Magnetic metal organic framework material, preparation method thereof and application of magnetic metal organic framework material in enrichment and extraction of aflatoxin in oil phase

Through the preparation of magnetic metal-organic framework materials, the problems of high cost, complex operation and poor selectivity in food pre-processing technology are solved, efficient adsorption and recovery of aflatoxin is achieved, the operating process is simplified and detection efficiency is improved.

CN118725314APending Publication Date: 2024-10-01INNER MONGOLIA YILI IND GROUP CO LTD +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310290310.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing food pre-treatment technology has problems such as high cost, complex operation, poor selectivity, and inability to be reused, especially in the detection and removal process of aflatoxin, which is difficult to effectively solve.

Method used

Using the preparation method of magnetic metal-organic framework materials, magnetic Fe3O4 particles, ligands H3CTTA and Al(NO3)3·9H2O are mixed with N,N-dimethylformamide and acetic acid through a solvothermal reaction to prepare a stable and reproducible Magnetic metal-organic framework materials used for adsorption and enrichment of aflatoxins.

Benefits of technology

It achieves efficient adsorption and good recovery rate of aflatoxins, simplifies the operation process, avoids clogging of adsorbent packing, improves detection efficiency and accuracy, and has market application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725314A_ABST
    Figure CN118725314A_ABST
Patent Text Reader

Abstract

The invention provides a magnetic metal organic framework material, a preparation method thereof and application of the magnetic metal organic framework material in enrichment and extraction of aflatoxin in an oil phase, and the preparation method comprises the following steps: mixing raw materials including magnetic Fe3O4 particles, ligand H3CTTA and Al (NO3) 3.9 H2O with N, N-dimethylformamide and acetic acid, and carrying out solvothermal reaction to obtain the magnetic metal organic framework material. The magnetic metal organic framework material is good in stability, has high adsorption performance and good recovery rate on aflatoxin, and can be used for detecting or removing aflatoxin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of sample pretreatment and composite material synthesis, and specifically relates to the preparation of a magnetic metal organic framework material and the application of the material in enriching aflatoxin in an oil phase. Background Art

[0002] Nowadays, the problem of mycotoxin contamination in vegetable oils has gradually attracted widespread attention from countries around the world and has become the focus of attention in the field of food safety. Aflatoxin is a highly toxic hepatocarcinogen, mainly a secondary metabolite produced by Aspergillus flavus and Aspergillus parasites. Among them, aflatoxin B1 (AFB1) is identified as a Class I carcinogen by the International Agency for Research on Cancer and is the strongest carcinogenic compound among known carcinogens. GB2761-2017 "National Food Safety Standard Limits of Mycotoxins in Food" stipulates that the content of AFB1 in peanut oil and corn oil shall not exceed 20μg / kg, and that in other edible oils shall not exceed 10μg / kg. Although there are no restrictions on the content of aflatoxin B2, G1 and G2 in edible oils, the problem of aflatoxin contamination is seriously threatening the development of the grain and oil industry and affecting the health of the people. It is also very important to strengthen the monitoring of aflatoxin B2, G1 and G2 in edible oils. For the detection of aflatoxin, the sample pretreatment process determines the detection limit, precision and accuracy of the method, and is one of the most important steps in the detection and analysis.

[0003] Magnetic solid phase extraction (MSPE) technology is a new type of sample pretreatment technology developed in recent years. The magnetic properties of the adsorbent can be used to separate the adsorbent from the sample solution under the action of an external magnetic field. Compared with traditional filtration or centrifugation steps, it improves the separation efficiency and avoids the problem of adsorbent filler clogging. MSPE adsorbent materials play a key role in magnetic solid phase extraction. Choosing a suitable magnetic adsorbent is crucial to improving the selectivity, adsorption capacity and efficiency of MSPE.

[0004] Metal-organic frameworks (MOFs) are a new type of hybrid material that combines metal ions with organic linkers through coordination bonds. MOFs have attracted widespread interest in the fields of gas storage, sensors, separations, and sample pretreatment. Due to their advantages such as different structural topologies, adjustable pore sizes, permanent nanoporosity, high specific surface area, and good thermal stability, magnetic MOFs are also widely used in sample pretreatment for food testing. Summary of the invention

[0005] In order to solve the problems of high cost, complicated operation, poor selectivity, and non-reusability in current food pretreatment technology, the purpose of the present invention is to provide a magnetic metal organic framework material and its preparation method and application. The magnetic metal organic framework material has good stability, high adsorption performance and good recovery rate for aflatoxin, can be used for the detection or removal of aflatoxin, and the material is reusable.

[0006] In order to achieve the above object, the present invention provides a method for preparing a magnetic metal organic framework material, which comprises the following steps:

[0007] Mixing raw materials including magnetic Fe3O4 particles, ligand H3CTTA, Al(NO3)3·9H2O with N,N-dimethylformamide and acetic acid; wherein the mass ratio of the magnetic Fe3O4 particles, the ligand H3CTTA, and Al(NO3)3·9H2O is (0.5-3):(5-8):6; the volume ratio of the acetic acid to N,N-dimethylformamide is (1-4):15, and the total mass concentration of the magnetic Fe3O4 particles, the ligand H3CTTA, and Al(NO3)3·9H2O is 6.6-9.35 g / L;

[0008] The magnetic metal organic framework material is obtained through a solvent thermal reaction.

[0009] According to a specific embodiment of the present invention, preferably, the mass ratio of the magnetic Fe3O4 particles, the ligand H3CTTA, and Al(NO3)3·9H2O is 1-3:5:6.

[0010] In the above preparation method, the ligand H3CTTA (chemical formula is C 30 H 24 O6; 1,3,5-trimethyl-2,4,6-tris(4-carboxyphenyl)benzene) has the following structure:

[0011]

[0012] In the synthesis process of magnetic materials, the combination effect of magnetic microspheres Fe3O4 and metal organic framework materials (BUT-18) is not ideal. The magnetic material prepared by the present invention has a stable combination and optimizes the usage of magnetic microspheres Fe3O4 in the reaction conditions.

[0013] According to a specific embodiment of the present invention, preferably, the magnetic Fe3O4 particles are prepared by a solvothermal method, and the solvothermal method comprises the following steps:

[0014] Weigh FeCl3·6H2O and dissolve it in ethylene glycol, add sodium acetate trihydrate, pour it into a polytetrafluoroethylene-lined and sealed reactor after dissolution, place it in an oven for reaction, wash it with water and ethanol after the reaction is completed, and dry it to obtain the magnetic Fe3O4 particles.

[0015] According to a specific embodiment of the present invention, preferably, the temperature of the solvent thermal reaction is 200-220° C., and the reaction time is 48-72 h.

[0016] According to a specific embodiment of the present invention, the above preparation method specifically comprises the following steps:

[0017] (1) Using a solvothermal method to synthesize magnetic Fe3O4 particles in one step: FeCl3·6H2O is weighed and dissolved in an ethylene glycol solution, and then a certain proportion of sodium acetate trihydrate is added thereto. After heating at a certain temperature and stirring with a magnetic stirrer to ensure complete dissolution, the mixture is poured into a polytetrafluoroethylene-lined and sealed reactor and placed in an oven for reaction. After the reaction is completed, the mixture is washed with water and ethanol and dried in an oven to obtain black magnetic Fe3O4 particles;

[0018] (2) Weigh a certain proportion of magnetic Fe3O4 particles, organic ligand H3CTTA and metal compound Al(NO3)3·9H2O into a polytetrafluoroethylene liner;

[0019] (3) Add N,N-dimethylformamide and acetic acid solution to the above polytetrafluoroethylene liner, transfer the mixed solution to a polytetrafluoroethylene-lined stainless steel autoclave after ultrasonic treatment and place it in an oven for reaction; the specific dosage ratio is, for example: 10 mg magnetic Fe3O4 particles, 50 mg H3CTTA and 60 mg Al(NO3)3·9H2O metal compound, as well as 15 mL of N,N-dimethylformamide and 2.5 mL of acetic acid.

[0020] According to a specific embodiment of the present invention, preferably, the above preparation method further comprises step (4): after the reaction is completed, the product is collected by external magnetic force, washed with N,N-dimethylformamide and methanol, and placed in an oven to dry to obtain a magnetic composite metal-organic framework material, represented by Fe3O4@BUT-18.

[0021] According to a specific embodiment of the present invention, preferably, the diluent is water.

[0022] The present invention also provides a magnetic metal organic framework material, which is prepared by the above preparation method.

[0023] The present invention also provides the use of the magnetic metal organic framework material as a magnetic solid phase extraction adsorbent in enriching and extracting aflatoxin in an oil phase, specifically as a magnetic solid phase extraction adsorbent to adsorb, detect or remove pollutants containing aflatoxin in the oil phase.

[0024] According to a specific embodiment of the present invention, preferably, the aflatoxin includes one or a combination of two or more of aflatoxin B1, aflatoxin B2, aflatoxin G1, and aflatoxin G2.

[0025] According to a specific embodiment of the present invention, preferably, the aflatoxin is a combination of aflatoxin B1, aflatoxin B2, aflatoxin G1, aflatoxin G2, etc. The magnetic metal organic framework material provided by the present invention can simultaneously achieve the adsorption of the above four aflatoxins.

[0026] According to a specific embodiment of the present invention, preferably, the above application can be carried out according to the following steps:

[0027] (1) Take the oil phase to be tested, add the extract and centrifuge to obtain the supernatant;

[0028] (2) adding a diluent to the supernatant, and adding the magnetic metal organic framework material provided by the present invention to obtain a mixed solution;

[0029] (3) recovering the magnetic metal organic framework material in the mixed solution by magnetic adsorption separation, and eluting aflatoxin from the recovered magnetic metal organic framework material by an eluent to obtain an eluent;

[0030] (4) The eluate is blown dry with nitrogen and the target substance is detected after redissolution.

[0031] According to a specific embodiment of the present invention, preferably, in the above application, the oil phase is vegetable oil, such as peanut oil, corn oil, soybean oil and the like.

[0032] The traditional experimental procedure is generally to blow the extracted liquid with nitrogen to dryness, then add an appropriate amount of solution to dissolve it and then conduct a magnetic solid phase extraction experiment. The method provided by the present invention directly conducts a magnetic solid phase extraction experiment after diluting the extract with an aqueous solution, which effectively improves the pretreatment efficiency compared to the nitrogen blowing experimental procedure.

[0033] According to a specific embodiment of the present invention, preferably, the ratio of the amount of the magnetic metal organic framework material added to the volume of the supernatant is (6-16):1, more preferably (6-12):1, for example 10:1.

[0034] According to a specific embodiment of the present invention, preferably, in step (2), the mixed solution is subjected to ultrasonic treatment for 2-30 min, more preferably for 2 min.

[0035] According to a specific embodiment of the present invention, preferably, in step (2), the volume ratio of the diluent to the supernatant is (8-12):1, more preferably 10:1.

[0036] According to a specific embodiment of the present invention, preferably, in step (3), the eluent is an acetonitrile solution containing formic acid, more preferably an acetonitrile solution containing 0.1% formic acid (v / v, calculated based on the total volume of the formic acid-acetonitrile mixed solution formed as 100%).

[0037] According to a specific embodiment of the present invention, preferably, in step (3), the volume ratio of the eluent to the mixed solution is (1-2):11.

[0038] According to a specific embodiment of the present invention, the above-mentioned application method specifically comprises the following steps:

[0039] (1) Take an appropriate amount of vegetable oil and place it in a centrifuge tube, add a certain amount of extract to the vegetable oil sample, vortex mix, place it in a shaker for extraction, and centrifuge to obtain the supernatant for later use;

[0040] (2) Accurately take a certain amount of supernatant into a test tube, add an appropriate amount of water (diluent) to dilute and vortex, then add the material Fe3O4@BUT-18 and perform ultrasonic treatment to adsorb aflatoxin;

[0041] (3) using a magnet to separate and recover Fe3O4@BUT-18 in the mixed solution and pouring out the supernatant, and then adding an eluent to elute the target substance from the magnetic material to obtain an eluent;

[0042] (4) Finally, collect the eluted liquid and blow it with nitrogen until it is nearly dry. After re-dissolving, pass it through a membrane and conduct testing on a machine.

[0043] The magnetic metal organic framework material prepared by the preparation method provided by the present invention has good stability, and has both high adsorption performance and good recovery rate for aflatoxin. When it is applied to the detection of aflatoxin, the aflatoxin adsorbed in the magnetic material must be desorbed in the solvent with a corresponding solvent and then tested on a machine, and the material is separated and recovered by adsorption with a magnet. Compared with traditional filtration or centrifugation steps, the separation efficiency is improved, the problem of clogging of the adsorbent filler is avoided, and it has the characteristics of simple operation, excellent adsorption performance and market application potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is the SEM electron microscope image of the magnetic Fe3O4 particles in Example 1;

[0045] Figure 2 is the XRD diffraction pattern of Fe3O4@BUT-18 in Example 1;

[0046] Figure 3 is the XRD diffraction pattern of Fe3O4@BUT-18 in Example 2;

[0047] Figure 4 is the XRD diffraction pattern of Fe3O4@BUT-18 in Example 3;

[0048] Figure 5 FT-IR image of Fe3O4@BUT-18 in Example 1;

[0049] Figure 6 It is the VSM diagram of Fe3O4@BUT-18 in Example 1;

[0050] Figure 7 is the TGA graph of Fe3O4@BUT-18 in Example 1;

[0051] Figure 8 This is the result diagram of the effect of dilution volume on aflatoxin recovery rate;

[0052] Fig. 9 This is the result diagram of the effect of adsorbent dosage on aflatoxin recovery rate;

[0053] Fig.10 This is the result diagram of the effect of adsorption time on the recovery rate of aflatoxin;

[0054] Fig.11 This is the result diagram of the effect of pH value on the recovery rate of aflatoxin;

[0055] Fig.12 This is the result diagram of the effect of eluent on the recovery rate of aflatoxin;

[0056] Fig.13 This is the result diagram of the effect of elution time on the recovery rate of aflatoxin;

[0057] Fig.14 This is the result diagram of the effect of the eluent volume on the recovery rate of aflatoxin;

[0058] Fig.15 This is the XRD diagram of Fe3O4@BUT-18 under boiling water, PH=1, PH=10 and other conditions for 24 hours. DETAILED DESCRIPTION

[0059] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0060] The following specific examples all use the magnetic microspheres Fe3O4 obtained in Preparation Example 1, and the Fe3O4@BUT-18 material is synthesized mainly by changing the addition amount of magnetic Fe3O4 particles.

[0061] Preparation Example 1

[0062] This preparation example provides a magnetic Fe3O4 particle, which is prepared by the following steps:

[0063] The solvothermal method was used to synthesize magnetic Fe3O4 particles in one step: 1.3g FeCl3·6H2O was weighed and dissolved in 75ml ethylene glycol. After stirring with a magnetic stirrer at 50°C for 15min, 3.6g sodium acetate trihydrate was added and stirred for 30min. After ensuring complete dissolution, the mixture was poured into a polytetrafluoroethylene-lined and sealed reactor and placed in a 200°C oven for reaction for 16h. After the reaction was completed, the mixture was washed with water and ethanol three times each and dried at 65°C to obtain black magnetic Fe3O4 particles. The SEM electron microscope image is shown below. Figure 1 shown.

[0064] Example 1

[0065] This embodiment provides a magnetic metal organic framework material, which is prepared by the following steps:

[0066] 10 mg of magnetic Fe3O4 particles, 50 mg of organic ligand H3CTTA and 60 mg of metal compound Al(NO3)3·9H2O were weighed into a polytetrafluoroethylene liner; 15 mL of N,N-dimethylformamide and 2.5 mL of acetic acid were added, the mixed solution was ultrasonically treated for 10 min, then transferred to a polytetrafluoroethylene-lined stainless steel autoclave and placed in an oven at 200°C for reaction for 48 h; after the reaction, the product was collected by external magnetic force, washed with N,N-dimethylformamide and methanol for 3 times respectively, and placed in an oven at 80°C for drying to obtain the magnetic metal organic framework material Fe3O4@BUT-18, whose XRD diffraction pattern is shown as follows: Figure 2 As shown in the FT-IR diagram Figure 5 As shown in the VSM diagram Figure 6 As shown in the TGA diagram Figure 7 shown.

[0067] Example 2

[0068] This embodiment provides a magnetic metal organic framework material, which is prepared by the following steps:

[0069] Weigh 20 mg of magnetic Fe3O4 particles, 50 mg of organic ligand H3CTTA and 60 mg of metal compound Al(NO3)3·9H2O in a polytetrafluoroethylene liner; add 15 mL of N,N-dimethylformamide and 2.5 mL of acetic acid, transfer the mixed solution to a polytetrafluoroethylene-lined stainless steel autoclave after ultrasonic treatment for 10 min and place it in an oven at 200°C for reaction for 48 h; after the reaction, collect the product with an external magnetic force, wash it with N,N-dimethylformamide and methanol three times respectively, and place it in an oven at 80°C to dry, thereby obtaining the magnetic metal organic framework material Fe3O4@BUT-18, whose XRD diffraction pattern is shown in the figure. Figure 3 shown.

[0070] Example 3

[0071] This embodiment provides a magnetic metal organic framework material, which is prepared by the following steps:

[0072] 30 mg of magnetic Fe3O4 particles, 50 mg of organic ligand H3CTTA and 60 mg of metal compound Al(NO3)3·9H2O were weighed into a polytetrafluoroethylene liner; 15 mL of N,N-dimethylformamide and 2.5 mL of acetic acid were added, and the mixture was ultrasonically treated for 10 min and then transferred to a polytetrafluoroethylene-lined stainless steel autoclave and placed in an oven at 200°C for reaction for 48 h; after the reaction, the product was collected by external magnetic force, washed with N,N-dimethylformamide and methanol for 3 times respectively, and placed in an oven at 80°C for drying to obtain the magnetic metal organic framework material Fe3O4@BUT-18, whose XRD diffraction pattern is shown as follows: Figure 4 shown.

[0073] Magnetic solid phase extraction optimization

[0074] 1 ml of the vegetable oil sample extract was measured in a test tube and 10 ml of water was added to mix and dilute, and then 10 mg of Fe3O4@BUT-18 in Example 1 was added to obtain a mixed solution, and the test tube was ultrasonically treated for 2 minutes to adsorb aflatoxin; Fe3O4@BUT-18 in the mixed solution was separated and recovered by magnet adsorption and the supernatant was poured out, and then 1 ml of eluent (acetonitrile solution containing 0.1% formic acid, v / v, calculated based on the total volume of the formed formic acid-acetonitrile mixed solution as 100%) was added to elute the pollutants from the magnetic material to obtain an eluent; finally, the eluent was collected, blown to near dryness with nitrogen, and then re-dissolved and passed through a membrane for detection on a machine (according to standard GB5009.22-2016, using a high performance liquid chromatography-mass spectrometer for detection).

[0075] In order to improve the extraction efficiency of aflatoxin, the following AFs standard solution with a concentration of 20 μg / L was used to study the extraction parameters (diluent volume, adsorbent dosage, adsorption time, eluent type, eluent volume and elution time), and the extraction performance was evaluated by the extraction recovery rate, which was calculated according to the spike recovery formula;

[0076] Spike recovery formula: P = ((c2-c1) / c3) × 100%;

[0077] Wherein, P is the spike recovery rate; c1 is the sample concentration, i.e. the sample measurement value; c2 is the spiked sample concentration, i.e. the spiked sample measurement value; and c3 is the spiked amount.

[0078] 1. Effect of diluent volume

[0079] The extraction solution used for aflatoxin extraction in vegetable oil is acetonitrile-water solution (84:16, v:v), which has a desorption effect on aflatoxin adsorbed by magnetic materials. Therefore, water needs to be added during the adsorption process to reduce the desorption effect and allow the adsorbent material to adsorb as much toxin as possible. The recovery effect of adding 8, 10, 12, 14, and 16 mL of diluent (water) was explored. Figure 8 As shown, when the dilution volume was 10 ml, the magnetic metal organic framework material Fe3O4@BUT-18 had the highest recovery rate for the four toxins AFB1, AFB2, AFG1 and AFG2, which were 73.83%, 74.33%, 77% and 79.17% respectively.

[0080] 2. Effect of Fe3O4@BUT-18 dosage and adsorption time

[0081] The results of Fe3O4@BUT-18 dosage investigation are as follows Fig. 9 As shown in the figure, when the amount of Fe3O4@BUT-18 is 10 mg, the extraction efficiency is the highest. The continuous increase of Fe3O4@BUT-18 does not significantly improve the recovery rate. However, under the same elution conditions, too much adsorbent may affect the elution effect. Therefore, the amount of adsorbent is preferably 10 mg (relative to 1 mL, 20 μg / L concentration of AFs standard solution).

[0082] The results of adsorption time investigation are as follows Fig.10 As shown in the figure, in the 1-10 min adsorption process, the adsorption efficiency of the four toxins in the first 2 minutes reached more than 70%, and considering the importance of AFB1, 2 min was selected as the optimal adsorption time.

[0083] 3. Solution pH

[0084] The pH value will affect the extraction efficiency of AFs by the adsorbent. Therefore, the effect of solution pH on the extraction efficiency of AFs was studied in the range of 5-9. Fig.11 As shown, at different pH values, there was no significant difference in the recovery effect of the adsorbent on the target substance, and the solution with pH = 7 was selected for subsequent experimental optimization.

[0085] 4. Optimization of desorption conditions

[0086] Solid phase extraction is divided into two parts, one is the adsorption process, and the other is the desorption process, including the main influencing factors such as elution solvent, eluent volume and desorption time. Acetonitrile, methanol, ethanol, methanol: acetonitrile (v / v = 1:1) were selected as eluents (the eluents all contained 0.1% formic acid, v / v, calculated based on the total volume of the formed mixed solution as 100%) to study the elution effect on AFs. The results are shown in Fig.12As shown in the figure, all elution solvents have a certain elution effect, and acetonitrile has the best desorption effect. Therefore, acetonitrile is selected as the desorption solvent. In order to obtain better desorption conditions, the effect of desorption time on the extraction efficiency of AFs was studied. The experimental results show (see Fig.13 ), the recovery rate after 2 min did not increase due to the extension of desorption time and remained relatively stable. Therefore, 2 min was selected as the optimal desorption time. In addition, the effect of eluent volume on AFs desorption was studied in the range of 1-3 ml. When the eluent volume increased, the recovery efficiency did not change significantly ( Fig.14 ). Therefore, 1 ml of acetonitrile (containing 0.1% formic acid, v / v, calculated based on the total volume of the formic acid-acetonitrile mixed solution formed as 100%) was selected as the elution solvent.

[0087] Test Example 1

[0088] The Fe3O4@BUT-18 of the present application (the Fe3O4@BUT-18 obtained in Example 1 was used for the experiment) was immersed in a hydrochloric acid solution (pH=1), a sodium hydroxide solution (pH=10) and boiling water for 24 hours, and the XRD pattern measured (see Fig.15 ) shows its maintained crystallinity and unchanged structure, indicating that the material has good stability.

Claims

1. A method for preparing a magnetic metal organic framework material, comprising the following steps: Mixing raw materials including magnetic Fe3O4 particles, ligand H3CTTA, Al(NO3)3·9H2O with N,N-dimethylformamide and acetic acid, wherein the mass ratio of the magnetic Fe3O4 particles, the ligand H3CTTA, and Al(NO3)3·9H2O is (0.5-3):(5-8):6; the volume ratio of the acetic acid to N,N-dimethylformamide is (1-4):15; and the total mass concentration of the magnetic Fe3O4 particles, the ligand H3CTTA, and Al(NO3)3·9H2O is 6.6-9.35 g / L; Through a solvothermal reaction, the magnetic metal organic framework material is obtained; Preferably, the mass ratio of the magnetic Fe3O4 particles, the ligand H3CTTA, and Al(NO3)3·9H2O is 1-3:5:

6.

2. The preparation method according to claim 1, wherein The magnetic Fe3O4 particles are prepared by a solvothermal method, which comprises the following steps: Weigh FeCl3·6H2O and dissolve it in ethylene glycol, add sodium acetate trihydrate, pour it into a polytetrafluoroethylene-lined and sealed reactor after dissolution, place it in an oven for reaction, wash it with water and ethanol after the reaction is completed, and dry it to obtain the magnetic Fe3O4 particles.

3. The preparation method according to claim 1, wherein The temperature of the solvent thermal reaction is 200-220° C., and the reaction time is 48-72 hours.

4. A magnetic metal organic framework material, prepared by the preparation method according to any one of claims 1 to 3.

5. Use of the magnetic metal organic framework material according to claim 4 as a magnetic solid phase extraction adsorbent in enriching and extracting aflatoxin in an oil phase.

6. The use according to claim 5, wherein: The aflatoxins include one or a combination of two or more of aflatoxin B1, aflatoxin B2, aflatoxin G1, and aflatoxin G2.

7. The use according to claim 6, wherein: The aflatoxins are a combination of aflatoxin B1, aflatoxin B2, aflatoxin G1 and aflatoxin G2.

8. The use according to any one of claims 5 to 7, wherein: The application comprises the following steps: (1) Take the oil phase to be tested, add the extract and centrifuge to obtain the supernatant; (2) adding a diluent to the supernatant and adding the magnetic metal organic framework material to obtain a mixed solution; (3) recovering the magnetic metal organic framework material in the mixed solution by magnetic adsorption separation, and eluting aflatoxin from the recovered magnetic metal organic framework material with an eluent to obtain an eluent; Preferably, the eluent is further blown to dryness with nitrogen, and the target is detected after redissolution; Preferably, the diluent is water.

9. The use according to claim 8, wherein: The ratio of the amount of the magnetic metal organic framework material added to the volume of the supernatant is (6-16):1, preferably (6-12):1; Preferably, in step (2), the mixed solution is subjected to ultrasonic treatment for 2-30 min, more preferably for 2 min; Preferably, in step (2), the volume ratio of the diluent to the supernatant is (8-12):1, more preferably 10:1; Preferably, in step (3), the eluent is an acetonitrile solution containing formic acid, more preferably an acetonitrile solution containing 0.1% formic acid; Preferably, in step (3), the volume ratio of the eluent to the mixed solution is (1-2):

11.

10. The use according to claim 5 or 8, wherein: The oil phase is vegetable oil.

Citation Information

Cited By

  • Preparation method of ferroferric oxide and fluorine-containing organic framework core-shell structure material

    CN119588326A