Transition metal nickel complex, preparation method and application thereof, and catalyst composition
By designing a transition metal nickel complex with a large sterically hindered heterocyclic aryl acridine substituent and a cocatalyst combination, the problems of decomposition and insufficient activity of existing catalysts at high temperatures have been solved, and the preparation and thermal stability of hyperbranched ethylene have been achieved. properties, meeting the needs of industrial production and expanding the application scope of polymers.
Patent Information
- Application Number
- CN202310321633.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
Existing ethylene catalysts decompose at high temperatures and are difficult to prepare highly branched polyethylene. Their catalytic activity and thermal stability are insufficient, and they cannot meet the demand for highly branched polyethylene in industrial production.
A transition metal nickel complex was designed, using a large sterically hindered heterocyclic acridine substituent, prepared through a condensation reaction with an aniline compound and 2-acetylpyridine, and combined with aluminoxane and other cocatalysts to form a highly active catalyst combination material for ethylene polymerization.
High reactivity and molecular weight control are achieved. The polyethylene obtained by catalysis has a high degree of branching and thermal stability. It is suitable for the production of films, fibers and functional materials, and expands the application range of polymers.
Smart Images

Figure CN118724982A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyolefin catalysts, and in particular to a transition metal nickel complex and a preparation method and application thereof, and a catalyst composition. Background Art
[0002] Since the discovery that N,N-bidentate nickel complexes can produce highly branched polyethylene through a unique "chain walking" mechanism, various research groups have conducted extensive research. This is very different from the mechanism of ethylene polymerization catalyzed by N,N,N-tridentate iron and cobalt complexes, and the polyethylene obtained by catalysis usually has the characteristics of high branching. The development of catalysts is inseparable from the design and synthesis of new ligands. By modifying the types of substituents on the ligands, a series of new nickel complex catalytic systems can be developed. For many years, 2-iminopyridine nickel (II) complexes have been widely used as representative N,N-bidentate complex catalysts in the field of catalytic ethylene preparation of highly branched polyethylene materials, and their catalytic potential has been deeply explored. In order to overcome the shortcomings of 2-iminopyridine nickel (II) complexes that are easy to decompose and produce low molecular weight polymers at elevated reaction temperatures, some studies have attempted to develop aniline substituted with large steric substituents and introduce them into the ligand structure of 2-iminopyridine, and the catalytic activity and thermal stability of the resulting nickel complexes have been significantly improved. The corresponding nickel complex catalysts containing 1-aminonaphthalene (A, Formula 1) or aniline derivatives (B and C, Formula 1) substituted with bulky benzhydryl groups have high catalytic activity in ethylene polymerization, some of which are as high as 10 7 g of PE(mol Ni) -1 h -1 .
[0003]
[0004] The inventor has been committed to the design and development of olefin polymerization catalysts and the exploration of catalytic processes, and has done a lot of work around transition metal catalysts and N^N ligands. The results show that by changing the ligand structure, the electronic effect and steric effect of the structure can be effectively regulated; thereby achieving effective regulation of the resulting polyethylene structure. In the face of the society's growing demand for highly branched polyethylene, in addition to improving the preparation conditions and efficiency, how to obtain a highly active ethylene polymerization catalyst with good thermal stability to adapt to industrial production and meet the society's demand for highly branched polyethylene products has become the core content of scholars' research and the key to whether industrialization can be promoted as soon as possible. Summary of the invention
[0005] Based on the above technical problems, the purpose of the present invention is to provide a transition metal nickel complex and its preparation method and application, and a catalyst composition. The complex has a large sterically hindered heterocyclic aromatic acridine substituent and can produce a highly branched polyolefin product containing unsaturated bonds.
[0006] To achieve the above object, the present invention provides a transition metal nickel complex having a structure as shown in formula (I):
[0007]
[0008]
[0009] wherein each X is the same or different and is independently selected from F, Cl, Br, I;
[0010] R 1 , R 2 , R 3 , R 4 , R 5 The same or different, each independently selected from one or more R a Substituted with the following groups: H, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-20 Aryl or C 6-20 Heteroatom aromatic group;
[0011] R a Selected from H, F, Cl, Br, I, C 1-6 Alkyl, C 1-6 Alkoxy, C 3-10 Heterocyclic group, C 6-20 Aryl or C 6-20 heteroatom aromatic, and each R a Same or different.
[0012] In the present invention, the term "C 1-6 The term "alkyl" refers to a straight or branched chain alkyl group having 1 to 6 carbon atoms, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, sec-butyl, pentyl, and neopentyl.
[0013] The term "C 1-6 "Alkoxy" is to be understood as meaning preferably a linear or branched, saturated, monovalent hydrocarbon radical of the formula -O-alkyl having 1 to 6 carbon atoms, for example methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, pentyloxy, isopentyloxy, hexyloxy or the isomers thereof.
[0014] The term "C 1-3 "Alkoxy" is understood to mean preferably a linear or branched, saturated, monovalent hydrocarbon radical of the formula -O-alkyl having 1 to 3 carbon atoms, for example methoxy, ethoxy or propoxy.
[0015] The term "C 3-10"Heterocyclyl" is understood to mean preferably a group of the formula -N / O / S-cycloalkyl having 3 to 10 carbon atoms. The heterocyclyl may be linked to the remainder of the molecule via any of the carbon atoms or the nitrogen atom, if present. In particular, the heterocyclyl may include, but is not limited to: a 4-membered ring, such as azetidinyl, oxetanyl; a 5-membered ring, such as tetrahydrofuranyl, dioxolyl, pyrrolidinyl, imidazolidinyl, pyrazolidinyl, pyrrolinyl; or a 6-membered ring, such as tetrahydropyranyl, piperidinyl, morpholinyl, dithianyl, thiomorpholinyl, piperazinyl or trithianyl; or a 7-membered ring, such as diazepanyl. Optionally, the heterocyclyl It may be benzo-fused. The heterocyclic group may be bicyclic, for example, but not limited to, a 5,5-membered ring, such as a hexahydrocyclopenta[c]pyrrole-2(1H)-yl ring, or a 5,6-membered bicyclic ring, such as a hexahydropyrrolo[1,2-a]pyrazine-2(1H)-yl ring. The ring containing nitrogen atoms may be partially unsaturated, i.e., it may contain one or more double bonds, for example, but not limited to, 2,5-dihydro-1H-pyrrolyl, 4H-[1,3,4]thiadiazinyl, 4,5-dihydrooxazolyl or 4H-[1,4]thiazinyl, or it may be benzo-fused, for example, but not limited to, dihydroisoquinolinyl. According to the present invention, the heterocyclic group is non-aromatic.
[0016] The term "C 6-20 "Aryl" is understood to mean preferably a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic hydrocarbon ring having 6 to 20 carbon atoms, preferably "C 6-14 The term "C 6-14 "Aryl" is understood to mean preferably a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic hydrocarbon ring ("C 6-14 Aryl), especially a ring having 6 carbon atoms ("C 6 aryl), such as phenyl; or biphenyl, or a ring having 9 carbon atoms ("C 9 aryl), such as indanyl or indenyl, or a ring having 10 carbon atoms ("C 10 aryl), such as tetrahydronaphthyl, dihydronaphthyl or naphthyl, or a ring having 13 carbon atoms ("C 13 aryl), such as fluorenyl, or a ring having 14 carbon atoms ("C 14 "aryl"), for example anthracenyl.
[0017] The term "C 6-20The term "heteroatom aryl" is understood to mean preferably a group of the formula -N-aryl or -N-heteroaryl having 6 to 20 carbon atoms. Examples of monocyclic heteroaryl groups include, but are not limited to, thienyl, furanyl, pyrrolyl, oxazolyl, thiazolyl, imidazolyl, pyrazolyl, isoxazolyl, isothiazolyl, oxadiazolyl, triazolyl, thiadiazolyl, thia-4H-pyrazolyl, and the like, as well as their benzo derivatives, such as benzofuranyl, benzothienyl, benzoxazolyl, benzisoxazolyl, and the like. Oxazolyl, benzimidazolyl, benzotriazolyl, indazolyl, indolyl, isoindolyl, etc.; or pyridyl, pyridazinyl, pyrimidinyl, pyrazinyl, triazinyl, etc., and benzo derivatives thereof, such as quinolyl, quinazolinyl, isoquinolyl, etc.; or azinyl, indolizinyl, purinyl, etc., and benzo derivatives thereof; or cinnolinyl, phthalazinyl, quinazolinyl, quinoxalinyl, naphthyridinyl, pteridinyl, carbazolyl, acridinyl, phenazinyl, phenothiazinyl, phenoxazinyl, etc.
[0018] The transition metal nickel complex of the present invention, in formula (I), R 1 Selected from C 1-3 Alkyl and Cl; more preferably methyl.
[0019] The transition metal nickel complex of the present invention, in formula (I), R 2 Selected from C 1-3 Alkyl and Cl; more preferably methyl.
[0020] The transition metal nickel complex of the present invention, in formula (I), R 3 , R 4 The same or different, each independently selected from H and C 1-6 Alkyl; more preferably all are H.
[0021] The transition metal nickel complex of the present invention, in formula (I),
[0022] R 1 =R 2 =Me, X is Cl, R 3 , R 4 , R 5 All are H; or
[0023] R 1 =R 2 =Et, X is Cl, R 3 , R 4 , R 5 All are H; or
[0024] R 1 =R 2 =iPr, X is Cl, R 3 , R 4 , R 5 All are H; or
[0025] R 1 =Me, R 2 =Et, X is Cl, R 3 , R 4 , R 5 All are H; or
[0026] R 1 =R 2 =Cl, X is Cl, R 3 , R 4 , R 5 Both are H.
[0027] To achieve the above object, the present invention also provides a method for preparing the transition metal nickel complex, comprising the following steps:
[0028] The aniline compound shown in formula (II) is reacted with 2-acetylpyridine and a compound NiX 2 Carrying out a condensation reaction to obtain a metal complex represented by formula (I);
[0029]
[0030] wherein each X is the same or different and is independently selected from F, Cl, Br, I;
[0031] R 1 , R 2 , R 3 , R 4 , R 5 The same or different, each independently selected from one or more R a Substituted with the following groups: H, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-20 Aryl or C 6-20 Heteroatom aromatic group;
[0032] R a Selected from H, F, Cl, Br, I, C 1-6 Alkyl, C 1-6 Alkoxy, C 3-10 Heterocyclic group, C 6-20 Aryl or C 6-20 heteroatom aromatic, and each R a Same or different.
[0033] The preparation method of the present invention, the compound NiX 2 The addition form is not limited, and can be a nickel halide, or a hydrate or solvate of a halide, for example, NiCl 2 or NiBr 2 (DME).
[0034] In the preparation method of the present invention, the condensation reaction is carried out under oxygen-free conditions, for example, under the protection of an inert gas such as nitrogen.
[0035] In the preparation method of the present invention, the condensation reaction is carried out under the catalysis of an organic acid; the organic acid is one or more of formic acid, acetic acid and p-toluenesulfonic acid, preferably acetic acid.
[0036] In the preparation method of the present invention, the condensation reaction is carried out under heating reflux for 6 to 12 hours, preferably 8 to 10 hours.
[0037] The preparation method of the present invention, the compound NiX 2 The molar ratio of the aniline compound represented by the formula (II) is 1:2 to 3, preferably 1:2 to 2.5, and more preferably 1:2.5.
[0038] The preparation method of the present invention further comprises the step of purifying the obtained metal complex represented by formula (I), wherein the purification method comprises the following steps:
[0039] A) removing volatile substances from the metal complex represented by formula (I) to obtain a concentrated solution, and adding the concentrated solution into an organic solvent for precipitation;
[0040] b) subjecting the material precipitated in step a) to solid-liquid separation, washing the solid phase with an organic solvent and drying it.
[0041] Wherein, the organic solvent is an anhydrous organic solvent.
[0042] To achieve the above objectives, the present invention also provides a catalyst composition, including a main catalyst and, optionally, a co-catalyst, wherein the main catalyst is the transition metal nickel complex, and the co-catalyst is one or more of aluminoxane, alkylaluminum and alkylaluminum chloride.
[0043] The catalyst composition of the present invention, wherein the aluminoxane is methylaluminoxane (MAO) and / or methylaluminoxane modified with triisobutylaluminum (MMAO); the alkyl group in the alkylaluminum chloride is selected from C 1-3 Alkyl, preferably diethylaluminum chloride (Et 2 AlCl) and / or dimethylaluminum chloride (Me 2 AlCl).
[0044] The catalyst composition of the present invention has a molar ratio of the metal Al in the co-catalyst to the central metal Ni in the transition metal nickel complex of (200-4000):1, preferably a molar ratio of (200-3500):1, for example, 500:1, 800:1, 1000:1, 1500:1, 1750:1, 2000:1, 2250:1, 2500:1, 2750:1, or 3250:1.
[0045] In the catalyst composition of the present invention, when the co-catalyst is methylaluminoxane, the molar ratio of the metal Al in the methylaluminoxane to the central metal Ni in the transition metal nickel complex is (2000-3000):1, and the more preferred molar ratio is 2500:1, for example, it can be 2200:1, 2300:1, 2400:1, 2550:1, 2700:1, 2950:1.
[0046] When the co-catalyst is methylaluminoxane modified with triisobutylaluminum, the molar ratio of the metal Al in the methylaluminoxane modified with triisobutylaluminum to the central metal Ni in the transition metal nickel complex is (1000-2500):1, and the more preferred molar ratio is 1750:1, for example, it can be 1200:1, 1500:1, 1750:1, 2000:1, 2250:1.
[0047] When the co-catalyst is alkylaluminum chloride, the molar ratio of metal Al in the alkylaluminum chloride to the central metal Ni in the transition metal nickel complex is (200-1500):1, and the more preferred molar ratio is 500:1, for example, 200:1, 500:1, 800:1, 1000:1, 1500:1.
[0048] To achieve the above object, the present invention also provides a use of the transition metal nickel complex or the catalyst composition in catalyzing olefin polymerization.
[0049] The transition metal nickel complex or catalyst composition provided by the present invention is particularly suitable for the polymerization reaction of ethylene.
[0050] When the transition metal nickel complex or catalyst composition provided by the present invention is used to catalyze the polymerization reaction, the polymerization reaction conditions are conventional reaction conditions in the art, such as the polymerization reaction temperature can be 20-80°C, specifically 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C; preferably 20-60°C; the polymerization reaction time can be 5-60min, specifically 30min; the polymerization reaction pressure can be 0.5-10atm, specifically 10atm; the polymerization reaction solvent can be selected from one or more of toluene, o-xylene, dichloromethane, ethanol, tetrahydrofuran, hexane or cyclohexane.
[0051] Beneficial effects of the present invention:
[0052] 1. The imine pyridine nickel complex containing a large sterically hindered heterocyclic aromatic group provided by the present invention can be used as a catalyst for olefin polymerization, especially for ethylene polymerization, has high reaction activity, and has extremely strong control performance on polyethylene molecular weight.
[0053] 2. The preparation method of the imine pyridine intermediate and transition metal nickel complex of N-aryl-introduced bulky heterocyclic aromatic acridine provided by the present invention has the advantages of easy large-scale synthesis and simple operating conditions.
[0054] 3. The method for preparing polyolefins provided by the present invention is simple to operate, the reaction conditions are easy to control, and the obtained product has adjustable molecular weight and melting point. For the nickel complex, the polyethylene product obtained by catalyzing ethylene polymerization has a molecular weight of 13 to 24.1 kg·mol -1 In addition, high temperature NMR 1 H / 13 The obtained polyethylene material was characterized and calculated by C means, and the results showed that it had a relatively high degree of branching, and the remote large sterically hindered heterocyclic aromatic acridine substituent had a great influence on the degree of branching and branching content of the polymer chain. There were 82 branched chains per 1000 carbons in the obtained polymer product, including methyl (53.1%), butyl (6.7%) and long chain branches (40.2%). In particular, in addition to the highly branched characteristics, signal peaks of unsaturated end groups were still found in the high-temperature nuclear magnetic resonance spectrum of the polymer, further expanding its functional application range. It can be used as films, fibers and various types of pipes, etc., showing potential applications in the production of long-chain copolymers, functional polymers and coating materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 Temperature-elevated H-NMR spectrum of the polymer obtained in Example 6b).
[0056] Figure 2 Temperature-elevated NMR carbon spectrum of the polymer obtained in Example 6b). DETAILED DESCRIPTION
[0057] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.
[0058] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0059] Unless otherwise specified, the concentrations in the following examples are molar concentrations.
[0060] Methylaluminoxane (MAO) and diethyl chloride (Et 2 AlCl) was purchased from AkzoNobel, USA. Al / Ni in the following examples refers to the molar ratio of the metal Al in the cocatalyst MAO or MMAO to the Ni in the added metal complex catalyst.
[0061] The molecular weight (M) of the polymer obtained in the ethylene polymerization examples 6-15 w ) were determined by conventional high temperature GPC method, and the melting point (T m ) were determined according to the conventional DSC method, and the polymerization activity of the polymers were calculated according to the following formula: polymerization activity = polymer yield / (catalyst dosage*polymerization time).
[0062] All synthesized compounds described below were confirmed by infrared and elemental analysis.
[0063] Examples 1-5 The complexes were prepared by the following reaction scheme:
[0064]
[0065] Example 1
[0066] Preparation of 2,6-dimethyl-4-acridineaniline (A1)
[0067] 2,6-Dimethylaniline (1.45 g, 12 mmol) and 9-hydroxyacridine (3 g, 15 mmol) were placed in a 250 mL round-bottom flask. The mixture was stirred at 130 °C under nitrogen for 30 minutes, and then a catalytic amount of ZnCl in HCl solution was added dropwise. 2 The reaction mixture was further heated for 2 hours and after cooling, the solid was dissolved in DCM (200 mL). It was filtered and washed twice with saturated solutions of ammonium chloride and sodium chloride. The organic portion was collected and washed with anhydrous Na 2 SO 4 Dry and concentrate under reduced pressure. The product was recrystallized from DCM using n-heptane to give a white crystalline solid (1.25 g, 34%).
[0068] The structural confirmation data are as follows:
[0069] 1 H NMR (400 MHz, CDCl 3 ,TMS): 1 H NMR (400 MHz, CDCl 3,TMS): δ7.18(t,J=3.8Hz,2H,Ar-H),7.16(m,4H,Ar-H),7.09(t,J=7.0Hz,2H,Ar-H),6.76(s,2H,Ar-H m ),5.08(s,1H,–CH–)2.8(s,2H,NH 2 ),2.10(s,6H,–CH 3 ).
[0070] 13 C NMR (100 MHz, CDCl 3 ,TMS):d 151.1,141.3,136.3,129.8,128.2,127.5,125.2,123.1,121.9,116.3,77.3,77.0,76.7,43.6,17.7
[0071] Preparation of 2-[1-(4-acridine-2,6-dimethylphenylimino)ethyl]-pyridinylnickel dibromide (Ni-1)
[0072] Nickel complex Ni-1(R 1 =R 2 =Me, X is Br, R 3 , R 4 , R 5 All H) were synthesized in one pot. The Schlenk tube was loaded with 2-acetylpyridine (0.024 g, 0.20 mmol), 2,6-dimethyl-4-acridinylaniline (0.20 g, 0.60 mmol) and NiBr 2 (DME) (0.06 g, 0.20 mmol) was refluxed with acetic acid (30 mL). The reaction was continued at 120 °C for 6 hours and the volatiles were evaporated using a pump to obtain a concentrated solution. The nickel complex was precipitated using ether (20 mL), filtered, washed with ether (3×15 mL), and isolated in good yield (0.11 g, 89%) as an air-stable brick-red powder.
[0073] The structural confirmation data are as follows:
[0074] FT-IR(cm -1 ):3001(w)1615(ν(C=N),m),1595(w),1577(w),1536(w),1479
[0075] (s),1450(s),1372(w),1301(w),1250(s),1214(w),1148(w),1118(m) ,1118(w),1096(w),1032(w),946(w),879(m),811(w),751(s),658(w).
[0076] Elemental analysis: C 28 H 23 Br 2 Ni 3 (616.96) Theoretical value: 54.24; H, 3.74; N, 6.78%. Experimental value: C, 54.47; H, 4.05; N, 6.99%.
[0077] Example 2
[0078] Preparation of 2,6-diethyl-4-acridineaniline (A2)
[0079] 2,6-Diethylaniline (1.79 g, 12 mmol) and 9-hydroxyacridine (3 g, 15 mmol) were placed in a 250 mL round bottom flask. The mixture was stirred at 130 °C under nitrogen for 30 minutes, and then a catalytic amount of ZnCl in HCl solution was added dropwise. 2 The reaction mixture was further heated for 2 hours and after cooling, the solid was dissolved in DCM (200 mL). It was filtered and washed twice with saturated solutions of ammonium chloride and sodium chloride. The organic portion was collected and washed with anhydrous Na 2 SO 4 Dry and concentrate under reduced pressure. The product was recrystallized from DCM using n-heptane to give a white crystalline solid (1.26 g, 38%).
[0080] The structural confirmation data are as follows:
[0081] 1 H NMR (400 MHz, CDCl 3 ,TMS): δ7.15(t,J=3.8Hz,2H,Ar-H),7.12–7.06(m,4H,Ar-H),6.96(t,J=3.8Hz,2H,Ar-H),6.76(s,2H,Ar-H m ),5.12(s,1H,–CH–),3.51(s,2H,NH 2 ),2.49–2.43(m,4H,–CH 2 –),1.18(t,J=7.6Hz,6H,–CH 3 ).
[0082] 13 C NMR (100 MHz, CDCl3 ,TMS):d 151.1,140.1,136.3,129.7,128.0,127.4,126.2,125.3,123.1,116.3,77.3,77.0,76.7,43.9,24.4,13.0.
[0083] Preparation of 2-[1-(4-acridine-2,6-diethylphenylimino)ethyl]-pyridinylnickel dibromide (Ni-2)
[0084] Nickel complex Ni-2(R 1 =R 2 =Et, X is Br, R 3 , R 4 , R 5 All H) were synthesized in one pot. The Schlenk tube was loaded with 2-acetylpyridine (0.024 g, 0.20 mmol), 2,6-diethyl 4-acridinylaniline (0.20 g, 0.60 mmol) and NiBr 2 (DME) (0.06 g, 0.20 mmol) was refluxed with acetic acid (30 mL). The reaction was continued at 120 °C for 6 hours and the volatiles were evaporated using a pump to obtain a concentrated solution. The nickel complex was precipitated using ether (20 mL), filtered, washed with ether (3×15 mL), and isolated in good yield (0.10 g, 77%) as an air-stable brick-red powder.
[0085] The structural confirmation data are as follows:
[0086] FT-IR(cm -1 ):2972(w),2870(w),1621(ν(C=N),w),1576(m),1543(w),1478
[0087] (s),1450(s),1301(w),1251(w),1211(m),1150(w),1118(w),1095(w),1030(w),981(w),940(w),881(m),808(w),749(s).
[0088] Elemental analysis: C 30 H 27 Br 2 Ni 3 (648.07) Theoretical value: C, 55.60; H, 4.20; N, 6.48%. Experimental value: C, 55.32; H, 4.62; N, 6.56%.
[0089] Example 3
[0090] Preparation of 2,6-diisopropyl-4-acridineaniline (A3)
[0091] 2,6-Diisopropylaniline (2.12 g, 12 mmol) and 9-hydroxyacridine (3 g, 15 mmol) were placed in a 250 mL round-bottom flask. The mixture was stirred at 130 °C under nitrogen for 30 minutes, and then a catalytic amount of ZnCl in HCl solution was added dropwise. 2 The reaction mixture was further heated for 2 hours and after cooling, the solid was dissolved in DCM (200 mL). It was filtered and washed twice with saturated solutions of ammonium chloride and sodium chloride. The organic portion was collected and washed with anhydrous Na 2 SO 4 The mixture was dried and concentrated under reduced pressure. The product was recrystallized from DCM using n-heptane to give a white crystalline solid (1.30 g, 36%).
[0092] The structural confirmation data are as follows:
[0093] 1 H NMR (400 MHz, CDCl 3 ,TMS): δ7.15(t,J=6.8Hz,2H,Ar-H),7.10–7.05(m,4H,Ar-H),6.95(t,J=7.4Hz,2H,Ar-H),6.81(s,2H,Ar-H),5.13(s,1H,–CH–),3.51(s,2H,NH) 2 ),2.89–2.80(m,2H,–CH–),1.27(t,J=4.4Hz,12H,–CH 3 ).
[0094] 13 C NMR (100 MHz, CDCl 3 ,TMS):d 151.3,138.8,136.0,132.6,129.6,127.4,125.5,123.0,77.3,77.0,76.7,44.3,28.0,22.4.
[0095] Preparation of 2-[1-(4-acridine-2,6-diisopropylphenylimino)ethyl]-pyridinylnickel dibromide (Ni-3)
[0096] Nickel complex Ni-3(R 1 =R 2 =iPr, X is Br, R 3 , R 4 , R 5All H) were synthesized in one pot. The Schlenk tube was loaded with 2-acetylpyridine (0.024 g, 0.20 mmol), 2,6-diisopropyl 4-acridinylaniline (0.21 g, 0.60 mmol) and NiBr 2 (DME) (0.06 g, 0.20 mmol) was refluxed with acetic acid (30 mL). The reaction was continued at 120 °C for 6 hours and the volatiles were evaporated using a pump to obtain a concentrated solution. The nickel complex was precipitated using ether (20 mL), filtered, washed with ether (3×15 mL), and isolated in good yield (0.12 g, 89%) as an air-stable brick-red powder.
[0097] The structural confirmation data are as follows:
[0098] FT-IR(cm -1 ):2961(m),2868(w),1609(ν(C=N),w),1570(w),1550(w),1473
[0099] (m),1449(s),1303(w),1251(s),1079(w),1028(w),944(w),833(w),812(w),751(s),657(w).
[0100] Elemental analysis: C 32 H 31 Br 2 Ni 3 (676.12) Theoretical value: C, 56.85; H, 4.62; N, 6.21%. Experimental value: C, 56.40; H, 4.70; N, 6.19%.
[0101] Example 4
[0102] Preparation of 2-methyl-6-ethyl-4-acridineaniline (A4)
[0103] 2-Methyl-6-ethylaniline (1.62 g, 12 mmol) and 9-hydroxyacridine (3 g, 15 mmol) were placed in a 250 mL round-bottom flask. The mixture was stirred at 130 °C under nitrogen for 30 minutes, and then a catalytic amount of ZnCl in HCl solution was added dropwise. 2 The reaction mixture was further heated for 2 hours and after cooling, the solid was dissolved in DCM (200 mL). It was filtered and washed twice with saturated solutions of ammonium chloride and sodium chloride. The organic portion was collected and washed with anhydrous Na 2 SO 4 Dry and concentrate under reduced pressure. The product was recrystallized from DCM using n-heptane to give a white crystalline solid (1.01 g, 32%).
[0104] The structural confirmation data are as follows:
[0105] 1 H NMR (400 MHz, CDCl 3 ,TMS):d 7.11(t,J=4.2Hz,2H,Ar-H),7.09–6.96(m,4H,Ar-H),6.95(t,J=4Hz,2H,Ar-H),6.81(s,1H,Ar-H m ),6.72(s,1H,Ar-H m ),5.11(s,1H,–CH–),3.51(s,2H,NH 2 ),2.51–2.45(m,2H,–CH 2 –),2.09(s,3H,–CH 3 ),1.39(t,J=4Hz,3H,–CH3).
[0106] 13 C NMR (100 MHz, CDCl 3 ,TMS):d 151.1,140.7,136.3,129.7,128.2,127.6,127.5126.3,125.3,123.1,122.4,116.3,77.4,77.0,76.7,43.8,24.4,17.8,13.1.
[0107] Preparation of 2-[1-(4-acridinium-2-methyl-6-ethylphenylimino)ethyl]-pyridinylnickel dibromide (Ni-4)
[0108] Nickel complex Ni-4(R 1 =Me, R 2 =Et, X is Br, R 3 , R 4 , R 5 All H) were synthesized in one pot. The Schlenk tube was loaded with 2-acetylpyridine (0.024 g, 0.20 mmol), 2-methyl-6-ethyl-4-acridinylaniline (0.19 g, 0.60 mmol) and NiBr 2 (DME) (0.06 g, 0.20 mmol) was refluxed with acetic acid (30 mL). The reaction was continued at 120 °C for 6 hours and the volatiles were evaporated using a pump to obtain a concentrated solution. The nickel complex was precipitated using ether (20 mL), filtered, washed with ether (3×15 mL), and isolated in good yield (0.09 g, 71%) as an air-stable brick-red powder.
[0109] The structural confirmation data are as follows:
[0110] FT-IR(cm -1 ):3031(w),2962(w),2264(w),1608(ν(C=N),w),1543(m),1478
[0111] (m),1448(s),1373(w),1304(w),1251(s),1210(w),1116(w),1095(w),1029(w),945(w),880(w),812(w),753(s).
[0112] Elemental analysis: C 29 H 25 Br 2 Ni 3 (634.04) Theoretical value: C, 54.94; H, 3.97, N, 6.63%. Exp. value: C, 55.13; H, 3.91; N, 6.42%.
[0113] Example 5
[0114] Preparation of 2,6-dichloro-4-acridineaniline (A5)
[0115] 2,6-Dichloroaniline (1.94 g, 12 mmol) and 9-hydroxyacridine (3 g, 15 mmol) were placed in a 250 mL round bottom flask. The mixture was stirred at 130 °C under nitrogen for 30 minutes, and then a catalytic amount of ZnCl in HCl solution was added dropwise. 2 The reaction mixture was further heated for 2 hours and after cooling, the solid was dissolved in DCM (200 mL). It was filtered and washed twice with saturated solutions of ammonium chloride and sodium chloride. The organic portion was collected and washed with anhydrous Na 2 SO 4 Dry and concentrate under reduced pressure. The product was recrystallized from DCM using n-heptane to give a white crystalline solid (1.30 g, 36%).
[0116] The structural confirmation data are as follows:
[0117] 1 H NMR (400 MHz, CDCl 3 ,TMS):d 7.15(t,J=3.8Hz,2H,Ar-H),7.12–7.06(m,4H,Ar-H),6.96(t,J=3.8Hz,2H,Ar-H),6.76(s,2H,Ar-H m ),5.12(s,1H),3.51(s,2H,NH 2 ).
[0118] 13C NMR (100 MHz, CDCl 3 ,TMS):d 151.1,141.7,135.3,129.4,128.1,127.8,127.5126.2,125.6,122.3,119.1,77.4,77.4,76.3,42.7,23.3,22.5.
[0119] Preparation of 2-[1-(4-acridine-2,6-dichlorophenylimino)ethyl]-pyridinylnickel dibromide (Ni-5)
[0120] Nickel complex Ni-5(R 1 =R 2 =Cl, X is Br, R 3 , R 4 , R 5 All H) were synthesized in one pot. The Schlenk tube was loaded with 2-acetylpyridine (0.024 g, 0.20 mmol), 2,6-dichloro-4-acridinylaniline (0.21 g, 0.60 mmol) and NiBr 2 (DME) (0.06 g, 0.20 mmol) was refluxed with acetic acid (30 mL). The reaction was continued at 120 °C for 6 hours and the volatiles were evaporated using a pump to obtain a concentrated solution. The nickel complex was precipitated using ether (20 mL), filtered, washed with ether (3×15 mL), and isolated in good yield (0.10 g, 76%) as an air-stable brick-red powder.
[0121] The structural confirmation data are as follows:
[0122] FT-IR(cm -1 )::3296(w),2962(w),1624(ν(C=N),w),1547(w),1478(m),1448
[0123] (s),1371(w),1304(w),1251(s),1116(w),1095(w),1028(w),944(w),880(w),812(w),752(s).
[0124] Elemental analysis: C 26 H 17 Br 2 Cl 2 Ni 3 (660.84) Theoretical value: C, 47.26; H, 2.59; N, 6.36%. Experimental value: C, 47.38; H, 2.79; N, 6.34%.
[0125] Example 6 Complex Ni-1 and co-catalyst Et2 Ethylene polymerization under AlCl high pressure combined catalysis
[0126] a) Under ethylene atmosphere, 25 mL of a toluene solution of catalyst Ni-1 (3.0 μmol) was injected into a 250 mL stainless steel autoclave equipped with a mechanical stirrer, followed by the addition of 25 mL of toluene and the required amount of 1.3 mL of the cocatalyst Et 2 AlCl (1.17 mol / L in toluene), continue to add toluene to make the total volume of the solvent 100 mL. At this time, Al / Ni = 500:1. Mechanical stirring begins, maintained at 400 rpm, when the polymerization temperature reaches 20°C, ethylene is filled into the reactor, and the polymerization reaction begins. Maintain an ethylene pressure of 10 atm at 20°C, stir and carry out the polymerization reaction for 30 minutes. Neutralize the reaction solution with 10% hydrochloric acid-acidified ethanol solution to obtain a polymer precipitate, wash it several times with ethanol, vacuum dry it at 60°C to constant weight, weigh 5.76 g of polymer, polymerization activity: 3.84×10 6 g(PE)(mol Ni) -1 h -1 The molecular weight of the obtained polymer is M w =13kg·mol -1 , molecular weight distribution M w / M n =1.6(M w is the weight average molecular weight of the polymer, M n is the number average molecular weight of the polymer, obtained by GPC test), polymer T m =66.4℃(T m is the melting temperature of the polymer, measured by DSC).
[0127] b) is basically the same as method a) in this embodiment, except that the polymerization temperature is 30°C. Polymerization activity: 4.58×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =15.9 kg·mol -1 , molecular weight distribution M w / M n =1.5, polymer T m =55.6℃.
[0128] Take 10 mg of the obtained polymer, dissolve it in 3 ml of deuterated 1,1,2,2-tetrachloroethane, and test the polymer at 100 °C. 1 H data, such as Figure 1 As shown, the signal is accumulated 64 times.
[0129] Take 60 mg of the obtained polymer, dissolve it in 3 ml of deuterated 1,1,2,2-tetrachloroethane, and test the polymer at 100 °C. 13 C data, such as Figure 2 The signal is accumulated 3000 times.
[0130] c) is basically the same as method a) in this embodiment, except that the polymerization temperature is 40°C. Polymerization activity: 1.8×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =21.1 kg·mol -1 , molecular weight distribution M w / M n =1.8, polymer T m =62.1℃.
[0131] d) is basically the same as method a) in this embodiment, except that the polymerization temperature is 50°C. Polymerization activity: 0.4×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =13.1kg·mol -1 , molecular weight distribution M w / M n =1.5, polymer T m =68.5℃.
[0132] e) is basically the same as method b) in this embodiment, except that: 0.8 mL of the co-catalyst Et 2 AlCl (1.17 mol / L in toluene) makes Al / Ni=300:1. Polymerization activity: 3.43×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =15.8kg·mol -1 , molecular weight distribution M w / M n =1.7, polymer T m =53.0℃.
[0133] f) is basically the same as method b) in this embodiment, except that: 1.0 mL of the co-catalyst Et 2 AlCl (1.17 mol / L in toluene) makes Al / Ni=400:1. Polymerization activity: 3.8×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight Mw =14.4 kg·mol -1 , molecular weight distribution M w / M n =1.6, polymer T m =55.7℃.
[0134] g) is basically the same as method b) in this embodiment, except that: 1.5 mL of the co-catalyst Et 2 AlCl (1.17 mol / L in toluene) makes Al / Ni=600:1. Polymerization activity: 3.83×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =16.8kg·mol -1 , molecular weight distribution M w / M n =1.6, polymer T m =55.8℃.
[0135] h) is basically the same as method b) in this embodiment, except that: 1.8 mL of the co-catalyst Et 2 AlCl (1.17 mol / L in toluene) makes Al / Ni=700:1. Polymerization activity: 3.49×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =17.6 kg·mol -1 , molecular weight distribution M w / M n =1.6, polymer T m =52.2℃.
[0136] i) is basically the same as method b) in this embodiment, except that: 2.0 mL of the co-catalyst Et 2 AlCl (1.17 mol / L in toluene) makes Al / Ni=800:1. Polymerization activity: 2.54×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =16.3kg·mol -1 , molecular weight distribution M w / M n =1.59, polymer T m =51.1℃.
[0137] Example 7 Complex Ni-2 and co-catalyst Et 2Ethylene polymerization under AlCl high pressure combined catalysis
[0138] Basically the same as Example 6b), except that the main catalyst is Ni-2. Polymerization activity: 3.87×10 6 g(PE)(molNi) -1 h -1 , polymer molecular weight M w =15.7 kg·mol -1 , molecular weight distribution M w / M n =1.5, polymer T m =67.1℃.
[0139] Example 8 Complex Ni-3 and Promoter Et 2 Ethylene polymerization under AlCl high pressure combined catalysis
[0140] Basically the same as Example 6b), except that the main catalyst is Ni-3. Polymerization activity: 0.05×10 6 g(PE)(molNi) -1 h -1 , polymer molecular weight M w =15.4 kg·mol -1 , molecular weight distribution M w / M n =1.7, polymer T m =75.7℃.
[0141] Example 9 Complex Ni-4 and Promoter Et 2 Ethylene polymerization under AlCl high pressure combined catalysis
[0142] Basically the same as Example 6b), except that the main catalyst is Ni-4. Polymerization activity: 3.68×10 6 g(PE)(molNi) -1 h -1 , polymer molecular weight M w =19.4 kg·mol -1 , molecular weight distribution M w / M n =1.6, polymer T m =66.6℃.
[0143] Example 10 Complex Ni-5 and co-catalyst Et 2 Ethylene polymerization under AlCl high pressure combined catalysis
[0144] Basically the same as Example 6b), except that the main catalyst is Ni-5. This catalytic combination has no catalytic activity for ethylene polymerization.
[0145] Example 11: Co-catalyzed ethylene polymerization by complex Ni-1 and co-catalyst MMAO under high pressure
[0146] a) In an ethylene atmosphere, 25 mL of a toluene solution of catalyst Ni-1 (3.0 μmol) was injected into a 250 mL stainless steel autoclave equipped with mechanical stirring, followed by the addition of 25 mL toluene, the required amount of 1.5 mL of co-catalyst MMAO (2.00 mol / L in n-hexane), and the addition of toluene to make the total volume of the solvent 100 mL. At this time, Al / Ni = 1000:1. Mechanical stirring was started and maintained at 400 rpm. When the polymerization temperature reached 20°C, ethylene was charged into the reactor and the polymerization reaction began. The ethylene pressure was maintained at 10 atm at 20°C and the polymerization reaction was stirred for 30 min. The reaction solution was neutralized with an ethanol solution acidified with 10% hydrochloric acid to obtain a polymer precipitate, which was washed several times with ethanol and dried at 60°C in vacuum to constant weight. 4.50 g of polymer was weighed, and the polymerization activity was 3.0×10 6 g(PE)(mol Ni) -1 h -1 The molecular weight of the obtained polymer is M w =16.8kg·mol -1 , molecular weight distribution M w / M n =1.8(M w is the weight average molecular weight of the polymer, M n is the number average molecular weight of the polymer, obtained by GPC test), polymer T m =74.9℃(T m is the melting temperature of the polymer, measured by DSC).
[0147] b) is basically the same as method a) in this embodiment, except that the polymerization temperature is 30°C. Polymerization activity: 3.6×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =18.7 kg·mol -1 , molecular weight distribution M w / M n =1.70, polymer T m =59.7℃.
[0148] c) is basically the same as method a) in this embodiment, except that the polymerization temperature is 40°C. Polymerization activity: 2.3×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =15.7 kg·mol -1, molecular weight distribution M w / M n =1.57, polymer T m =58.1℃.
[0149] d) is basically the same as method a) in this embodiment, except that the polymerization temperature is 50°C. Polymerization activity: 1.1×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =13.1kg·mol -1 , molecular weight distribution M w / M n =1.55, polymer T m =50.4℃.
[0150] e) is basically the same as method a) in this embodiment, except that the polymerization temperature is 60°C. Polymerization activity: 0.8×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =20.5kg·mol -1 , molecular weight distribution M w / M n =1.55, polymer T m =61.6℃.
[0151] f) is basically the same as method b) in this example, except that 1.9 mL of the cocatalyst MMAO (2.00 mol / L in n-hexane) is used to make Al / Ni=1500:1. Polymerization activity: 4.0×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =18.9 kg·mol -1 , molecular weight distribution M w / M n =1.67, polymer T m =59.3℃.
[0152] g) is basically the same as method b) in this example, except that 2.3 mL of the cocatalyst MMAO (2.00 mol / L in n-hexane) makes Al / Ni=1750:1. Polymerization activity: 4.6×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =23.0kg·mol -1 , molecular weight distribution Mw / M n =1.67, polymer T m =59.3℃.
[0153] h) is basically the same as method b) in this example, except that 3.0 mL of the cocatalyst MMAO (2.00 mol / L in n-hexane) is used to make Al / Ni=2000:1. Polymerization activity: 2.9×10 6 g(PE)(mol Ni) -1 h -1 , polymer molecular weight M w =20.8kg·mol -1 , molecular weight distribution M w / M n =1.62, polymer T m =63.9℃.
[0154] Example 12: Co-catalyzed ethylene polymerization under high pressure using complex Ni-2 and co-catalyst MMAO
[0155] Basically the same as Example 11g), except that the main catalyst is Ni-2. Polymerization activity: 4.3×10 6 g(PE)(molNi) -1 h -1 , polymer molecular weight M w =21.1 kg·mol -1 , molecular weight distribution M w / M n =1.69, polymer T m =82.6℃.
[0156] Example 13: Co-catalyzed ethylene polymerization under high pressure using complex Ni-3 and co-catalyst MMAO
[0157] Basically the same as Example 11g), except that the main catalyst is Ni-3. Polymerization activity: 0.21×10 6 g(PE)(molNi) -1 h -1 , polymer molecular weight M w =13.6 kg·mol -1 , molecular weight distribution M w / M n =1.75, polymer T m =75.3℃.
[0158] Example 14: Co-catalyzed ethylene polymerization under high pressure using complex Ni-4 and co-catalyst MMAO
[0159] Basically the same as Example 11g), except that the main catalyst is Ni-4. Polymerization activity: 2.4×10 6 g(PE)(molNi) -1 h -1 , polymer molecular weight M w =24.1kg·mol -1 , molecular weight distribution M w / M n =1.68, polymer T m =75.3℃.
[0160] Example 15: Co-catalyzed ethylene polymerization under high pressure using complex Ni-5 and co-catalyst MMAO
[0161] Basically the same as Example 11g), except that the main catalyst is Ni-5. Polymerization activity: 0.06×10 6 g(PE)(molNi) -1 h -1 , polymer molecular weight M w =17.3kg·mol -1 , molecular weight distribution M w / M n =1.54, polymer T m =82.8℃.
[0162] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A transition metal nickel complex, characterized in that: Having a structure as shown in formula (I): wherein each X is the same or different and is independently selected from F, Cl, Br, I; R 1 , R 2 , R 3 , R 4 , R 5 The same or different, each independently selected from one or more R a Substituted with the following groups: H, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-20 Aryl or C 6-20 Heteroatom aromatic group; R a Selected from H, F, Cl, Br, I, C 1-6 Alkyl, C 1-6 Alkoxy, C 3-10 Heterocyclic group, C 6-20 Aryl or C 6-20 heteroatom aromatic, and each R a Same or different.
2. The transition metal nickel complex according to claim 1, characterized in that In formula (I), R 1 Selected from C 1-3 Alkyl and Cl; more preferably methyl.
3. The transition metal nickel complex according to claim 1, characterized in that In formula (I), R 2 Selected from C 1-3 Alkyl and Cl; more preferably methyl.
4. The transition metal nickel complex according to claim 1, characterized in that In formula (I), R 3 , R 4 The same or different, each independently selected from H and C 1-6 Alkyl; more preferably all are H.
5. The transition metal nickel complex according to claim 1, characterized in that In formula (I), R 1 =R 2 =Me, X is Cl, R 3 , R 4 , R 5 All are H; or R 1 =R 2 =Et, X is Cl, R 3 , R 4 , R 5 All are H; or R 1 =R 2 =iPr, X is Cl, R 3 , R 4 , R 5 All are H; or R 1 =Me, R 2 =Et, X is Cl, R 3 , R 4 , R 5 All are H; or R 1 =R 2 =Cl, X is Cl, R 3 , R 4 , R 5 Both are H.
6. The method for preparing the transition metal nickel complex according to any one of claims 1 to 5, characterized in that: The following steps are involved: The aniline compound represented by formula (II) is subjected to condensation reaction with 2-acetylpyridine and compound NiX2 to obtain a metal complex represented by formula (I); wherein each X is the same or different and is independently selected from F, Cl, Br, I; R 1 , R 2 , R 3 , R 4 , R 5 The same or different, each independently selected from one or more R a Substituted with the following groups: H, C 1-6 Alkyl, C 1-6 Alkoxy, C 6-20 Aryl or C 6-20 Heteroatom aromatic group; R a Selected from H, F, Cl, Br, I, C 1-6 Alkyl, C 1-6 Alkoxy, C 3-10 Heterocyclic group, C 6-20 Aryl or C 6-20 heteroatom aromatic, and each R a Same or different.
7. The preparation method according to claim 6, characterized in that: The condensation reaction is carried out under anaerobic conditions.
8. The preparation method according to claim 6, characterized in that: The condensation reaction is carried out under the catalysis of an organic acid; the organic acid is one or more of formic acid, acetic acid and p-toluenesulfonic acid, preferably acetic acid.
9. The preparation method according to claim 6, characterized in that: The condensation reaction is carried out under heating reflux for 6 to 12 hours, preferably 8 to 10 hours.
10. The preparation method according to claim 6, characterized in that: The molar ratio of the compound NiX2 to the aniline compound represented by the formula (II) is 1:2-3, preferably 1:2-2.5, and more preferably 1:2.
5.
11. The preparation method according to claim 6, characterized in that: The method further comprises the step of purifying the obtained metal complex represented by formula (I), wherein the purification method comprises the following steps: A) removing volatile substances from the metal complex represented by formula (I) to obtain a concentrated solution, and adding the concentrated solution into an organic solvent for precipitation; b) subjecting the material precipitated in step a) to solid-liquid separation, washing the solid phase with an organic solvent and drying it. Wherein, the organic solvent is an anhydrous organic solvent.
12. A catalyst composition, characterized in that It comprises a main catalyst and, optionally, a co-catalyst, wherein the main catalyst is the transition metal nickel complex according to any one of claims 1 to 5, and the co-catalyst is one or more of aluminoxane, alkylaluminum and alkylaluminum chloride.
13. The catalyst composition according to claim 12, characterized in that The aluminoxane is methylaluminoxane and / or triisobutylaluminum-modified methylaluminoxane; the alkyl group in the alkylaluminum chloride is selected from C 1-3 The alkyl group is preferably diethylaluminum chloride and / or dimethylaluminum chloride.
14. The catalyst composition according to claim 12, characterized in that The molar ratio of the metal Al in the co-catalyst to the central metal Ni in the transition metal nickel complex is (200-4000):1, and the preferred molar ratio is (200-3500):
1.
15. The catalyst composition according to claim 14, characterized in that When the co-catalyst is methylaluminoxane, the molar ratio of the metal Al in the methylaluminoxane to the central metal Ni in the transition metal nickel complex is (2000-3000):1, and the more preferred molar ratio is 2500:1; When the co-catalyst is triisobutylaluminum-modified methylaluminoxane, the molar ratio of the metal Al in the triisobutylaluminum-modified methylaluminoxane to the central metal Ni in the transition metal nickel complex is (1000-2500):1, and the more preferred molar ratio is 1750:1; When the co-catalyst is alkylaluminum chloride, the molar ratio of metal Al in the alkylaluminum chloride to the central metal Ni in the transition metal nickel complex is (200-1500):1, and the more preferred molar ratio is 500:
1.
16. Use of the transition metal nickel complex according to any one of claims 1 to 5 or the catalyst composition according to any one of claims 12 to 15 in catalyzing olefin polymerization reactions.