Anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion as well as preparation method and application thereof
Through the preparation of anionic hyperbranched vegetable oil-based water-based polyurethane emulsion, and the copolymerization reaction of branched soybean oil-based polyol and isophorone diisocyanate, the problem of insufficient water resistance and hardness of water-based polyurethane wood paint is solved, and high water resistance is achieved The coating effect of toughness and hardness promotes its application in the field of wood paint.
Patent Information
- Application Number
- CN202411026979.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing water-based polyurethane wood paints have deficiencies in water resistance and hardness, which limits their application and sustainable development.
Anionic hyperbranched vegetable oil-based water-based polyurethane emulsion is used, through the copolymerization reaction of branched soybean oil-based polyol, isophorone diisocyanate and 2,4-dihydroxymethylbutyric acid, combined with a neutralizing agent for pre-neutralization and neutralization Emulsified to form a polyurethane coating with high water resistance and hardness.
It significantly improves the water resistance and hardness of vegetable oil-based water-based polyurethane wood paint, broadens its application field in water-based wood paint, and the method is safe, green, and simple to operate.
Smart Images

Figure CN118725237A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane emulsions, and specifically relates to an anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion and a preparation method and application thereof. Background Art
[0002] With the development of economy and the improvement of environmental awareness, people are paying more attention to the improvement of life quality and health, and the application of home decoration and furniture coatings has quietly changed from oil-based paint to water-based paint. Today, as people pay more and more attention to paint safety and environmental protection indicators, the promotion of water-based wood coatings has a very positive role in promoting the rational use of resources and the improvement of environmental protection. It is becoming more and more popular in the market because of its low-hazard and low-pollution characteristics.
[0003] Waterborne polyurethane wood paint is based on polyurethane resin as the main component and film-forming material. In addition to being environmentally friendly, it also has the advantages of good construction performance, high solid content, high paint film hardness, excellent wear resistance and impact resistance, and is an environmentally friendly wood coating with excellent performance. However, the preparation of waterborne polyurethane still mainly relies on petrochemical resources, which makes waterborne polyurethane wood paint affected by many factors such as the increasing consumption of petrochemical resources and the unstable price of fossil raw materials, which is not conducive to the durability and sustainable development of waterborne polyurethane wood paint. Vegetable oil is a typical renewable biomass resource, and natural oils (such as tung oil) have been used for wood coatings for a long time. Using vegetable oil to replace petrochemical resources to develop bio-based waterborne polyurethane for wood coating is not only theoretically feasible, but also has the advantage of sustainable regeneration and easy availability. However, as the main film-forming component in waterborne wood paint, the practical performance of vegetable oil-based waterborne polyurethane is still limited. For example, vegetable oil-based waterborne polyurethane wood paint still has the disadvantages of poor water resistance and low hardness.
[0004] Therefore, it is necessary to design a vegetable oil-based waterborne polyurethane wood paint with high water resistance and high hardness to meet its use requirements. Summary of the invention
[0005] The purpose of the present invention is to provide an anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion and a preparation method and application thereof. The waterborne polyurethane emulsion provided by the present invention has the advantages of excellent water resistance and high hardness after film formation.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The invention provides an anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion, which comprises the following components in parts by weight: 80-120 parts of branched soybean oil-based polyol, 30-70 parts of isophorone diisocyanate, 8-20 parts of 2,4-dihydroxymethylbutyric acid, 5-12 parts of a neutralizer and 500-800 parts of water.
[0008] Preferably, the neutralizing agent includes one or more of triethylamine, triethanolamine, ammonia water, diethanolamine, sodium hydroxide, potassium hydroxide, trimethylamine and tripropylamine.
[0009] Preferably, the solid content of the anionic hyperbranched vegetable oil-based aqueous polyurethane emulsion is 20-40%.
[0010] Preferably, the biobased content of the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion is 40-60%.
[0011] The present invention also provides a method for preparing the anionic hyperbranched vegetable oil-based aqueous polyurethane emulsion described in the above technical solution, comprising the following steps:
[0012] Mixing 2,4-dihydroxymethylbutyric acid and a neutralizing agent to obtain pre-neutralized 2,4-dihydroxymethylbutyric acid;
[0013] The pre-neutralized 2,4-dihydroxymethylbutyric acid, branched soybean oil-based polyol and isophorone diisocyanate are mixed and polymerized, and when the viscosity of the obtained prepolymer increases, an organic solvent is added for dilution, and the reaction is continued until the NCO group content in the system drops below 5%, thereby obtaining a polymer system;
[0014] The polymer system is cooled to room temperature, water is added for emulsification, and then the organic solvent is removed to obtain the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion.
[0015] Preferably, the molar ratio of active groups in the pre-neutralized 2,4-dihydroxymethylbutyric acid, branched soybean oil-based polyol and isophorone diisocyanate is: -OH group: -OH group: -NCO group = 0.69-1.19: 1: 1.7-2.2.
[0016] Preferably, the polymerization temperature is 65 to 90° C. and the polymerization time is 5 to 30 minutes.
[0017] Preferably, the organic solvent includes one or more of butanone and acetone;
[0018] Based on the weight of the branched soybean oil-based polyol, the weight of the organic solvent is 120 to 300 parts.
[0019] Preferably, the NCO group content is determined by back titration, with bromocresol green in the titration solution as an indicator and 0.5 mol / L KOH solution as a standard titrant.
[0020] The present invention also provides the use of the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion described in the above technical scheme or the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion prepared by the preparation method described in the above technical scheme in waterborne wood paint.
[0021] The present invention provides an anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion, comprising the following components in parts by weight: 80 to 120 parts of branched soybean oil-based polyol, 30 to 70 parts of isophorone diisocyanate, 8 to 20 parts of 2,4-dihydroxymethylbutyric acid, 5 to 12 parts of a neutralizer, and 500 to 800 parts of water. In the present invention, the neutralizer can pre-neutralize 2,2-dihydroxymethylbutyric acid, and further copolymerization can occur between the branched soybean oil-based polyol and the pre-neutralized 2,2-dihydroxymethylbutyric acid and isophorone diisocyanate, thereby increasing the degree of ionization of the hyperbranched polyurethane network and promoting the formation of a more stable polyurethane emulsion. The present invention utilizes the branched structure of the branched soybean oil-based polyol to construct a hyperbranched waterborne polyurethane, which can be applied to waterborne wood paint, and improves the water resistance and hardness of the vegetable oil-based waterborne polyurethane wood paint coating through a dense cross-linked structure.
[0022] The present invention also provides a method for preparing the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion described in the above technical solution, comprising the following steps: mixing 2,4-dihydroxymethylbutyric acid and a neutralizer to obtain pre-neutralized 2,4-dihydroxymethylbutyric acid; mixing the pre-neutralized 2,4-dihydroxymethylbutyric acid, a branched soybean oil-based polyol and isophorone diisocyanate to polymerize, adding an organic solvent to dilute the obtained prepolymer when the viscosity increases, and continuing to react until the NCO group content in the system decreases to less than 5% to obtain a polymer system; cooling the polymer system to room temperature, adding water to emulsify it, and then removing the organic solvent to obtain the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion. The present invention uses only branched soybean oil-based polyol as a single polyol, and the reaction conditions without toxic catalysts make the synthesis route of polyurethane safer and greener, with a high degree of reaction. The use of hyperbranched soybean oil-based polyol improves the tensile strength and hardness of water-based polyurethane, and the operation is simple. Compared with the same type of materials, the paint film has higher water resistance, can be applied to water-based wood paint, and further broadens its application field. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic diagram of the technical route for preparing the polyurethane emulsion in Example 1;
[0024] Figure 2 The appearance and particle size distribution diagram of the polyurethane emulsions obtained in the examples and comparative examples;
[0025] Figure 3 The water resistance test results of the polyurethane emulsions obtained in the examples and comparative examples are as follows;
[0026] Figure 4 The figure is a graph showing the hardness test results of the polyurethane emulsions obtained in the examples and comparative examples after film formation. DETAILED DESCRIPTION
[0027] The invention provides an anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion, which comprises the following components in parts by weight: 80-120 parts of branched soybean oil-based polyol, 30-70 parts of isophorone diisocyanate, 8-20 parts of 2,4-dihydroxymethylbutyric acid, 5-12 parts of a neutralizer and 500-800 parts of water.
[0028] In the present invention, unless otherwise specified, all components are commercially available products well known to those skilled in the art.
[0029] In parts by weight, the anionic hyperbranched vegetable oil-based aqueous polyurethane emulsion provided by the present invention includes 80 to 120 parts of branched soybean oil-based polyols, more preferably 90 to 110 parts, and more preferably 95 to 100 parts. In the present invention, the branched soybean oil-based polyols are preferably soybean oil-based polyols commercially available from Nantong Haierma Technology Co., Ltd., and the models preferably include HM-11350, HM-635A, HM-635C, HM-10100, HM-10200, HM-1070, HM-13150, HM-11350B, HM-13160, HM-13160A, HM-13200 or HM-828T-165.
[0030] Based on the weight of the branched soybean oil-based polyol, the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion provided by the present invention includes 30 to 70 parts of isophorone diisocyanate, more preferably 40 to 60 parts, and more preferably 50 parts.
[0031] Based on the weight of the branched soybean oil-based polyol, the anionic hyperbranched vegetable oil-based aqueous polyurethane emulsion provided by the present invention includes 8 to 20 parts of 2,4-dihydroxymethylbutyric acid, more preferably 10 to 18 parts, and more preferably 12 to 15 parts.
[0032] Based on the weight of the branched soybean oil-based polyol, the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion provided by the present invention includes 5 to 12 parts of a neutralizer, more preferably 6 to 11 parts, and more preferably 7 to 10 parts. In the present invention, the neutralizer preferably includes one or more of triethylamine, triethanolamine, ammonia water, diethanolamine, sodium hydroxide, potassium hydroxide, trimethylamine and tripropylamine.
[0033] Based on the weight percentage of the branched soybean oil-based polyol, the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion provided by the present invention includes 500 to 800 parts of water, and more preferably 600 to 700 parts.
[0034] In the present invention, the solid content of the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion is preferably 20-40%, more preferably 30%. In the present invention, the biobased content of the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion is preferably 40-60%, more preferably 50%.
[0035] The present invention also provides a method for preparing the anionic hyperbranched vegetable oil-based aqueous polyurethane emulsion described in the above technical solution, comprising the following steps:
[0036] Mixing 2,4-dihydroxymethylbutyric acid and a neutralizing agent to obtain pre-neutralized 2,4-dihydroxymethylbutyric acid;
[0037] The pre-neutralized 2,4-dihydroxymethylbutyric acid, branched soybean oil-based polyol and isophorone diisocyanate are mixed and polymerized, and when the viscosity of the obtained prepolymer increases, an organic solvent is added for dilution, and the reaction is continued until the NCO group content in the system drops below 5%, thereby obtaining a polymer system;
[0038] The polymer system is cooled to room temperature, water is added for emulsification, and then the organic solvent is removed to obtain the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion.
[0039] The present invention mixes 2,4-dihydroxymethylbutyric acid and a neutralizer to obtain pre-neutralized 2,4-dihydroxymethylbutyric acid.
[0040] The present invention has no particular limitation on the mixing process, and any method known to those skilled in the art may be used.
[0041] After obtaining the pre-neutralized 2,4-dihydroxymethylbutyric acid, the present invention mixes the pre-neutralized 2,4-dihydroxymethylbutyric acid, branched soybean oil-based polyol and isophorone diisocyanate to perform polymerization. When the viscosity of the obtained prepolymer increases, an organic solvent is added for dilution, and the reaction is continued until the NCO group content in the system drops to less than 5%, thereby obtaining a polymer system.
[0042] In the present invention, the molar ratio of active groups in the pre-neutralized 2,4-dihydroxymethylbutyric acid, branched soybean oil-based polyol and isophorone diisocyanate is preferably: -OH group: -OH group: -NCO group = 0.69-1.19: 1: 1.7-2.2.
[0043] In the present invention, the polymerization temperature is preferably 65 to 90° C., and the polymerization time is preferably 5 to 30 minutes. In the present invention, no catalyst is added during the polymerization process.
[0044] In the present invention, the organic solvent preferably includes one or more of butanone and acetone; based on the weight of the branched soybean oil-based polyol, the weight of the organic solvent is preferably 120 to 300 parts, more preferably 150 to 280 parts, and more preferably 200 to 250 parts.
[0045] In the present invention, the NCO group content is preferably determined by back titration, and bromocresol green is preferably used as an indicator in the titration solution, and 0.5 mol / L KOH solution is preferably used as a standard titrant. The present invention has no special limitation on the process of the back titration method, and the method well known to those skilled in the art can be used.
[0046] After obtaining the polymer system, the present invention cools the polymer system to room temperature, adds water for emulsification, and then removes the organic solvent to obtain the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion.
[0047] In the present invention, the emulsification is carried out under stirring conditions, the stirring speed is preferably 300-500 rpm, and the time is preferably 2 hours.
[0048] In the present invention, the method of removing the organic solvent is preferably rotary evaporation. The present invention has no special limitation on the process of rotary evaporation, and the process well known to those skilled in the art can be adopted.
[0049] The present invention also provides the use of the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion described in the above technical solution or the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion prepared by the preparation method described in the above technical solution in waterborne wood coatings. The present invention does not specifically limit the specific implementation methods of the application, and those familiar to those skilled in the art can be used.
[0050] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] Example 1
[0052] Mix triethylamine (5.4 g) and 2,4-dihydroxybutyric acid (8.1 g) to obtain pre-neutralized 2,4-dihydroxybutyric acid;
[0053] Branched soybean oil polyol (HM-10100, 90 g), isophorone diisocyanate (30.3 g) and the pre-neutralized 2,4-dihydroxybutyric acid obtained above were added into a dry two-necked flask and stirred for 30 minutes. No catalyst was added during the reaction, and the reaction temperature was 68°C.
[0054] When the viscosity of the prepolymer in the system increases, 120g of butanone is added to reduce the viscosity of the prepolymer, and the reaction is continued. The NCO group is determined by back titration. Bromocresol green is used as an indicator in the titration solution, and a 0.5 mol / L KOH solution is used as a standard titrant. The NCO group content of the polymer is determined until it drops below 5%, and the system temperature is lowered to room temperature. Finally, deionized water (535.6g) is added to the double-necked bottle, and the polyurethane is emulsified for 2 hours by stirring at a speed of 350rpm; after removing the butanone by a rotary evaporator, the anionic hyperbranched soybean oil-based waterborne polyurethane emulsion is obtained.
[0055] Example 2
[0056] Mix triethylamine (8.55 g) and 2,4-dihydroxybutyric acid (13.05 g) to obtain pre-neutralized 2,4-dihydroxybutyric acid;
[0057] Branched soybean oil polyol (HM-13160, 90 g), isophorone diisocyanate (48.5 g) and the pre-neutralized 2,4-dihydroxybutyric acid obtained above were added into a dry two-necked flask and stirred for 25 minutes. No catalyst was added during the reaction, and the reaction temperature was 75°C.
[0058] When the viscosity of the prepolymer in the system increases, 150g of butanone is added to reduce the viscosity of the prepolymer, and the reaction is continued. The NCO group is determined by back titration. Bromocresol green is used as an indicator in the titration solution, and a 0.5 mol / L KOH solution is used as a standard titrant. The NCO group content of the polymer is determined until it drops below 5%, and the system temperature is lowered to room temperature. Finally, deionized water (641.1g) is added to the double-necked bottle, and the polyurethane is emulsified for 2 hours by stirring at a speed of 380rpm; after removing the butanone by a rotary evaporator, the anionic hyperbranched soybean oil-based waterborne polyurethane emulsion is obtained.
[0059] Example 3
[0060] Mix triethylamine (10.2 g) and 2,4-dihydroxybutyric acid (15.6 g) to obtain pre-neutralized 2,4-dihydroxybutyric acid;
[0061] Branched soybean oil polyol (HM-13150, 90 g), isophorone diisocyanate (57.45 g) and the pre-neutralized 2,4-dihydroxybutyric acid obtained above were added into a dry two-necked flask and stirred for 20 minutes. No catalyst was added during the reaction, and the reaction temperature was 80°C.
[0062] When the viscosity of the prepolymer in the system increases, 180g of butanone is added to reduce the viscosity of the prepolymer, and the reaction is continued. The NCO group is determined by back titration, and bromocresol green is used as an indicator in the titration solution, and a 0.5 mol / L KOH solution is used as a standard titrant to determine the NCO group content of the polymer until it drops below 5%, and the system temperature is lowered to room temperature. Finally, deionized water (693.9g) is added to the double-necked bottle, and the polyurethane is emulsified for 2 hours by stirring at a speed of 400rpm; after removing the butanone by a rotary evaporator, the anionic hyperbranched soybean oil-based waterborne polyurethane emulsion is obtained.
[0063] Example 4
[0064] Mix triethylamine (10.8 g) and 2,4-dihydroxybutyric acid (16.35 g) to obtain pre-neutralized 2,4-dihydroxybutyric acid;
[0065] Branched soybean oil polyol (HM-13200, 90 g), isophorone diisocyanate (60.6 g) and the pre-neutralized 2,4-dihydroxybutyric acid obtained above were added into a dry two-necked flask and stirred for 13 minutes. No catalyst was added during the reaction, and the reaction temperature was 85°C.
[0066] When the viscosity of the prepolymer in the system increases, 220g of butanone is added to reduce the viscosity of the prepolymer, and the reaction is continued. The NCO group is determined by back titration. Bromocresol green is used as an indicator in the titration solution, and a 0.5 mol / L KOH solution is used as a standard titrant. The NCO group content of the polymer is determined until it drops below 5%, and the system temperature is lowered to room temperature. Finally, deionized water (711.1g) is added to the double-necked bottle, and the polyurethane is emulsified for 2 hours by stirring at a speed of 430rpm; after removing the butanone by a rotary evaporator, the anionic hyperbranched soybean oil-based waterborne polyurethane emulsion is obtained.
[0067] Example 5
[0068] Mix triethylamine (10.8 g) and 2,4-dihydroxybutyric acid (16.35 g) to obtain pre-neutralized 2,4-dihydroxybutyric acid;
[0069] Branched soybean oil polyol (HM-10200, 90 g), isophorone diisocyanate (60.6 g) and the pre-neutralized 2,4-dihydroxybutyric acid obtained above were added into a dry two-necked flask and stirred for 10 minutes. No catalyst was added during the reaction, and the reaction temperature was 88°C.
[0070] When the viscosity of the prepolymer in the system increases, 270g of butanone is added to reduce the viscosity of the prepolymer, and the reaction is continued. The NCO group is determined by back titration. Bromocresol green is used as an indicator in the titration solution, and a 0.5 mol / L KOH solution is used as a standard titrant. The NCO group content of the polymer is determined until it drops below 5%, and the system temperature is lowered to room temperature. Finally, deionized water (750.6g) is added to the double-necked bottle, and the polyurethane is emulsified for 2 hours by stirring at a speed of 480rpm; after removing the butanone by a rotary evaporator, the anionic hyperbranched soybean oil-based waterborne polyurethane emulsion is obtained.
[0071] Comparative Example 1
[0072] Branched soybean oil polyol (HM-10100, 90 g), isophorone diisocyanate (30.3 g) and 2,4-dihydroxybutyric acid (8.1 g) were added into a dry two-necked flask and stirred for 30 minutes. No catalyst was added during the reaction, and the reaction temperature was 68°C.
[0073] When the viscosity of the prepolymer in the system increases, 120g of butanone is added to reduce the viscosity of the prepolymer, and the reaction is continued. The NCO group is determined by back titration. Bromocresol green is used as an indicator in the titration solution, and a 0.5mol / L KOH solution is used as a standard titrant. The NCO group content of the polymer is determined until it drops below 5%, and the system temperature is lowered to room temperature; triethylamine (5.4g) is added to neutralize the carboxyl group for 0.5h, and finally deionized water (535.6g) is added to the double-necked bottle, and the mixture is stirred at a speed of 350rpm. The polyurethane agglomerates in the deionized water and cannot be dispersed to form an emulsion.
[0074] Comparative Example 2
[0075] Mix triethylamine (5.4 g) and 2,4-dihydroxybutyric acid (8.1 g) to obtain pre-neutralized 2,4-dihydroxybutyric acid;
[0076] Branched soybean oil polyol (HM-10100, 90 g), isophorone diisocyanate (30.3 g) and the pre-neutralized 2,4-dihydroxybutyric acid obtained above were added to a dry two-necked flask and stirred for 30 minutes, and then an appropriate amount of dibutyltin dilaurate (15 μL) was added as a catalyst, and the reaction temperature was 68°C;
[0077] When the viscosity of the prepolymer in the system increases, 120g of butanone is added to reduce the viscosity of the prepolymer, and the reaction is continued. The NCO group is determined by back titration. Bromocresol green is used as an indicator in the titration solution, and a 0.5 mol / L KOH solution is used as a standard titrant. The NCO group content of the polymer is determined until it drops below 5%, and the system temperature is lowered to room temperature. Finally, deionized water (535.6g) is added to the double-necked bottle, and the polyurethane is emulsified for 2 hours by stirring at a speed of 350rpm; after removing the butanone by a rotary evaporator, an aqueous polyurethane emulsion is obtained.
[0078] Comparative Example 3
[0079] Mix triethylamine (8.7 g) and 2,4-dihydroxybutyric acid (13.2 g) to obtain pre-neutralized 2,4-dihydroxybutyric acid;
[0080] Castor oil polyol (90 g), isophorone diisocyanate (49.05 g) and the pre-neutralized 2,4-dihydroxybutyric acid obtained above were added into a dry two-necked flask and stirred for 30 minutes. No catalyst was added during the reaction, and the reaction temperature was 68°C.
[0081] When the viscosity of the prepolymer in the system increases, 120g of butanone is added to reduce the viscosity of the prepolymer, and the reaction is continued. The NCO group is determined by back titration. Bromocresol green is used as an indicator in the titration solution, and a 0.5 mol / L KOH solution is used as a standard titrant. The NCO group content of the polymer is determined until it drops below 5%, and the system temperature is lowered to room temperature. Finally, deionized water (644.7g) is added to the double-necked bottle, and the polyurethane is emulsified for 2 hours by stirring at a speed of 400rpm; after removing the butanone by a rotary evaporator, an aqueous polyurethane emulsion is obtained.
[0082] Performance Testing
[0083] Test Example 1
[0084] The properties of the polyurethane emulsions obtained in Examples 1 to 5 and Comparative Examples 1 to 3 were tested;
[0085] Sample preparation: The sample to be tested was diluted to 0.01 wt% and tested 4 times in parallel at room temperature, and the data were recorded as the mean ± standard deviation.
[0086] The particle size, distribution and Zeta potential of all samples were tested on a Zeta-sizerNano ZSE instrument.
[0087] The storage stability of the WPU dispersion was evaluated by centrifugation at 3000 rpm for 30 min in a Tomos 3-18 centrifuge. The test results are shown in Table 1. The appearance photos of the emulsion and the particle size distribution are shown in Table 1. Figure 2 As shown;
[0088] Table 1 Performance test results of polyurethane emulsions obtained in Examples and Comparative Examples
[0089] Group Appearance Storage period (years) Particle size (nm) Zeta potential (mV) Comparative Example 1WPU-HM-10100A - - - - Comparative Example 2WPU-HM-10100B milky 2 223.2±0.66 -41.3±0.13 Comparative Example 3WPU-CO milky 0.5 245.7±0.10 -40.4±0.02 Example 1 WPU-HM-10100 milky 2 200.7±0.10 -42.2±0.23 Example 2 WPU-HM-13160 milky 2 194.4±0.23 -59.8±1.28 Example 3 WPU-HM-13150 Blue transparent 2 130.4±0.21 -50.8±2.38 Example 4 WPU-HM-13200 Blue transparent 2 45.7±0.10 -49.8±1.28 Example 5 WPU-HM-10200 Blue transparent 2 34.4±0.23 -50.4±0.38
[0090] As can be seen from Table 1, the difference between Comparative Example 1 WPU-HM-10100A and Example 1 WPU-HM-10100 is that in the preparation scheme of Comparative Example 1 WPU-HM-10100A, the neutralizing agent triethylamine is added to the system to neutralize the carboxylic acid after the polyurethane polymerization reaction is completed. Due to the formation of the hyperbranched structure of the polyurethane, the carboxylic acid groups in the polyurethane are distributed in the hyperbranched structure, and the triethylamine will be affected by the hyperbranched structure during the neutralization of the carboxylic acid, so that the triethylamine is not fully neutralized with the carboxylic acid groups, and the insufficient hydrophilic groups in the polymer structure make it difficult to disperse during the emulsification process. In the scheme of Example 1 WPU-HM-10100, the neutralizing agent triethylamine is first neutralized with 2,4-dihydroxybutyric acid before the reaction, and the neutralized 2,4-dihydroxybutyric acid is then polymerized with isocyanate and polyol to prepare polyurethane. The salted carboxylic acid groups are distributed in the hyperbranched structure of the polyurethane to provide sufficient hydrophilicity for the polyurethane segments to promote the dispersion of polyurethane in water.
[0091] The difference between Comparative Example 2 WPU-HM-10100B and Example 1 WPU-HM-10100 is that in the preparation process of Comparative Example 2 WPU-HM-10100B, a catalyst dibutyltin dilaurate is added to promote the polymerization rate. The accelerated polymerization rate will lead to polymerization inhomogeneity and excessive crosslinking degree in some areas, which will further lead to uneven particle size distribution of polyurethane during dispersion (see Figure 2 ). In Example 1 WPU-HM-10100, due to the presence of 2,4-dihydroxybutyric acid neutralized by triethylamine, the alkaline triethylamine has a weak catalytic effect, which not only ensures the polymerization rate of the polyurethane, but also avoids excessive local cross-linking, and can form a homogeneous dispersion during the emulsification process.
[0092] In addition, it can be seen from Table 1 that the storage period of all examples is longer than that of Comparative Example 3. This is because the waterborne polyurethane prepared by branched soybean oil-based polyol has a more compact cross-linked structure than the waterborne polyurethane prepared by castor oil, so that the particle size of the formed polyurethane emulsion is smaller. In addition, the relatively small particle size has a larger specific surface area, which increases the Zeta potential of the emulsion. Small particle size and large Zeta potential provide dual guarantees for the storage stability of the emulsion.
[0093] Test Example 2
[0094] The polyurethane emulsions obtained in Examples 1 to 5 and Comparative Examples 2 to 3 were subjected to film formation; the film formation process was as follows: a certain amount of the emulsion was poured into a pre-siliconized glass dish, placed in a horizontal area to dry naturally for one week, and then the film was placed in an oven at 50° C. for further drying for 48 hours to obtain a final film sample;
[0095] The water resistance of the obtained film was evaluated by immersion method. The film was cut into squares with a length of 10 mm (thickness of about 0.5 mm), first dried at 60 ° C for 12 hours, and then the dried film was immersed in deionized water for 72 hours. Finally, the water absorption rate of the film in water was calculated as follows:
[0096] Water absorption rate (%) = (m 1 -m 0 ) / m 0 ×100%
[0097] The weight of the sample before and after immersion is measured as m 0 and m 1 . Each sample was measured more than four times and the average value was taken. The test results are as follows Figure 3 As shown;
[0098] Depend on Figure 3 It can be seen that the water absorption rate of comparative example 3 WPU-CO is as high as 32.36% after being immersed in deionized water for 72 hours. Compared with the comparative example, the water absorption rate of the embodiment with a hyperbranched structure after absorbing water for 72 hours is much lower than that of comparative example 3. Among them, Example 4 has the highest water absorption rate of 9.53%, which is 70% lower than that of comparative example 3 WPU-CO. In addition, the water absorption rate of the film is also closely related to the hydroxyl value and molecular weight of the polyol. HM-10200 used in Example 5 has the highest hydroxyl value and the largest molecular weight, which shows that HM-10200 has a highly branched structure, and the prepared waterborne polyurethane has the highest degree of hyperbranching, and the cross-linking structure is also the most compact, resulting in the material having the best water resistance (water absorption rate: 5.32%). The water absorption rate of the comparative example 2 WPU-HM-10100B film is twice that of the WPU-HM-10100 film in the example 1. This is because the addition of a catalyst in the comparative example 2 WPU-HM-10100B leads to an uneven distribution of hydrophilic groups and hydrophobic structures in the material structure, and the hydrophilic groups are more easily exposed to water molecules.
[0099] Test Example 3
[0100] The pencil hardness of the coatings prepared from the polyurethane emulsions of Examples 1 to 5 and Comparative Examples 2 to 3 was tested;
[0101] The pencil hardness of the coating was tested using ASTM D-3363. 1 mL of polyurethane emulsion was poured on a 5×10 cm 2The samples were prepared by placing the samples on tinplate and drying them in vacuum. Four parallel samples were tested for each sample.
[0102] The test results obtained are as follows Figure 4 As shown;
[0103] like Figure 4 As shown, the comparative example 3WPU-CO prepared from castor oil exhibits the worst pencil hardness of HB. This is because the flexible triglyceride structure of castor oil is relatively loose, and the three-dimensional network structure formed is loose and soft, resulting in a coating showing a lower pencil hardness. Compared with castor oil with a flexible triglyceride structure, the reactive sites of branched soybean oil-based polyols are dense, and a polyurethane coating with a more concentrated hard segment can be obtained, showing a higher pencil hardness. And the branched crosslinking points act as hard segment crosslinking in the coating to further increase the pencil hardness of the coating. Therefore, the coating prepared by HM-10200 with the highest hydroxyl value and molecular weight has the highest pencil hardness of 3H, which is 3 levels higher than the pencil hardness of comparative example 3WPU-CO. In addition, there is also a significant difference in the pencil hardness between comparative example 2WPU-HM-10100B and example 1WPU-HM-10100. The accumulation of the flexible structure in comparative example 2WPU-HM-10100B makes its pencil hardness only HB.
[0104] Test Example 4
[0105] Testing of film tensile properties;
[0106] Sample preparation and test method: The film samples of the obtained polyurethane emulsion after drying at room temperature were cut into rectangular samples of 30mm×10mm×1mm (length×width×thickness). The tensile properties of the film were measured on a tensile machine at an extension rate of 50mm / min. All samples were tested more than three times in the test, and the data were recorded as the average value ± standard deviation. The detailed data are shown in Table 2.
[0107] Table 2 Test results of tensile properties of polyurethane emulsion films obtained in Examples and Comparative Examples
[0108] sample Tensile strength(MPa) Elongation at break (%) Comparative Example 1WPU-HM-10100A - - Comparative Example 2WPU-HM-10100B 10.56±0.25 145.86±30.89 Comparative Example 3WPU-CO 6.73±0.50 257.07±75.25 Example 1 WPU-HM-10100 17.02±0.54 350.35±31.97 Example 2 WPU-HM-13160 14.80±0.38 318.63±56.85 Example 3 WPU-HM-13150 22.03±0.18 308.23±43.75 Example 4 WPU-HM-13200 16.25±0.56 337.26±34.52 Example 5 WPU-HM-10200 20.03±0.86 284.13±35.62
[0109] As can be seen from Table 2, in Comparative Example 1WPU-HM-10100A, the neutralizing agent triethylamine is added to the system to neutralize the carboxylic acid after the polyurethane polymerization reaction is completed. Due to the formation of the hyperbranched structure of the polyurethane, the carboxylic acid groups in the polyurethane are distributed in the hyperbranched structure. The carboxylic acid neutralization process of triethylamine will be affected by the hyperbranched structure, making the triethylamine inadequate in neutralizing the carboxylic acid groups, and the insufficient hydrophilic groups in the polymer structure make it difficult to disperse during the emulsification process. Therefore, it is impossible to prepare a film by emulsion film formation for tensile testing. The tensile strength and elongation at break of the film of Example 1 WPU-HM-10100 are 17.02MPa and 350.35%, respectively, while the tensile strength and elongation at break of the film of Comparative Example 2 WPU-HM-10100B are lower than those of Example 1 WPU-HM-10100, respectively, 10.56MPa and 145.86%, the main reason being that the catalyst dibutyltin dilaurate promotes the uneven polymerization of Comparative Example 2 WPU-HM-10100B, resulting in uneven distribution of the soft and hard segments of the film, causing stress concentration of the film during the stretching process. In addition, it can be seen from Table 2 that the tensile strength of all the examples is higher than that of Comparative Example 3 WPU-CO (tensile strength of 6.73MPa, elongation at break of 257.07%), which is because the waterborne polyurethane prepared by branched soybean oil-based polyol has a hyperbranched structure, and has a higher crosslinking density than the waterborne polyurethane prepared by castor oil.
[0110] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. An anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion, characterized in that: The invention comprises the following components in parts by weight: 80-120 parts of branched soybean oil-based polyol, 30-70 parts of isophorone diisocyanate, 8-20 parts of 2,4-dihydroxymethylbutyric acid, 5-12 parts of a neutralizing agent and 500-800 parts of water.
2. The anionic hyperbranched vegetable oil-based aqueous polyurethane emulsion according to claim 1, characterized in that: The neutralizing agent includes one or more of triethylamine, triethanolamine, ammonia water, diethanolamine, sodium hydroxide, potassium hydroxide, trimethylamine and tripropylamine.
3. The anionic hyperbranched vegetable oil-based aqueous polyurethane emulsion according to claim 1 or 2, characterized in that: The solid content of the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion is 20-40%.
4. The anionic hyperbranched vegetable oil-based aqueous polyurethane emulsion according to claim 3, characterized in that: The bio-based content of the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion is 40-60%.
5. The method for preparing the anionic hyperbranched vegetable oil-based aqueous polyurethane emulsion according to any one of claims 1 to 4, characterized in that: The following steps are involved: Mixing 2,4-dihydroxymethylbutyric acid and a neutralizing agent to obtain pre-neutralized 2,4-dihydroxymethylbutyric acid; The pre-neutralized 2,4-dihydroxymethylbutyric acid, branched soybean oil-based polyol and isophorone diisocyanate are mixed and polymerized, and when the viscosity of the obtained prepolymer increases, an organic solvent is added for dilution, and the reaction is continued until the NCO group content in the system drops below 5%, thereby obtaining a polymer system; The polymer system is cooled to room temperature, water is added for emulsification, and then the organic solvent is removed to obtain the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion.
6. The preparation method according to claim 5, characterized in that: The molar ratio of active groups in the pre-neutralized 2,4-dihydroxymethylbutyric acid, branched soybean oil-based polyol and isophorone diisocyanate is: -OH group: -OH group: -NCO group = 0.69-1.19: 1: 1.7-2.
2.
7. The preparation method according to claim 5, characterized in that: The polymerization temperature is 65-90° C. and the polymerization time is 5-30 min.
8. The preparation method according to claim 5, characterized in that: The organic solvent includes one or more of butanone and acetone; Based on the weight of the branched soybean oil-based polyol, the weight of the organic solvent is 120 to 300 parts.
9. The preparation method according to claim 5, characterized in that: The NCO group content is determined by back titration, with bromocresol green in the titration solution as an indicator and 0.5 mol / L KOH solution as a standard titrant.
10. Use of the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion according to any one of claims 1 to 4 or the anionic hyperbranched vegetable oil-based waterborne polyurethane emulsion prepared by the preparation method according to any one of claims 5 to 9 in waterborne wood coatings.
Citation Information
Patent Citations
Preparation method of waterborne polyurethane, inner-crosslinking polyurethane-acrylate and preparation method of inner-crosslinking polyurethane-acrylate
CN107556454A
Vegetable oil-based anionic type waterborne polyurethane emulsion as well as preparation method and application thereof
CN108467467A
Application of plant oil-base waterborne polyurethane emulsion as styling product and hair styling product
CN109796569A
Aqueous polyurethane dispersion for use as binder in quick-drying paint for cars, is based on high- and low-molecular weight diol compounds with polyhydroxy component, polyisocyanate and hydroxy- or amino-acid
DE19907988A1
An improved process for the preparation of stable aqueous urethane dispersions
EP0982331A1