as the primary degradation mechanism. Diffusion of acidic electrolytes into the thermoset matrix leads to a corresponding degradation of the material properties and even controlled chemical degradation of the thermoset resin matrix to enable composite fiber recycling and polymer recycling.

[0012] (4) Alkaline hydrolysis: Chien et al. treated waste circuit boards through the oxidation of supercritical water. By adding hydrogen peroxide and alkali solution, epoxy resin can be completely decomposed. In their research on the recycling of waste printed circuit boards, Xu Min et al. added sodium chloride, acetic acid and sodium hydroxide as catalysts. Compared with the decomposition effect of pure water, sodium hydroxide promoted the decomposition of epoxy resin. These experiments show that alkaline systems can provide more hydroxide ions to promote resin depolymerization. Compared with water immersion, the alkaline solution environment promotes the hydrolysis reaction of epoxy resin molecular chains.

[0013] (5) Alcohol-base combined method: Compared with the above-mentioned hydrolysis, acid hydrolysis and alkaline hydrolysis methods, the alcohol-base combined method has defects, such as harsh reaction conditions, incomplete dissociation, difficulty in separating intermediate products, slow reaction speed and high cost. The new process for chemical decomposition of epoxy resin waste by Chongqing University in China - alcohol-base combined separation of epoxy resin process is relatively mature. It uses EG and Lewis base as raw materials to depolymerize epoxy resin under normal pressure and relatively low temperature conditions. Wang Shanshan et al. optimized and simplified the process conditions based on the research of Chongqing University. Under normal pressure, relatively low temperature and environmentally friendly experimental conditions, PET is depolymerized by alcohol first and then by alkali: ethylene glycol is used to alcoholize epoxy resin, and then the alcoholysis solution is hydrolyzed by sodium hydroxide, and then the generated sodium salt is acidified to obtain TPA and EG and other substances that can be recycled. While simplifying the process conditions, compared with other processes such as acid hydrolysis or hydrolysis, it is more in line with the reaction mechanism of epoxy resin depolymerization.

[0014] The recycling of epoxy resin can be roughly divided into material recycling and energy recycling. Among them, energy recovery is mostly carried out through incineration (heat recovery), while material recycling is divided into: chemical recycling, mechanical recycling, electrical recycling and biotechnology recycling. The latter three are not common, while chemical recycling and heat recovery have been extensively studied, and heat recovery is a common technology used in industry. Chemical recycling is more environmentally friendly and economical than heat recovery, so chemical recycling has gradually been put into industrial applications with the progress of scientific research.

[0015] Next, we will focus on reviewing the research on chemical recycling:

[0016] Chemical recycling is done by breaking the matrix polymer bonds using a suitable solvent at appropriate temperature and pressure. The process parameters are usually lower than for pyrolysis processes. Chemical processes can be divided into solvolytic processes, which means the breaking of primary (intramolecular) bonds, and solvent-based processes, where only secondary (intermolecular) bonds are dissolved without damaging the macromolecules. Usually these processes are carried out in ambient atmosphere, but a nitrogen purge can also be performed to prevent decomposition of specific solvents.

[0017] Knappich F et al. found that solvent decomposition can be carried out under subcritical or supercritical conditions. Under supercritical conditions, bodies have special characteristics. Good diffusivity enables them to penetrate porous solids like steam. The solubility is high, and the removal of the product is guaranteed because the mass transfer coefficient is increased compared to the liquid. Another advantage of the supercritical process is that the solvent used is harmless under normal conditions. In the study, the most commonly used solvent is water, sometimes combined with alcohol, phenol or amine, and organic solvents such as benzyl alcohol, methanol, ethanol, propanol, acetone or ethylene glycol have also been studied, usually under alkaline conditions. The disadvantages of the supercritical process are high temperatures of more than 400 ° C and pressures of more than 600 bar, which lead to high energy consumption and require sturdy equipment. In contrast, the solvent decomposition process under subcritical conditions usually requires corrosive solvents such as nitric acid, sulfuric acid or acid, which are harmful to people and the environment. For dissolution of epoxy resins, for example, nitric acid has been applied at 8°C for 90 min, or a mixture of hydrogen peroxide and N,N-dimethylformamide has been used at 90°C for 30 min, both of which are corrosive and toxic to organisms.

[0018] Ma Y et al. applied depolymerization and acid digestion to amine / epoxy composites, including composites produced from laboratory fabrication and aerospace prepregs, as well as commercial composite waste. The results showed that acid digestion was more effective than depolymerization for highly cross-linked amine / epoxy composites. The relationship between epoxy functionality, fiber bed structure, fiber reinforcement, laminate thickness and matrix dissolution rate was investigated, and the key parameters affecting the dissolution rate were identified. The data showed that the main rate-limiting factor for acid digestion is the diffusion rate, not the chemical reaction rate. Two strategies to increase the diffusion rate, pretreatment and mechanical shredding, were evaluated and both were effective.

[0019] The existing technology does not efficiently recycle the effective components in the waste resin, resulting in the current low recycling rate of the waste resin. Summary of the invention

[0020] The invention provides a method for preparing 4-cyclohexene-1,2-dicarboxylic acid, which is prepared by recycling epoxy resin.

[0021] The present invention provides a method for preparing 4-cyclohexene-1,2-dicarboxylic acid, which is prepared by recycling epoxy resin and comprises the following steps:

[0022] a. Epoxy resin degradation:

[0023] Take epoxy resin, add ethylene glycol EG in a mass ratio of 1:9, pass nitrogen, heat to 180°C for degradation, and remove the solvent EG by vacuum distillation of the mixed solution after degradation to obtain a viscous epoxy degradation product DEP;

[0024] b. Add NaOH to the epoxy degradation product DEP, remove water, and add ethanol to obtain a sodium salt precipitate, which is cyclohexene-2-carboxylate sodium R-THA-Na.

[0025] Wherein, the epoxy monomer used in the epoxy resin has an ester bond structure.

[0026] Wherein, the alkaline hydrolysis temperature in step b is 60-100° C.; the reaction time is 2.5-10 hours; the mass ratio of epoxy degradation product DEP to NaOH is: 10:(2.0-3.0); and the concentration of sodium hydroxide is 5%-20%.

[0027] Further preferably, the alkaline hydrolysis temperature in step b is 60° C.; the reaction time is 2.5 h; the mass ratio of epoxy degradation product DEP to NaOH is 10:2; and the concentration of sodium hydroxide is 10%.

[0028] The present invention also provides application of the prepared 4-cyclohexene-1,2-dicarboxylic acid in the preparation of epoxy resin.

[0029] The present invention also provides a method for preparing an epoxy resin, which comprises the following steps:

[0030] a. Take the prepared sodium cyclohexene-2-carboxylate R-THA-Na, add 5 mol / L sulfuric acid solution to adjust the pH of the solution to 2, age it to obtain a white solid precipitate, filter and dry the precipitate to obtain R-THA;

[0031] b. R-THA, epichlorohydrin ECH, and benzyltrimethylammonium chloride in a molar ratio of 1:8-16:0.015-0.025 are heated to 100°C for reaction for 1 hour, and then cooled to 55°C, and a 20wt% NaOH aqueous solution is added dropwise until the pH value is 7. The upper layer of water is removed by a separatory funnel, and ECH is removed by rotary evaporation to obtain a recycled epoxy monomer (R-EP);

[0032] c. R-EP epoxy is used as a monomer and IPDA as a curing agent. After the two are mixed evenly, they are poured into a mold coated with a silicone release agent and placed in a vacuum drying oven for degassing until the bubbles are completely expelled. After the bubbles are removed, they are placed in a blast oven at 80°C for curing for 6 hours, and then taken out after cooling to room temperature to obtain the recycled epoxy resin R-EP+IPDA.

[0033] Wherein, the reaction temperature of the sodium salt acidification in step a is 25°C-75°C; the reaction time is 0.5-2h; the sodium salt concentration is 10%-20%; and the aging time is 24h-72h.

[0034] Further preferably, the reaction temperature of the sodium salt acidification in step a is 50° C.; the reaction time is 0.5 h; the sodium salt concentration is 20%; and the aging time is 72 h.

[0035] Further preferably, the molar ratio of R-THA, epichlorohydrin ECH and benzyltrimethylammonium chloride in step b is 1:13:0.015.

[0036] The beneficial effects of the present invention are:

[0037] (1) Using EG and sodium hydroxide to decompose polyester epoxy / amine curing materials in sequence can achieve normal pressure, rapid and complete depolymerization and separation of curing materials, becoming a new process for recycling ester epoxy / amine curing materials.

[0038] (2) The acidity value obtained after acidification with sodium salt is 467.3 mg KOH / g and the purity is 99%. After epoxidation of the acid, the original epoxy resin monomer structure is obtained, and its comprehensive performance is equivalent to that of the original epoxy resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The preparation method of 4-cyclohexene-1,2-dicarboxylic acid and the synthesis flow chart of recycled epoxy of the present invention;

[0040] Figure 2 (a) Degradation efficiency of epoxy block ethylene glycol system at different times (b) GPC of degradation products;

[0041] Figure 3 Degradation mechanism of epoxy resin in alcohol solution;

[0042] Figure 4 Degradation mechanism of DEP using NaOH;

[0043] Figure 5 Orthogonal test sodium salt H NMR spectrum;

[0044] Figure 6 Structural analysis of R-THA-NA and THA-NA (A) IR spectrum (b) H NMR spectrum;

[0045] Figure 7 R-THA structural analysis (a) IR spectrum (b) H NMR spectrum;

[0046] Figure 8 R-EP structural analysis (a) IR spectrum (b) H-NMR spectrum;

[0047] Fig. 9 Comprehensive properties of R-EP+IPDA ((a) Epoxy resin R-EP (b) DSC analysis of R-EP+IPDA (c) DTG analysis of R-EP+IPDA (d) Stress-strain diagram of R-EP+IPDA). DETAILED DESCRIPTION

[0048] Example 1 Preparation method of 4-cyclohexene-1,2-dicarboxylic acid and synthesis of recycled epoxy

[0049] (1) Preparation of epoxy resin cured product

[0050] Tetrahydrophthalic acid diglycidyl ester (TADE) is used as a monomer and isophorone diamine (IPDA) is used as a curing agent. After mixing the two evenly, pour them into a mold coated with a silicone release agent and place them in a vacuum drying oven for degassing until the bubbles are completely discharged. After the bubbles are removed, place them in a blast oven at 80°C for curing for 6 hours. After the curing is completed, wait for them to cool to room temperature and then take them out to obtain epoxy resin cured material specimens, which are marked as EP. The specimens EP are cut into uniform specimens with a size of 10mm×10mm×2mm by a cutting machine for later use.

[0051] (2) Degradation of epoxy cured products

[0052] A uniform sample of 10mm×10mm×2mm in size and EG were added into a three-necked flask at a mass ratio of 1:9. After nitrogen was passed through the device to exhaust the gas in the device, the temperature was raised to 180℃ for degradation. Subsequently, the mixed liquid after degradation was distilled under reduced pressure to remove the solvent EG, and a viscous epoxy degradation product was obtained, which was named DEP in the experiment.

[0053] DEP was further degraded with NaOH to prepare sodium salt. The liquid obtained by alkaline hydrolysis was subjected to a rotary evaporator to remove water, and then ethanol was added to obtain a sodium salt precipitate. The recovered sodium cyclohexene-2-carboxylate was named (R-THA-Na) in the experiment.

[0054] (3) Recycling of DEP

[0055] A 5 mol / L sulfuric acid solution was added dropwise to the R-THA-Na aqueous solution to adjust the pH of the solution to 2, thereby obtaining a white solid precipitate. The precipitate was filtered and dried to obtain the acid (R-THA).

[0056] (4) Synthesis of recycled epoxy

[0057] Add acid, ECH and benzyltrimethylammonium chloride in a molar ratio of 1:13:0.015 to a three-necked flask equipped with a thermometer, a stirring device and a reflux condenser, heat to 100°C and react for 1 hour, wait for it to cool to 55°C, add 20wt% NaOH aqueous solution until pH=7, remove the upper layer of water through a separatory funnel, and remove ECH by rotary evaporation to obtain a recycled epoxy monomer (R-EP). R-EP epoxy is used as a monomer and IPDA is used as a curing agent. After the two are mixed evenly, pour them into a mold coated with a silicone release agent and place them in a vacuum drying oven for degassing until the bubbles are completely discharged. After the bubbles are removed, place them in a blast oven at 80°C for curing for 6 hours, and take them out after cooling to room temperature. The recycled epoxy resin cured material specimen is obtained and marked as (R-EP+IPDA). (See Figure 1 )

[0058] Example 2 Parameter screening test of the preparation method of the present invention

[0059] 1. Experimental steps

[0060] (1) Two-step degradation of epoxy resin cured products

[0061] A uniform sample of size 10mm×10mm×2mm and EG are added into a three-necked flask at a mass ratio of 1:9. After nitrogen is passed through the device to exhaust the gas in the device, the temperature is raised to 180°C for degradation. Subsequently, the mixed solution after degradation is subjected to reduced pressure distillation to remove the solvent EG to obtain a viscous epoxy degradation product, which is named DEP in the experiment. Solid epoxy resin samples are taken out from the solution at regular intervals, cleaned and weighed to monitor the change of residual mass over time. By measuring the residual mass (m t ) to the original solid mass (m0) t / m0) to monitor the catalytic degradation rate of epoxy resin.

[0062] DEP was further degraded with NaOH and sodium salt was prepared. The liquid obtained by alkaline hydrolysis was used to remove water by a rotary evaporator, and then ethanol was added to obtain a sodium salt precipitate. The recovered sodium cyclohexene-2-carboxylate was named (R-THA-Na) in the experiment. In order to explore the effect of NaOH on the separation effect of DEP, four factors were considered, including reaction temperature (A), reaction time (B), the ratio between DEP and sodium hydroxide (C), and sodium hydroxide concentration (D). Each factor includes 3 levels: A: 60℃, 80℃, 100℃; B: 2.5h, 5h, 10h; C: 10:2, 10:2.5, 10:3; D: 5%, 10%, 20%. The level of each factor level (Table 1) and the orthogonal table L9 (34) is selected without considering the interactions between factors.

[0063] Table 1 Alkaline hydrolysis experimental factors and levels

[0064]

[0065] (2) Recycling of DEP

[0066] ①Sodium chloride acidification

[0067] In order to explore the effect of acidification, the effects of four factors were considered, including reaction temperature (A), sodium salt concentration (B), reaction time (C), and aging time (D), and each factor included 3 levels: A: 25°C, 50°C, 75°C; B: 10%, 15%, 20%; C: 0.5h, 1h, 2h; D: 24h, 48h, 72h. The level of each factor level (Table 2) and the orthogonal table L9 (34) is selected without considering the interactions between factors.

[0068] Table 2 Acidification experimental factors and levels

[0069]

[0070] 5 mol / L sulfuric acid solution was added dropwise to each group of experiments to adjust the pH of the solution to 2, and a white solid precipitate was obtained. The precipitate was filtered and dried to obtain the acid (R-THA).

[0071] ②Synthesis of recycled epoxy

[0072] In a three-necked flask equipped with a thermometer, a stirring device and a reflux condenser, an acid, ECH and benzyltrimethylammonium chloride in a molar ratio of 1:13:0.015 were added, the temperature was raised to 100°C for reaction for 1 hour, and after cooling to 55°C, a 20wt% NaOH aqueous solution was added dropwise until the pH value was 7, the upper layer of water was removed by a separatory funnel, and the ECH was removed by rotary evaporation to obtain a recycled epoxy monomer (R-EP).

[0073] R-EP epoxy is used as a monomer and IPDA as a curing agent. After the two are mixed evenly, they are poured into a mold coated with a silicone release agent and placed in a vacuum drying oven for degassing until the bubbles are completely discharged. After the bubbles are removed, they are placed in a blast oven at 80°C for curing for 6 hours and can be taken out after cooling to room temperature. The recycled epoxy resin cured material specimen is obtained and marked as (R-EP+IPDA).

[0074] 2. Testing and Characterization

[0075] (1) H NMR spectroscopy ( 1 H NMR)

[0076] The sodium salt (R-THA-Na), acid (R-THA), and epoxy (R-EP) were analyzed using a nuclear magnetic resonance spectrometer from Bruker, Switzerland. 1H NMR. R-THA-Na uses deuterated H2O reagent to dissolve the sodium salt, R-THA and R-EP use deuterated dimethyl sulfoxide reagent to dissolve, and TMS is used as the internal standard for testing.

[0077] (2) Infrared spectroscopy (FT-IR)

[0078] The infrared spectra of sodium salt (R-THA-Na) and acid (R-THA) were tested at room temperature using an infrared spectrometer (Nicolet-5700) from Nicolet Corporation of the United States. The samples were prepared using the KBr pellet method.

[0079] (3) Differential Scanning Calorimetry (DSC)

[0080] The glass transition temperature of the synthesized product (R-EP / IPDA) was tested using NETZSCH (STA 449C) in a temperature range of 20-250°C, a heating rate of 10°C / min, and a test atmosphere of N2.

[0081] (4) GPC

[0082] The molecular weight and distribution of DEP were characterized by gel chromatography (PL-GPC220) produced by PL Company of Britain, and polystyrene standards were used for calibration. Tetrahydrofuran was used as eluent.

[0083] (5) Thermal weight loss

[0084] The thermal stability of R-EP / IPDA was tested using a German NETZSCH STA449C comprehensive thermal analyzer in a nitrogen atmosphere at a gas flow rate of 30 mL / min, a temperature range of 30 to 800 °C, and a heating rate of 10 °C / min.

[0085] (6) Mechanical properties test

[0086] The tensile properties of the cured specimens (R-EP / IPDA) were tested using an electronic universal testing machine (ETM-104C) from Shenzhen WanCe Testing Co., Ltd. The test was conducted in accordance with the GB / T1447-2005 test standard, with a tensile rate of 2 mm / min.

[0087] (7) Epoxy value test

[0088] The epoxy value of the product was determined by the hydrochloric acid acetone method. Take epoxy resin m (g) and add it to an experimental bottle containing the same volume of hydrochloric acid acetone solution (configured according to the volume ratio of hydrochloric acid: acetone = 1:40) as the experimental group, with a total of 5 groups. Add 2 to 3 drops of phenolphthalein indicator and leave it for about 30 minutes to allow the epoxy to fully dissolve in the solution. Set up 3 blank control groups. Prepare NaOH ethanol solution with c = 0.1 mol / L for titration, the titration volume is V1 (mL), and the blank control group is titrated V2. Calculate the average value of V2 as V.

[0089] Calculate according to formula 4-1 and take the average of the 5 groups of values.

[0090]

[0091] (8) Viscosity test

[0092] The viscosity of epoxy was tested using a digital viscometer (NDJ-8S) produced by Shanghai Fangrui Instrument Co., Ltd.

[0093] (9) Acid value test

[0094] Weigh 0.8-1.5% acid sample, add 20ml dimethyl sulfoxide to dissolve the acid, drop phenolphthalein as a color developer, and titrate with sodium hydroxide standard titration solution until the solution turns light red and does not fade for 30 seconds. Record the volume V (mL) of NaOH consumed. According to the reaction formula, Get the acid value.

[0095] 3. Results and Discussion

[0096] 3.1 Epoxy resin cured products degrade into oligomers in ethylene glycol (see Figure 2 )

[0097] The glycidyl ester / amine curing material selected by the present invention is a system with low viscosity and can be cured at low temperature (<90° C.), and can be used for large-scale potting devices such as wind turbine blades. Its degradation is in a surface erosion mode, and proceeds from the outside to the inside through a combination of ester exchange and alcohol diffusion, which meets the proven (Shrinking-core Model) shrinking core model.

[0098] The alcoholysis reaction between small molecule ethylene glycol and high molecular weight glycidyl ester / amine solids tends to generate diol esters, polyols and some oligomers in equilibrium. Figure 3 As shown in Figure 2, the substance can be completely degraded at 160°C under normal pressure, and its degradation efficiency is as follows: Figure 2 As shown in (a), it can be seen from the figure that the degradation can be completed in about 500 minutes. The degradation process is divided into two stages. In the first stage, the swelling rate is greater than the dissolution rate. When the maximum swelling rate is reached, the dissolution rate is greater than the swelling rate. Figure 2(b) and the gel permeation chromatography (GPC) analysis given in Table 3, the molecular weight of DEP is 10 14 , molecular weight distribution is 1.08, the solidified material is transformed from polymer to oligomer, and the final product is a mixture of various oligomers.

[0099] Table 3 Molecular weight and PDI of DEP

[0100]

[0101] 3.2 Further degradation of oligomers (see Figure 4 )

[0102] DEP was further degraded with NaOH, and the reaction equation was as follows Figure 4 First, ethylene glycol is used to degrade the epoxy curing material into oligomers and small molecules. Compared with the direct mixing and depolymerization method of alcohol and alkali in equal proportions,

[93] , avoiding the deposition of sodium cyclohexene-2-carboxylate on the surface of epoxy curing material to reduce the reaction speed and reducing side reactions. The infrared spectrum and nuclear magnetic hydrogen spectrum corresponding to the sodium salt separated from DEP are very similar to the structure of the standard substance, which also confirms the formation of sodium salt during alkaline hydrolysis. However, the separated sodium salt still retains the amine curing agent structure. The present invention uses the nuclear magnetic hydrogen spectrum of the sodium salt as the assessment index of product purity, and compares the nuclear magnetic hydrogen spectrum of the products obtained in each test with the standard product ( Figure 5), all the sodium salts separated in the experiment have peaks at chemical shifts of 5.71ppm and 2.79ppm, which correspond to the characteristic absorption peaks of hydrogen atoms on the double bond of cyclohexene. The displacements of 2.43ppm and 2.25ppm are the characteristic peaks of methylene hydrogen atoms on cyclohexene; the chemical shift of 2.79ppm is the characteristic absorption peak of hydrogen atoms connected to ester bonds, and the integral area ratio of the corresponding positions can be seen to be 1:1:1:1, which proves that the sodium salt is successfully separated. Compared with the standard substance, the sodium salts of each experiment also have peaks at displacements of 5.76ppm, 2.59ppm, 2.44ppm, and 2.07ppm, and the integral area ratio of each peak is 1:1:1:1. These The peak structure at the position corresponds to the trans structure of the separated sodium salt. In addition, the separated substance also peaks at chemical shifts of 1.19ppm, 1.06ppm, and 0.96ppm. These peak positions are characteristic peaks on the amine part. These peaks belong to the impurity peaks in the product. The purity of the product is judged by comparing the ratio of the integral area of ​​hydrogen atoms on the double bond of cyclohexene to the integral area of ​​the impurity peak at the chemical shift of 1.06ppm (Table 4). Finally, the range analysis of the comprehensive evaluation results is carried out. The range analysis results are listed in Table 5. From the range analysis, it can be seen that the order of influencing factors is sodium hydroxide concentration, reaction time, the ratio between DEP and sodium hydroxide, and reaction temperature. Sodium hydroxide concentration is the most critical factor for alkaline hydrolysis. The optimal process conditions are: reaction temperature is 60℃, reaction time is 2.5h, the ratio between DEP and sodium hydroxide is 10:2, and the sodium hydroxide concentration is 10%.

[0103] Table 4 Orthogonal table of factors affecting alkaline hydrolysis separation and range analysis results

[0104]

[0105]

[0106] Table 5 Orthogonal test H NMR spectrum analysis results

[0107]

[0108] The sodium salt obtained under the optimal process conditions of alkaline hydrolysis was subjected to infrared analysis, nuclear magnetic resonance analysis, and elemental analysis. Figure 6 As shown in (a), the C=O on the carboxylate has symmetric stretching and antisymmetric stretching vibrations, which can be observed from the infrared spectrum of R-THA-Na at 1582 cm -1 and 1378cm -1 The characteristic peaks at are the antisymmetric stretching and symmetric stretching of sodium salt, and both absorption peaks are relatively strong. Compared with the infrared spectrum of THA-Na, the peak positions of the infrared spectra of the two are basically the same. Figure 6(b) shows the one-dimensional hydrogen spectra of THA-Na and R-THA-Na. Both of them have peaks at chemical shifts of 5.71ppm, 2.79ppm, 2.43ppm, and 2.25ppm. The peak at chemical shift 5.71ppm corresponds to the characteristic absorption peak of hydrogen atoms on the double bond of cyclohexene. The chemical shifts of 2.43ppm and 2.25ppm are the characteristic peaks of methylene hydrogen atoms on cyclohexene. The chemical shift of 2.79ppm is the characteristic absorption peak of hydrogen atoms connected to ester bonds. It can be seen from the integrated area that the integrated area ratio of the corresponding positions is 1:1:1:1. Compared with THA-Na, R-THA-Na also has peaks at chemical shifts of 5.76ppm, 2.59ppm, 2.44ppm, and 2.07ppm, and the integrated area ratio of each peak is 1:1:1:1. The peak structures at these positions correspond to the trans structure of the separated sodium salt. The results show that the purity of the separated sodium salt is close to that of the standard DTA monomer. Table 6 shows the elemental analysis results of THA-Na and R-THA-Na, and the results show that the C, H, and N content of both are proportional, and the nitrogen content is negligible. Therefore, it can be shown that the purity of the separated sodium salt is close to that of the standard THA-Na monomer.

[0109] Table 6 Elemental analysis of R-THA-Na and THA-Na

[0110]

[0111] 3.3 Recycling of epoxy resin degradation products

[0112] (1) Acidification of epoxy degradation products with sodium salt

[0113] In the experiment, the separated R-THA-Na was further acidified to prepare acid (R-DTA). The influence of four factors was mainly considered. The experimental scheme and experimental results are shown in the table. The yield of each group of acidification was compared to evaluate. Finally, the comprehensive evaluation results were subjected to range analysis. The range analysis results are listed in Table 7. From the range analysis, it can be seen that the order of influencing factors is sodium salt concentration, reaction temperature, reaction time and aging time. Since the acidification process is the reverse process of acid-base neutralization, compared with acid-base neutralization, its reverse process requires higher reaction activation energy and more stringent reaction conditions. Therefore, the appropriate temperature is selected, which is more conducive to the reaction. The precipitation of sodium salt requires a certain amount of time, and a certain amount of aging is more conducive to the reaction. In the whole reaction process, sodium salt concentration is the most critical factor in the acidification process. This is because if the sodium salt concentration is too high, the sodium salt cannot be completely dissolved, which will affect the subsequent reaction. If the sodium salt concentration is too low, that is, water accounts for too much of the entire reaction system, the acid obtained by the reaction has a certain solubility in water, so it will eventually affect the yield of the experiment. The optimal process conditions are: reaction temperature of 50℃, reaction time of 0.5h, sodium salt concentration of 20%, and aging time of 72h.

[0114] Table 7 Orthogonal table of factors affecting acidification experiment and range analysis results

[0115]

[0116] Based on the above experiments, the sodium salt was further acidified, and its infrared Figure 7 As shown in (a), the most obvious change is at 1540cm -1 and 1398cm -1 The two strong absorption peaks at 1740 cm-1 (corresponding to the stretching vibrations of C=O and CO of the ester group in the sodium salt) disappeared, while the characteristic peak of carboxylic acid at 1740 cm-1 - and 920cm -1 This indicates that ACOOK is protonated to form ACOOH. Similar results are also confirmed in the HNMR graph ( Figure 7 (b)). Chemical shifts of 5.71 ppm and 5.58 ppm corresponding to the cyclohexene structure appeared in the sodium salt and acid. Due to the hydrolysis of the ester group to the carboxylic acid group, a characteristic peak of hydrogen on the carboxylic acid group with a chemical shift of 12.13 ppm appeared in the acid.

[0117] (2) Synthesis of recycled epoxy

[0118] The prepared acid was reacted with epichlorohydrin to obtain the epoxy resin monomer product R-EP, whose corresponding infrared spectrum and nuclear magnetic hydrogen spectrum were very similar to those of the standard substance ( Figure 8 ), from the nuclear magnetic hydrogen spectrum of the product, it can be seen that the chemical shift of 5.67ppm is the characteristic peak of the hydrogen atoms on cyclohexene; the chemical shifts of 4.38ppm and 3.85ppm have quartets, which are the characteristic absorption peaks of the hydrogen atoms of -O-CH2-, and the absorption peaks of the hydrogen atoms on CH2 on the epoxy group are at 2.62ppm and 2.37ppm, respectively, with two quartets; the chemical shift of 3.17ppm is the characteristic absorption peak of the hydrogen atoms on CH on the epoxy group, and the water peak and impurity peak appear at the chemical shift of 3.3ppm. It can be seen from the integrated area that the integrated area ratios corresponding to positions a, b, c, d, e, and f are 1:2:1:2:1:2, which proves the synthesis of diglycidyl tetrahydrophthalate. Similar results are also proved in the infrared graph. It can be seen from the spectrum that at 1640cm -1 The peak at 650cm is the stretching vibration peak of the product cyclohexene C=C; -1 ~730cm -1 The peak at 3500cm-1 can be determined to be the stretching vibration of the double bond CH. -1 The peak is the stretching vibration of -OH. The acid peak is 1690cm -1 The peak at 1728 cm is the characteristic peak of C=O of carboxyl group. -1The C=O stretching vibration peak of the ester bond is at 1126 cm -1 There is antisymmetric stretching vibration of COC, which is a strong absorption; the product is at 910cm -1 The absorption peak of epoxy group appeared at , indicating that the acid has been epoxidized.

[0119] (3) Comprehensive performance of R-EP

[0120] like Fig. 9 As shown in (a), the product synthesized in the experiment is diglycidyl tetrahydrogen diacid ester. The product is a light yellow transparent liquid at room temperature. Its viscosity at room temperature (25°C) is 797mPa.s as measured by a viscometer; its epoxy value is 0.63mol / 100g as measured by the hydrochloric acid-acetone method. The comprehensive properties of R-EP+IPDA and S-EP+IPDA were tested by DSC, DTG and universal tensile machine, as shown in Figure 1. Fig. 9 (b)(c)(d) As shown in the figure, the thermal and mechanical properties of the recycled epoxy are not significantly different from those of the original epoxy. g is 104℃. From the thermogravimetric data (Table 8), it can be obtained that T 5% , T 10% and T max The temperature of the recycled epoxy is about 282℃, 295℃ and 342℃ respectively. In general, the recycled epoxy has the same excellent thermal properties as the original epoxy. From the stress-strain curve, it can be seen that the mechanical strength of the recycled epoxy is 65MPa and the elongation at break is 8.8%. Compared with the original epoxy, its mechanical properties remain excellent.

[0121] Table 8 Analysis of thermal gravimetric loss results of R-EP+IPDA and S-EP+IPDA

[0122]

[0123] 4 Summary

[0124] The present invention takes the glycidyl ester / amine curing system as the research object, degrades the curing, separates the monomers that can be used to prepare the raw material epoxy from the degradation products, and uses the orthogonal experimental design method to explore the influencing factors of the separation alkaline hydrolysis process. Finally, the availability of recycled epoxy is explored, and the following conclusions are drawn:

[0125] (1) Using EG and sodium hydroxide to decompose polyester epoxy / amine curing materials in sequence can achieve normal pressure, rapid and complete depolymerization and separation of curing materials, becoming a new process for recycling ester epoxy / amine curing materials.

[0126] (2) The optimal alkaline hydrolysis process conditions are: reaction temperature of 60°C, reaction time of 2h, ratio of DEP to sodium hydroxide of 10:2, and sodium hydroxide concentration of 10%. Under these conditions, the purity of R-THA-Na is optimal.

[0127] (3) The optimal acidification process conditions are: reaction temperature of 60°C, reaction time of 0.5h, sodium salt concentration of 20%, and aging time of 72h. Under this condition, the yield of R-THA is the highest.

[0128] (4) The acidity value obtained after acidification with sodium salt is 467.3 mg KOH / g and the purity is 99%. After epoxidation of the acid, the original epoxy resin monomer structure is obtained, and its comprehensive performance is equivalent to that of the original epoxy resin.

Claims

1. A method for preparing 4-cyclohexene-1,2-dicarboxylic acid, characterized in that: It is prepared by recycling epoxy resin, including the following steps: a. Epoxy resin degradation: Take epoxy resin, add ethylene glycol EG in a mass ratio of 1:9, pass nitrogen, heat to 180°C for degradation, and remove the solvent EG by vacuum distillation of the mixed solution after degradation to obtain a viscous epoxy degradation product DEP; b. Add NaOH to the epoxy degradation product DEP, remove water, and add ethanol to obtain a sodium salt precipitate, which is cyclohexene-2-carboxylate sodium R-THA-Na.

2. The method for preparing 4-cyclohexene-1,2-dicarboxylic acid according to claim 1, characterized in that: The epoxy monomer used in the epoxy resin has an ester bond structure.

3. The method for preparing 4-cyclohexene-1,2-dicarboxylic acid according to claim 1, characterized in that: The alkaline hydrolysis temperature in step b is 60-100° C.; the reaction time is 2.5-10 hours; the mass ratio of epoxy degradation product DEP to NaOH is 10:(2.0-3.0); and the concentration of sodium hydroxide is 5%-20%.

4. The method for preparing 4-cyclohexene-1,2-dicarboxylic acid according to claim 3, characterized in that: The alkaline hydrolysis temperature in step b is 60° C.; the reaction time is 2.5 h; the mass ratio of epoxy degradation product DEP to NaOH is 10:2; and the concentration of sodium hydroxide is 10%.

5. Use of the 4-cyclohexene-1,2-dicarboxylic acid prepared according to any one of claims 1 to 4 in the preparation of epoxy resin.

6. A method for preparing an epoxy resin, characterized in that: It includes the following steps: a. Take the sodium cyclohexene-2-carboxylate R-THA-Na prepared according to any one of claims 1 to 4, add 5 mol / L sulfuric acid solution to adjust the pH of the solution to 2, age it to obtain a white solid precipitate, filter and dry the precipitate to obtain R-THA; b. R-THA, epichlorohydrin ECH, and benzyltrimethylammonium chloride in a molar ratio of 1:8-16:0.015-0.025 are heated to 100°C for reaction for 1 hour, and then cooled to 55°C, and a 20wt% NaOH aqueous solution is added dropwise until the pH value is 7. The upper layer of water is removed by a separatory funnel, and ECH is removed by rotary evaporation to obtain a recycled epoxy monomer (R-EP); c. R-EP epoxy is used as a monomer and IPDA as a curing agent. After the two are mixed evenly, they are poured into a mold coated with a silicone release agent and placed in a vacuum drying oven for degassing until the bubbles are completely expelled. After the bubbles are removed, they are placed in a blast oven at 80°C for curing for 6 hours, and then taken out after cooling to room temperature to obtain the recycled epoxy resin R-EP+IPDA.

7. The method for preparing the epoxy resin according to claim 6, characterized in that: The reaction temperature of the sodium salt acidification in step a is 25°C-75°C; the reaction time is 0.5-2h; the sodium salt concentration is 10%-20%; and the aging time is 24h-72h.

8. The method for preparing the epoxy resin according to claim 7, characterized in that: The reaction temperature of the sodium salt acidification described in step a is 50°C; the reaction time is 0.5h; the sodium salt concentration is 20%; and the aging time is 72h.

9. The method for preparing an epoxy resin according to claim 6, wherein: The molar ratio of R-THA, epichlorohydrin ECH and benzyltrimethylammonium chloride described in step b is 1:13:0.015.

Citation Information

Cited By