Polyether-ether-ketone / carbon nanotube composite material and preparation method thereof
By synthesizing and applying specific dispersants, the problem of insufficient dispersion of carbon nanotubes in polyether ether ketone is solved, achieving uniform dispersion and high-performance preparation of carbon nanotube and polyether ether ketone composite materials, ensuring uniform resistance and cost-effectiveness.
Patent Information
- Application Number
- CN202410902435.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-07
- Publication Date
- 2024-10-01
AI Technical Summary
The insufficient dispersion of carbon nanotubes in polyetheretherketone (PEEK) limits the improvement of composite material performance. Existing chemical modification methods have harsh reaction conditions and unstable modification effects.
By synthesizing a dispersant using the reactants 4,4′-difluorobenzophenone, 4,4′-dichlorodiphenylsulfone or mixtures thereof with 4-hydroxypyrene and potassium carbonate at a specific molar ratio, The formed dispersant is mixed with polyether ether ketone and carbon nanotubes, heated and reacted in a closed reactor and washed and dried to obtain a powdered dispersant, which is then mixed with carbon nanotubes in a high-speed mixer and extruded through twin-screws. Machine granulation.
The uniform dispersion of carbon nanotubes in polyetheretherketone is achieved, the surface resistance is evenly distributed, the resistance is in the range of 106-9, the addition amount is small and the cost is low, and the product foaming phenomenon is avoided.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention discloses a polyetheretherketone / carbon nanotube composite material and also provides a preparation method thereof, belonging to the technical field of polymer composite materials. Background Art
[0002] Carbon nanotubes have broad application prospects in the field of polymer composites due to their excellent electrical, thermal and mechanical properties. However, the dispersion of carbon nanotubes in polymer matrices has always been a key issue restricting their application. Polyetheretherketone (PEEK), as a high-performance engineering plastic, has excellent heat resistance, mechanical properties and chemical stability, and its combination with carbon nanotubes is expected to further improve its performance. However, the dispersion of carbon nanotubes in PEEK also faces challenges, which limits the performance improvement of its composite materials.
[0003] At present, the methods for improving the dispersibility of carbon nanotubes in polymers mainly include physical blending and chemical modification. Although the physical blending method is simple to operate, it is often difficult to achieve uniform dispersion of carbon nanotubes. The chemical modification method can improve the compatibility with the polymer matrix by introducing functional groups or molecular chains on the surface of carbon nanotubes, thereby improving the dispersibility. However, the existing chemical modification methods often have problems such as harsh reaction conditions and unstable modification effects. Summary of the invention
[0004] The invention discloses a polyetheretherketone / carbon nanotube composite material and a preparation method thereof, which solves the dispersion problem of carbon nanotubes in PEEK by synthesizing a uniformly dispersed antistatic composite material, and provides technical support for the preparation of high-performance carbon nanotube / PEEK composite materials.
[0005] The polyetheretherketone / carbon nanotube composite material of the present invention is characterized by:
[0006] The dispersant is synthesized with reactant a and reactant b and added into the polyetheretherketone / carbon nanotube mixed system; the molar ratio of reactant a, reactant b and potassium carbonate is 1-10:2-20:1:-10:3-10.
[0007] The reactant a is selected from: 4,4′-difluorobenzophenone, 4,4′-dichlorodiphenyl sulfone or a mixture thereof in a ratio of (1 to 10): (1 to 10); The reactant is selected from: 4-hydroxypyrene; The solvent is selected from: one or a mixture of N-methylpyrrolidone, cyclopentane sulfone, diphenyl sulfone, N,N-dimethylacetamide in a mixing ratio of (1-10): (1-10): (1-10): (1-10).
[0008] The method for preparing a polyetheretherketone / carbon nanotube composite material of the present invention comprises the following steps:
[0009] 1. In a closed reactor connected to a condenser, a water separator and a nitrogen interface, nitrogen is continuously introduced, reactant a, reactant 4-hydroxypyrene, potassium carbonate and a solvent are added, heated to 150-300°C and reacted for 1-4 hours.
[0010] 2. After the reaction is completed, pour out the material in the flask, cool and crush it, wash it with 0-100% ethanol / deionized water solution (V / V) at 0-100℃ for 3-10 times, and dry it to obtain a powdered dispersant.
[0011] The positive effects of the present invention are: The synthesized dispersant has good surface affinity with polyetheretherketone and carbon nanotubes; the dispersant does not cause foaming of the product; the surface resistance of the polyetheretherketone / carbon nanotube composite material with the addition of the dispersant is evenly distributed, and can reach a resistance of 10 6-9 Small amount of addition and low cost. DETAILED DESCRIPTION
[0012] The present invention is further described by way of the following examples, which do not limit the present invention in any way. Without departing from the technical solution of the present invention, any modification or change made to the present invention that is easily implemented by a person of ordinary skill in the art will fall within the scope of the claims of the present invention. Example 1
[0013] 1. Nitrogen is continuously introduced into a sealed glass four-necked flask connected to a condenser, a water separator and a nitrogen interface, and 109.1g (0.5mol) 4,4′-difluorobenzophenone, 218.25g (1mol) 1-hydroxypyrene, 79.1g (0.5mol) potassium carbonate and 360.4g (3mol) sulfolane are added and heated to 270°C for reaction for 3 hours. After the reaction is completed, the material in the flask is poured into cold water to wash out, crushed, and washed 3-10 times with 0-100% ethanol / deionized water solution (V / V) at 0-100°C, and dried to obtain a powdered dispersant; 2. Take 10g of the dispersant prepared in step 1, 1950g of polyetheretherketone, and 40g of carbon nanotubes, mix them in a high-speed mixer for 1 hour, and melt-extrude them into granules through a twin-screw extruder. The temperature distribution of the twin-screw extruder is: 380℃; 360℃; 370℃; 375℃; 380℃; 385℃; 385℃; 380℃;: 375℃; 370℃; the main engine speed is 350rpm / min. Measure the particle resistance, injection-mold the sample in the injection molding machine, and measure the surface resistance. The results are shown in Table 1. Example 2
[0014] Take 12g of the dispersant prepared in step 1 of case 1, 1948g of polyetheretherketone, and 40g of carbon nanotubes, mix them in a high-speed mixer for 1 hour, and melt-extrude them into granules through a twin-screw extruder. The temperature distribution of the twin-screw extruder is: 380℃; 360℃; 370℃; 375℃; 380℃; 385℃; 385℃; 380℃;: 375℃; 370℃; the main engine speed is 350rpm / min. Measure the particle resistance, injection mold the sample in the injection molding machine, and measure the surface resistance. The results are shown in Table 1. Example 3
[0015] Take 15g of the dispersant prepared in step 1 of case 1, 1945g of polyetheretherketone, and 40g of carbon nanotubes, mix them in a high-speed mixer for 1 hour, and melt-extrude them into granules through a twin-screw extruder. The temperature distribution of the twin-screw extruder is: 380℃; 360℃; 370℃; 375℃; 380℃; 385℃; 385℃; 380℃;: 375℃; 370℃; the main engine speed is 350rpm / min. Measure the particle resistance, injection mold the sample in the injection molding machine, and measure the surface resistance. The results are shown in Table 1.
[0016] Comparative Example
[0017] Take 1960g of polyetheretherketone and 40g of carbon nanotubes, mix them in a high-speed mixer for 1 hour, and melt-extrude them into granules through a twin-screw extruder. The temperature distribution of the twin-screw extruder is: 380℃; 360℃; 370℃; 375℃; 380℃; 385℃; 385℃; 380℃;: 375℃; 370℃; the main engine speed is 350rpm / min. Measure the particle resistance, injection-mold the sample in the injection molding machine, and measure the surface resistance. The results are shown in Table 1.
[0018] Table 1 (Resistance range is expressed by the value displayed by SIMCO resistivity meter):
[0019] Conclusion: Through the analysis of Examples 1 to 3 and the comparative example, the resistance range obtained is relatively small and can be used as an antistatic material; while the resistance range of the comparative example is very large, less than 10 6-9 scope.
Claims
1. A dispersant for a polyetheretherketone / carbon nanotube composite material, characterized in that: A dispersant is synthesized with reactant a and reactant b, and added into a polyetheretherketone / carbon nanotube mixed system; the molar ratio of reactant a, reactant b and potassium carbonate is 1-10:2-20:1:-10:3-10; The reactant a is selected from: 4,4′-difluorobenzophenone, 4,4′-dichlorodiphenyl sulfone or a mixture thereof in a ratio of (1 to 10): (1 to 10); The reactant is selected from: 4-hydroxypyrene; The solvent is selected from: one or a mixture of N-methylpyrrolidone, cyclopentane sulfone, diphenyl sulfone, N,N-dimethylacetamide (1-10): (1-10): (1-10): (1-10).
2. A method for preparing a polyetheretherketone / carbon nanotube composite material, comprising the following steps: 1) In a closed reactor connected to a condenser, a water separator and a nitrogen interface, nitrogen is continuously introduced, reactant a, reactant 4-hydroxypyrene, potassium carbonate and a solvent are added, heated to 150-300°C and reacted for 1-4 hours; 2) After the reaction is completed, pour out the material in the flask, cool and crush it, wash it with 0-100% ethanol / deionized water solution (V / V) at 0-100°C for 3-10 times, and dry it to obtain a powdered dispersant; 3) 10-50 g of the prepared dispersant, 1900-1950 g of polyetheretherketone, and 20-40 g of carbon nanotubes are mixed in a high-speed mixer for 1 hour, and melt-extruded into granules through a twin-screw extruder; The temperature distribution of the twin-screw extruder is: 380°C; 360°C; 370°C; 375°C; 380°C; 385°C; 385°C; 380°C; 375°C; 370°C; the main engine speed is 350rpm / min, and the polyetheretherketone / carbon nanotube composite material is obtained.
Citation Information
Cited By
High-strength and high-toughness polyether-ether-ketone antistatic composite material based on interface selective distribution and preparation method thereof
CN121758947A