TADF quaternary phosphonium salt scintillator material and preparation method and application thereof
By designing TADF quaternary phosphonium salt materials with a host-guest structure and using halogen components to improve X-ray absorption capabilities, the deficiencies of existing organic scintillator materials in X-ray absorption and exciton utilization are solved, achieving high efficiency and low cost. Preparation of organic scintillator materials.
Patent Information
- Application Number
- CN202410814815.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-24
AI Technical Summary
Existing organic scintillator materials perform poorly in terms of X-ray absorption capacity and exciton utilization, and the synthesis steps are complex and costly, making it difficult to achieve large-scale commercial production.
Using TADF quaternary phosphonium salt material, using the quaternary phosphonium nucleus as the electron acceptor and dimethylamine as the electron donor, we design molecules with a host-guest structure, use halogen components to improve X-ray absorption capabilities, and simplify the process through one-step synthesis.
It achieves high X-ray absorption capacity and high exciton utilization, simplifies the synthesis route, reduces costs, significantly improves light energy yield and photoluminescence quantum efficiency, and has excellent luminescence properties.
Smart Images

Figure CN118724955A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of organic light-emitting materials, and in particular to a TADF quaternary phosphonium salt scintillator material and a preparation method and application thereof. Background Art
[0002] Scintillator materials can convert high-energy particles (such as X-rays, gamma rays, beta particles, etc.) into ultraviolet light or visible light, and play a vital role in medical imaging, security inspection, industrial flaw detection, non-destructive testing and other fields.
[0003] Scintillators can be divided into two categories: inorganic scintillators and organic scintillators. Most inorganic scintillators are bulk single crystals. Currently, the most common commercial inorganic scintillators include sodium iodide (NaI), cesium iodide (CsI), bismuth germanate (BGO), Lu 1.8 Y 0.2 SiO5:Ce(LYSO), etc. However, inorganic scintillators are mainly prepared by the Bridgman method, which requires high temperature (>1000℃) and a high vacuum environment. The single crystal growth rate is slow, resulting in high cost. In addition, inorganic scintillators have poor mechanical flexibility and are difficult to be processed into the required shape. Compared with inorganic scintillators, organic scintillators have the inherent advantages of short radiation decay time, diverse structure, rich element reserves, easy raw materials, high mechanical flexibility, low temperature synthesis, and easy processing. However, the poor X-ray absorption ability and low exciton utilization rate of organic scintillators cause their scintillation performance to lag far behind that of inorganic scintillators. For example, anthracene, the most widely used organic scintillator, has a light energy yield of only 12,000 photons / MeV, which is much lower than that of inorganic scintillators.
[0004] Thermally activated delayed fluorescence (TADF) molecules have important applications in organic electroluminescent devices due to their high exciton utilization rate. The energy level difference between the singlet and triplet states of TADF molecules is relatively small. Among the excitons generated by electrical excitation, 75% are triplet excitons. Triplet excitons can overcome the energy barrier between the triplet and singlet states, reach the singlet state through antisystem crossing, and then radiate to produce TADF. The theoretical exciton utilization rate of TADF molecules is 100%. In order to ensure high triplet exciton utilization efficiency, the energy level difference between the singlet and triplet states of TADF molecules needs to be as small as possible. Quantum chemical calculation results show that by designing the host-guest structure within the molecule, a small singlet and triplet energy level difference can be achieved, so that the HOMO and LUMO orbits are localized on the donor and acceptor of the molecule, respectively. Although a variety of host-guest type TADF molecules have been reported in domestic and foreign literature, and the corresponding OLED devices have also shown excellent performance, the TADF molecules in the prior art are pure organic materials, containing carbon and hydrogen, and have poor absorption capacity for X-rays, making them unsuitable as scintillator materials. In addition, the synthesis steps of most organic molecules with host-guest structures are relatively complicated, requiring multiple steps of reaction, low yield, high cost, and requiring the use of some expensive precious metal catalysts. Therefore, it is urgent to develop an organic scintillator material with excellent performance, simple synthesis route, low cost, and large-scale commercial production. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a TADF quaternary phosphonium salt scintillator material and a preparation method and application thereof.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] In the first aspect, the present invention provides a TADF quaternary phosphonium salt scintillator material, referred to as R-NMe2PTPP-X, the structural formula of the material is:
[0008]
[0009] Wherein, the R is an alkyl group or an aromatic substituent; and the X is a halogen.
[0010] The invention uses a quaternary phosphonium core as an electron acceptor and dimethylamine as an electron donor, and uses a one-step method to react 2-diphenylphosphino-2'-(N,N-dimethylamino)biphenyl as a raw material with halogenated alkanes or halogenated aromatic hydrocarbons in a solvent to obtain a TADF quaternary phosphonium salt molecule with a host-guest structure.
[0011] The quaternary phosphonium derivative (PR3 +) is positively charged, has strong electron accepting ability, and is a suitable electron acceptor; nitrogen-containing and oxygen-containing functional groups are suitable electron donors. In the same molecule, a quaternary phosphonium salt material with an intramolecular host-guest structure is obtained by reaction, and the halogen component in the quaternary phosphonium salt has a large atomic number and has a strong absorption capacity for X-rays, which can effectively improve the X-ray attenuation capacity of the material. The 1mm thick TADF quaternary phosphonium salt scintillator material of the present invention can absorb 53.48% of X-rays, the photoluminescence quantum efficiency is close to 100%, and the light energy yield is 80817photons / MeV, which is an organic scintillator material with excellent luminescence performance.
[0012] As a preferred embodiment of the TADF quaternary phosphonium salt scintillator material of the present invention, the alkyl group is any one of a chain methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group and its derivatives, a cyclic cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group and its derivatives; the aromatic substituent is any one of a benzyl group, a phenethyl group, a phenpropyl group, a phenbutyl group, a phenpentyl group, 9-(2-ethyl)carbazole and its derivatives; the halogen is any one of chlorine, bromine and iodine.
[0013] In a second aspect, the present invention provides a method for preparing the TADF quaternary phosphonium salt scintillator material, comprising the following steps: dissolving 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl and halogenated alkane or halogenated aromatic hydrocarbon in a solvent for reaction, and collecting the precipitated product.
[0014] As a preferred embodiment of the method for preparing the TADF quaternary phosphonium salt scintillator material of the present invention, the halogenated alkane is any one of chain halogenated methane, halogenated ethane, halogenated propane, halogenated butane, halogenated pentane, halogenated hexane and their derivatives, cyclic halogenated cyclopropane, halogenated cyclobutane, halogenated cyclopentane, halogenated cyclohexane and their derivatives; the halogenated aromatic hydrocarbon is any one of halogenated benzyl, halogenated ethylbenzene, halogenated phenylpropane, halogenated phenylbutane, halogenated phenylpentane, 9-(2-haloethyl)carbazole and its derivatives; preferably, the halogen is any one of chlorine, bromine and iodine.
[0015] As a preferred embodiment of the method for preparing the TADF quaternary phosphonium salt scintillator material of the present invention, the solvent is at least one of toluene, ethyl acetate, methanol, tetrahydrofuran, n-hexane, and N,N-dimethylformamide.
[0016] As a preferred embodiment of the method for preparing the TADF quaternary phosphonium salt scintillator material of the present invention, the reaction temperature is controlled to be between room temperature and 150°C.
[0017] In a third aspect, the present invention provides a thin film comprising the TADF quaternary phosphonium salt scintillator material and a polymer; the mass ratio of the TADF quaternary phosphonium salt scintillator material and the polymer is (0.1-2):1.
[0018] In a fourth aspect, the present invention provides a method for preparing the film, comprising the following steps: mixing the TADF quaternary phosphonium salt scintillator material with a polymer, heating and melting, scraping and coating it on a substrate, and cooling. The heating and melting temperature is higher than the melting temperature of the polymer; the substrate is a substrate such as quartz or transparent glass. The film prepared by the preparation method can be used as an X-ray scintillation imaging screen to image school bags, peanuts, shrimps, etc., demonstrating its application potential in the fields of safety inspection, nondestructive testing, and agricultural seed selection.
[0019] In a fifth aspect, the present invention provides applications of the TADF quaternary phosphonium salt scintillator material and the thin film in organic light-emitting devices.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The TADF quaternary phosphonium salt scintillator material of the present invention has very bright visible light emission under ultraviolet light excitation due to its thermally activated delayed fluorescence mechanism, has strong absorption capacity for X-rays and high exciton utilization, has a very simple synthesis path, has a high yield, and can be synthesized in large quantities. The scintillator material prepared based on this type of TADF quaternary phosphonium salt exhibits excellent optical properties and shows great commercial application potential in organic light-emitting devices, such as being used to prepare X-ray detection imaging screens, light-emitting diodes, optical thermometers, light-emitting anti-counterfeiting chips, up-conversion light-emitting materials, and solid-state lighting lamps. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the reaction flow of the present invention;
[0023] Figure 2 This is a single crystal structure diagram of the product of Example 1 of the present invention;
[0024] Figure 3 This is the emission spectrum of the product of Example 1 of the present invention;
[0025] Figure 4 The graphs are the temperature-variable steady-state luminescence spectrum (a) and the temperature-variable transient luminescence spectrum (b) of the product of Example 1 of the present invention;
[0026] Figure 5 This is a single crystal structure diagram of the product of Example 2 of the present invention;
[0027] Figure 6 This is the emission spectrum of the product of Example 2 of the present invention;
[0028] Figure 7 The following is a schematic diagram of the reaction process of the product of Example 3 of the present invention and a photo of the product under ultraviolet light;
[0029] Figure 8 This is a photograph of a test example of the present invention under X-ray excitation;
[0030] Fig. 9 The figure is a graph of the X-ray attenuation efficiency (a) and a graph of the light energy yield test effect (b) of a test example of the present invention;
[0031] Fig.10 The following are photos of the product of the application example of the present invention under ultraviolet light (a) and a simulated safety inspection photo (b). DETAILED DESCRIPTION
[0032] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0033] Unless otherwise specified, the experimental methods used in the examples are all conventional methods; the materials, reagents, etc. used, unless otherwise specified, can be obtained from commercial channels.
[0034] Example 1: A TADF quaternary phosphonium salt scintillator material
[0035] Add 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl and iodine butane to toluene solvent. The amount of toluene used is sufficient to completely dissolve 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl. The amount of iodine butane used is greater than or equal to the molar amount of 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl. Reflux the above reaction system at room temperature to 150°C. As the reaction proceeds, a white precipitate is gradually generated. The obtained white precipitate is filtered, the mother liquor is removed, and the product is washed with toluene several times to obtain a butyl-substituted product (abbreviated as C4-NMe2PTPP-I). The reaction flow diagram is shown below: Figure 1 shown.
[0036] The composition of the product was determined by nuclear magnetic resonance spectroscopy, elemental analysis and high-resolution mass spectrometry, and the corresponding single crystal structure was analyzed by X-ray single crystal diffraction technology.
[0037] like Figure 2 As shown in the figure, it can be seen that the butyl group is connected to the phosphorus atom to form a new PC bond, indicating that the tertiary phosphine is successfully alkylated and the iodide ions are distributed between the quaternary phosphonium cations. From the structure of its smallest asymmetric unit, dimethylamine, iodide ions and one of the benzene rings connected to the quaternary phosphonium core form a sandwich-like interlayer structure, which is conducive to the charge transfer of dimethylamine and iodide ions to the quaternary phosphonium core.
[0038] like Figure 3As shown, the luminescence efficiency was evaluated using the photoluminescence quantum efficiency test system (C9920) produced by Hamamatsu Corporation. The synthesized C4-NMe2PTPP-I exhibited bright blue light emission under ultraviolet light excitation, with an emission peak at 473nm, and its photoluminescence quantum efficiency was close to 100%.
[0039] The FLS1000 fluorescence spectrometer produced by Edinburgh Company was used to test the temperature-dependent steady-state luminescence spectrum and temperature-dependent transient luminescence spectrum of C4-NMe2PTPP-I. Liquid nitrogen was used to cool the sample. A xenon lamp was used as the excitation light source for the steady-state luminescence spectrum, and a microsecond pulse flash lamp was used as the excitation light source for the transient luminescence spectrum. Figure 4 As shown in the figure, as the temperature of the sample decreases from room temperature to 78K, the emission peak of the sample gradually red-shifts from 473nm to 499nm, which are attributed to the emission of fluorescence and phosphorescence, respectively. The triplet state and triplet state energy level difference △E calculated from this ST It is 0.14eV, and it is generally believed that the △E of the material ST When the value is less than 0.2eV, the TADF phenomenon can occur. At the same time, the lifetime of the temperature-dependent transient spectrum at low temperatures is significantly extended, which is consistent with the characteristics of the TADF luminescence mechanism.
[0040] Example 2: A TADF quaternary phosphonium salt scintillator material
[0041] 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl and iodopropane are added to a toluene solvent, and the amount of toluene used is sufficient to completely dissolve 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl. The amount of iodopropane used is greater than or equal to the molar amount of 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl. The above reaction system is refluxed at room temperature to 150°C. As the reaction proceeds, a white precipitate is gradually generated. The obtained white precipitate is filtered, the mother liquor is removed, and the product is washed with toluene several times to obtain a propyl substituted product (abbreviated as C3-NMe2PTPP-I).
[0042] like Figure 5 As shown, its structure can be determined by single crystal diffraction. The propyl group is connected to the phosphorus atom to form a new PC bond, and the iodine ions are distributed between the quaternary phosphonium cations.
[0043] like Figure 6 As shown, C3-NMe2PTPP-I exhibits bright blue light emission under 365nm ultraviolet light, with an emission peak at 470nm and a photoluminescence efficiency of 94.4%.
[0044] Example 3: Two TADF quaternary phosphonium salt scintillator materials
[0045] (1) Add 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl and benzyl chloride to toluene solvent. The amount of toluene used should be sufficient to completely dissolve 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl. The amount of benzyl chloride used should be greater than or equal to the molar amount of 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl. Reflux the above reaction system at room temperature to 150° C. As the reaction proceeds, a white precipitate is gradually generated. The obtained white precipitate is filtered, the mother liquor is removed, and the product is washed with toluene for multiple times to obtain the final product (abbreviated as Bz-NMe2PTPP-Cl).
[0046] (2) Add 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl and benzyl bromide to toluene solvent. The amount of toluene used should be sufficient to completely dissolve 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl. The amount of benzyl bromide used should be greater than or equal to the molar amount of 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl. Reflux the above reaction system at room temperature to 150° C. As the reaction proceeds, a white precipitate is gradually generated. The obtained white precipitate is filtered, the mother liquor is removed, and the product is washed with toluene for multiple times to obtain the final product (abbreviated as Bz-NMe2PTPP-Br).
[0047] like Figure 7 As shown, Bz-NMe2PTPP-Cl and Bz-NMe2PTPP-Br exhibit blue-green and blue light emissions, respectively, under ultraviolet light irradiation.
[0048] Test example: Scintillator material performance test
[0049] The organic scintillator anthracene (purchased from Shanghai Aladdin Reagent Company) and the inorganic scintillator bismuth germanate (BGO) (purchased from Shanghai Shuojie Crystal Co., Ltd.) were used as controls.
[0050] like Figure 8 As shown, when the product C4-NMe2PTPP-I of Example 1 and the scintillator anthracene are placed under X-rays, it can be seen that compared with the commercial scintillator anthracene, C4-NMe2PTPP-I exhibits brighter luminescence, showing its application potential as an X-ray scintillator.
[0051] The X-ray scintillation performance and light energy yield of C4-NMe2PTPP-I were tested. Fig. 9 As shown in a, 1 mm thick C4-NMe2PTPP-I can absorb 53.48% of X-rays, while anthracene can only absorb 4.33%. Therefore, it can be seen that the X-ray absorption capacity of C4-NMe2PTPP-I is significantly better than that of the commercial organic scintillator anthracene.
[0052] Using bismuth germanate as a reference, a miniature radiation source (Mini-X2, Ag target) was used to irradiate the reference and the sample to be tested, and an integrating sphere was used to collect and calculate the number of photons (P total ), then use P total Divide by their respective attenuation efficiencies to obtain the normalized photon number (P norm ).like Fig. 9 As shown in b, the attenuation efficiency of 1 mm thick C4-NMe2PTPP-I is 53.48%. norm Divide by the reference P norm , multiplied by the reference standard light energy yield, we can calculate that the light energy yield of C4-NMe2PTPP-I is 80817photons / MeV (BGO light energy yield is 8200photons / MeV), and the calibrated light energy yield of anthracene is 11708photons / MeV, which is close to its standard value of 12000photons / MeV. Therefore, it can be seen that the light energy yield of C4-NMe2PTPP-I is significantly better than that of commercial scintillators bismuth germanate (BGO) and anthracene.
[0053] Application examples:
[0054] The thin film prepared based on the TADF quaternary phosphonium salt scintillator material of the present invention can be applied to X-ray scintillation imaging, such as Fig.10 As shown, C4-NMe2PTPP-I powder and polycaprolactone are mixed, the mass ratio of C4-NMe2PTPP-I powder to polycaprolactone is 1:1, and a uniform melt is obtained after heating to 210°C, and then coated on a quartz substrate, and a uniform film is obtained after cooling ( Fig.10 a). Fig.10 As shown in b, the prepared film can be used as an X-ray scintillation imaging screen to image school bags, peanuts, shrimps, etc., showing its application potential in safety inspection, non-destructive testing, agricultural seed selection and other fields.
[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A TADF quaternary phosphonium salt scintillator material, characterized in that: The structural formula of the material is: Wherein, the R is an alkyl group or an aromatic substituent; and the X is a halogen.
2. The TADF quaternary phosphonium salt scintillator material according to claim 1, characterized in that: The alkyl group is any one of chain methyl, ethyl, propyl, butyl, pentyl, hexyl and derivatives thereof, cyclic cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl and derivatives thereof; the aromatic substituent is any one of benzyl, phenethyl, phenylpropyl, phenbutyl, phenylpentyl, 9-(2-ethyl)carbazole and derivatives thereof; the halogen is any one of chlorine, bromine and iodine.
3. A method for preparing the TADF quaternary phosphonium salt scintillator material according to claim 1, characterized in that: The following steps are involved: The method is to dissolve 2-diphenylphospho-2'-(N,N-dimethylamino)biphenyl and halogenated alkane or halogenated aromatic hydrocarbon in a solvent, react, and collect the precipitated product to obtain the product.
4. The preparation method according to claim 3, characterized in that: The halogenated alkane is any one of chain halogenated methane, halogenated ethane, halogenated propane, halogenated butane, halogenated pentane, halogenated hexane and derivatives thereof, cyclic halogenated cyclopropane, halogenated cyclobutane, halogenated cyclopentane, halogenated cyclohexane and derivatives thereof; the halogenated aromatic hydrocarbon is any one of halogenated benzyl, halogenated ethylbenzene, halogenated phenylpropane, halogenated phenylbutane, halogenated phenylpentane, 9-(2-haloethyl)carbazole and derivatives thereof.
5. The preparation method according to claim 4, characterized in that: The halogen is any one of chlorine, bromine and iodine.
6. The preparation method according to claim 3, characterized in that: The solvent is at least one of toluene, ethyl acetate, methanol, tetrahydrofuran, n-hexane and N,N-dimethylformamide.
7. The preparation method according to claim 3, characterized in that: The reaction temperature is controlled to be between room temperature and 150°C.
8. A film, characterized in that: It comprises the TADF quaternary phosphonium salt scintillator material and a polymer as described in claim 1 or 2; the mass ratio of the TADF quaternary phosphonium salt scintillator material and the polymer is (0.1-2):
1.
9. A method for preparing the thin film according to claim 8, characterized in that: The following steps are involved: The TADF quaternary phosphonium salt scintillator material is mixed with a polymer, heated to melt, scraped onto a substrate, and cooled.
10. Use of the TADF quaternary phosphonium salt scintillator material according to claim 1 or 2 and the thin film according to claim 8 in an organic light-emitting device.
Citation Information
Patent Citations
Preparation method and application of lead-free A4MnBi2X12 perovskite material
CN110776914A
Organic room-temperature phosphorescent polymer, preparation thereof and application of organic room-temperature phosphorescent polymer in X-ray imaging
CN114539472A
Diphosphine donor-acceptor luminescent material, metal halide single crystal material as well as preparation method and application of metal halide single crystal material
CN116199715A
Preparation and application of heterocycle-containing polycyclic aromatic hydrocarbon and halogenated organic scintillator of heterocycle-containing polycyclic aromatic hydrocarbon