Special bending-resistant environment-friendly cable material for medical equipment

By adding aluminum hydroxide and antioxidants to the cable material, and performing high-speed kneading and extrusion processing, the problem of bending resistance of the cable material when bent at a small radius is solved, and the service life and safety of the cable are improved. It is widely used in medical equipment and is environmentally friendly and highly flame retardant.

CN118725409APending Publication Date: 2024-10-01ANHUI KANGLIYA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410970007.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing cable materials have unsatisfactory bending resistance in medical equipment and are prone to breakage when bent at a small radius, affecting the service life and safety of the cable.

Method used

Add aluminum hydroxide and antioxidant to the raw material ratio of the cable material, and prepare pellets with high tensile strength and elongation at break through high-speed kneading and extrusion. Set the appropriate kneading temperature and drying humidity. , improve the bending resistance of cable materials.

Benefits of technology

It improves the bending resistance of cable materials, prevents rupture, extends service life, reduces safety hazards, and expands the scope of application. It is environmentally friendly and highly flame retardant.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725409A_ABST
    Figure CN118725409A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of cable materials, in particular to a special bending-resistant environment-friendly cable material for medical equipment, which is prepared from the following raw materials in parts by weight: 3-5 parts of a silane coupling agent, 1-2 parts of a crosslinking aid, 2-3 parts of aluminum hydroxide 140FD, 1-3 parts of an antioxidant and 6-10 parts of magnesium hydroxide. According to the cable material, the aluminum hydroxide and the antioxidant are added during raw material proportioning, so that the aluminum hydroxide and the antioxidant are fully mixed with other raw materials, and then extrusion and pelletizing treatment are performed after kneading, so that the obtained granules have relatively high tensile strength and elongation at break, and the bending and winding resistance of the cable material can be improved; when the cable is bent by a small radius, the cable material wrapping the cable is not easy to break, so that the protection effect on the internal cable is ensured, the potential safety hazard caused by cable exposure and insulation performance reduction is reduced, the application range of the cable material can be expanded, and the cable can be widely applied in the field of medical equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cable materials, in particular to a bending-resistant and environmentally friendly cable material specially used for medical equipment. Background Art

[0002] Plastics used for insulation and sheathing of wires and cables are commonly known as cable materials, which include rubber, plastic, nylon and other varieties. Almost all wire and cable products, except bare wire products such as steel core aluminum stranded wire and magnet wire, require insulation sealing. In medical equipment, cable materials are usually used to wrap and protect the outside of the cable to reduce damage during use and bending.

[0003] In the prior art, the bending resistance of the cable is not ideal, and the bending radius is large when in use. When the cable of medical equipment is bent with a small radius, the outer wrapped cable material is subjected to greater force and is prone to rupture. After rupture, the internal structure of the cable is prone to leakage, affecting the normal use of the cable, reducing the protection effect of the internal cables, and thereby shortening the overall service life of the cable.

[0004] Therefore, the present invention provides a bending-resistant and environmentally friendly cable material specially used for medical equipment, which is used to solve the above-mentioned related technical problems. Summary of the invention

[0005] The object of the present invention is to provide a bending-resistant and environmentally friendly cable material for medical equipment. The bending-resistant and environmentally friendly cable material for medical equipment prepared by the present invention is prepared by adding aluminum hydroxide and an antioxidant during the raw material ratio so that the aluminum hydroxide and the antioxidant are fully mixed with other raw materials, and then extruded and pelletized after kneading, so that the obtained pellets have high tensile strength and elongation at break; the kneading temperature is set when the raw materials are kneaded at high speed, thereby avoiding the interference of high temperature on the performance of the cable material and ensuring the stable performance of the cable material, thereby improving the bending resistance of the cable material, and the cable material wrapped on the outside is not easy to break when the cable is bent with a small radius, thereby ensuring the protection effect of the internal cables and reducing the safety hazards caused by cable exposure and reduced insulation performance, and expanding the scope of use of the cable material, so as to facilitate wide application in the field of medical equipment, and the humidity detection is carried out after the pellets are dehydrated and dried, so as to adjust the humidity of the pellets and avoid the excessive humidity of the pellets affecting subsequent storage and use effects.

[0006] To achieve the above object, the present invention provides the following technical solutions: The invention provides a bending-resistant and environmentally friendly cable material specially used for medical equipment. The cable material is prepared from the following raw materials in parts by weight: 3-5 parts of a silane coupling agent, 1-2 parts of a cross-linking aid, 2-3 parts of aluminum hydroxide 140FD, 1-3 parts of an antioxidant, and 6-10 parts of magnesium hydroxide.

[0007] The present invention is further configured to include the following steps: S1. Preliminary processing and batching of raw materials: screening antioxidants and magnesium hydroxide to remove internal impurities, and then weighing the silane coupling agent, cross-linking aid, aluminum hydroxide, antioxidant and magnesium hydroxide required for preparing the cable material according to the weight ratio to achieve the batching of the raw materials; S2, high-speed kneading: add the various raw materials in step S1 into the high-speed mixer in sequence, start the mixer to work for 10-20 minutes, and mix the raw materials evenly; S3, melt extrusion: after the raw materials are evenly mixed, the materials are concentrated and sent into a twin-screw extruder, and after melt blending and extrusion, the materials are extruded to form strips; S4, pelletizing and cooling: the strip material extruded in step S3 is sent into water for cooling. After the initial cooling, the extruded strip material is quickly pelletized by a pelletizer. The pelletized material is cooled and dried and then collected in a storage box.

[0008] The present invention is further configured as follows: in step S2, the mixing temperature of the high-speed mixer is 55-75°C.

[0009] The present invention is further configured as follows: in step S3, the temperature of the extruder is 170-200°C.

[0010] The present invention is further configured as follows: in step S3, the diameter of the pellets after cutting is 2-5 mm.

[0011] The present invention is further configured as follows: in step S4, when cooling and drying the pellets, the following contents are also included: S41, auxiliary feeding: start the power supply to make the centrifuge run idle, detect the rotating speed of the turntable to determine whether the centrifuge has a fault, and after passing the test, use circulating water to assist the movement of the pellets, and feed the pelletized pellets into the centrifugal dryer at a uniform speed; S42, dehydration and drying: the power of the centrifugal dryer is started again, the turntable drives the pellets to rotate at high speed, dehydrates the pellets, and completes the preliminary drying of the pellets. After the drying process, the pellets are taken out from the centrifugal dryer in a centralized manner; S43. Humidity detection: Use a temperature and humidity sensor to detect the humidity of the dried pellets. If the humidity is within the error range of the preset value, the pellets are placed in a storage box for storage. If the humidity of the pellets is higher than the preset value, a fan is used to perform secondary drying on the pellets until the humidity of the pellets is within the error range of the preset value.

[0012] The present invention is further configured as follows: in step S42, the rotating disk speed is 1200-1600 rpm, and the drying time is 5-12 seconds.

[0013] The present invention is further configured as follows: in the step S43, when the pellets are dried by a fan, the drying time is 1-3 minutes.

[0014] Compared with the prior art, the present invention has the following beneficial effects: In the present invention, aluminum hydroxide and an antioxidant are added during the raw material proportioning, so that the aluminum hydroxide and the antioxidant are fully mixed with other raw materials, and then the raw materials are kneaded, extruded, and pelletized to obtain pellets with high tensile strength and elongation at break; the kneading temperature is set when the raw materials are kneaded at high speed, thereby avoiding the interference of high temperature on the performance of the cable material and ensuring the stable performance of the cable material, thereby improving the bending resistance of the cable material, and the cable material wrapped outside is not easy to break when the cable is bent with a small radius, thereby ensuring the protection effect of the internal cable, reducing the safety hazards caused by cable exposure and reduced insulation performance, and expanding the use scope of the cable material, which is convenient for wide application in the field of medical equipment. After the pellets are dehydrated and dried, humidity detection is performed to adjust the humidity of the pellets to avoid excessive humidity of the pellets affecting subsequent storage and use effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 This is a flow chart of a bending-resistant and environmentally friendly cable material specially used for medical equipment of the present invention; Figure 2 This is a bar graph of the tensile strength of a bending-resistant and environmentally friendly cable material specially used for medical equipment according to the present invention. DETAILED DESCRIPTION

[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] Embodiment 1 Please refer to Figure 1-2 As shown, this embodiment provides a bending-resistant and environmentally friendly cable material specially used for medical equipment, which is made of the following raw materials in parts by weight: 3 parts of silane coupling agent, 1 part of cross-linking aid, 2 parts of aluminum hydroxide 140FD, 1 part of antioxidant, and 6 parts of magnesium hydroxide.

[0019] Among them, the model of the silane coupling agent is V172, the model of the cross-linking auxiliary agent is PL-500-EO, the model of the antioxidant is ST1010, and the model of the magnesium hydroxide is H5.

[0020] The following steps are also included: Step 1: Preliminary treatment and batching of raw materials: screening the antioxidant and magnesium hydroxide to remove internal impurities, and then weighing the silane coupling agent, cross-linking aid, aluminum hydroxide, antioxidant and magnesium hydroxide required for preparing the cable material according to the weight ratio to achieve the batching of the raw materials; Step 2: high-speed kneading: add the various raw materials in step 1 into the high-speed mixer in sequence, start the mixer and mix for 15 minutes to evenly mix the raw materials. The mixing temperature of the high-speed mixer is 65°C; Step 3, melt extrusion: After the raw materials are evenly mixed, the materials are concentrated into a twin-screw extruder, and after melt blending and extrusion, the materials are extruded to form strips. The temperature of the extruder is 175°C, and the diameter of the pellets after cutting is 2mm; Step 4, pelletizing and cooling: the strip material extruded in step 3 is sent into water for cooling. After the initial cooling, the extruded strip material is quickly pelletized by a pelletizer. The pelletized material is cooled and dried and then collected in a storage box. When cooling and drying the pellets, the following contents are also included: 41. Auxiliary feeding: Start the power supply to make the centrifuge run idle, detect the speed of the turntable to determine whether the centrifuge has a fault. After passing the test, use circulating water to assist the movement of the pellets, and feed the pelletized pellets into the centrifugal dryer at a uniform speed; 42. Dehydration and drying: Start the power of the centrifugal dryer again, the turntable drives the pellets to rotate at high speed, dehydrate the pellets, and complete the preliminary drying of the pellets. After the drying process, the pellets are taken out of the centrifugal dryer. The rotating disk speed is 1600rpm and the drying time is 12 seconds. 43. Humidity detection: Use a temperature and humidity sensor to detect the humidity of the dried pellets. If the humidity is within the error range of the preset value, the pellets are placed in a storage box for storage. If the humidity of the pellets is higher than the preset value, use a fan to dry the pellets for a second time until the humidity of the pellets is within the error range of the preset value. When the pellets are dried by a fan, the drying time is 3 minutes.

[0021] Embodiment 2 Please refer to Figure 1-2 As shown, this embodiment provides a bending-resistant and environmentally friendly cable material specially used for medical equipment, which is made of the following raw materials in parts by weight: 4 parts of silane coupling agent, 1 part of cross-linking aid, 2 parts of aluminum hydroxide 140FD, 2 parts of antioxidant, and 8 parts of magnesium hydroxide.

[0022] Among them, the model of the silane coupling agent is V172, the model of the cross-linking auxiliary agent is PL-500-EO, the model of the antioxidant is ST1010, and the model of the magnesium hydroxide is H5.

[0023] The following steps are also included: Step 1: Preliminary treatment and batching of raw materials: screening the antioxidant and magnesium hydroxide to remove internal impurities, and then weighing the silane coupling agent, cross-linking aid, aluminum hydroxide, antioxidant and magnesium hydroxide required for preparing the cable material according to the weight ratio to achieve the batching of the raw materials; Step 2, high-speed kneading: Add the various raw materials in step 1 into the high-speed mixer in sequence, start the mixer and mix for 12 minutes to evenly mix the raw materials. The mixing temperature of the high-speed mixer is 55°C; Step 3, melt extrusion: After the raw materials are evenly mixed, the materials are concentrated into a twin-screw extruder, and after melt blending and extrusion, the materials are extruded to form strips. The temperature of the extruder is 185°C, and the diameter of the pellets after cutting is 3mm; Step 4, pelletizing and cooling: the strip material extruded in step 3 is sent into water for cooling. After the initial cooling, the extruded strip material is quickly pelletized by a pelletizer. The pelletized material is cooled and dried and then collected in a storage box. The following steps are also included: 41. Auxiliary feeding: Start the power supply to make the centrifuge run idle, detect the speed of the turntable to determine whether the centrifuge has a fault. After passing the test, use circulating water to assist the movement of the pellets, and feed the pelletized pellets into the centrifugal dryer at a uniform speed; 42. Dehydration and drying: Start the power of the centrifugal dryer again, the turntable drives the pellets to rotate at high speed, dehydrate the pellets, and complete the preliminary drying of the pellets. After the drying process, the pellets are taken out from the centrifugal dryer. The rotating disk speed is 1450rpm and the drying time is 8 seconds. 43. Humidity detection: Use a temperature and humidity sensor to detect the humidity of the dried pellets. If the humidity is within the error range of the preset value, the pellets are placed in a storage box for storage. If the humidity of the pellets is higher than the preset value, use a fan to perform secondary drying on the pellets until the humidity of the pellets is within the error range of the preset value. When the pellets are dried by a fan, the drying time is 2 minutes.

[0024] Embodiment 3 Please refer to Figure 1-2 As shown, this embodiment provides a bending-resistant and environmentally friendly cable material specially used for medical equipment, which is made of the following raw materials in parts by weight: 5 parts of silane coupling agent, 2 parts of cross-linking aid, 3 parts of aluminum hydroxide 140FD, 3 parts of antioxidant, and 10 parts of magnesium hydroxide.

[0025] Among them, the model of the silane coupling agent is V172, the model of the cross-linking auxiliary agent is PL-500-EO, the model of the antioxidant is ST1010, and the model of the magnesium hydroxide is H5.

[0026] The following steps are also included: Step 1: Preliminary treatment and batching of raw materials: screening the antioxidant and magnesium hydroxide to remove internal impurities, and then weighing the silane coupling agent, cross-linking aid, aluminum hydroxide, antioxidant and magnesium hydroxide required for preparing the cable material according to the weight ratio to achieve the batching of the raw materials; Step 2, high-speed kneading: Add the various raw materials in step 1 into the high-speed mixer in sequence, start the mixer and mix for 10 minutes to evenly mix the raw materials. The mixing temperature of the high-speed mixer is 75°C; Step 3, melt extrusion: After the raw materials are evenly mixed, the materials are concentrated into a twin-screw extruder, and after melt blending and extrusion, the materials are extruded to form strips. The temperature of the extruder is 195°C, and the diameter of the pellets after cutting is 5mm; Step 4, pelletizing and cooling: the strip material extruded in step 3 is sent into water for cooling. After the initial cooling, the extruded strip material is quickly pelletized by a pelletizer. The pelletized material is cooled and dried and then collected in a storage box. When cooling and drying the pellets, the following contents are also included: 41. Auxiliary feeding: Start the power supply to make the centrifuge run idle, detect the speed of the turntable to determine whether the centrifuge has a fault. After passing the test, use circulating water to assist the movement of the pellets, and feed the pelletized pellets into the centrifugal dryer at a uniform speed; 42. Dehydration and drying: Start the power of the centrifugal dryer again, the turntable drives the pellets to rotate at high speed, dehydrate the pellets, and complete the preliminary drying of the pellets. After the drying process, the pellets are taken out of the centrifugal dryer. The rotating disk speed is 1200rpm and the drying time is 5 seconds. 43. Humidity detection: Use a temperature and humidity sensor to detect the humidity of the dried pellets. If the humidity is within the error range of the preset value, the pellets are placed in a storage box for storage. If the humidity of the pellets is higher than the preset value, use a fan to dry the pellets for a second time until the humidity of the pellets is within the error range of the preset value. When the pellets are dried by a fan, the drying time is 1 minute.

[0027] Comparative Example 1 Please refer to Figure 1-2 As shown, this embodiment provides a bending-resistant and environmentally friendly cable material specially used for medical equipment. The preparation method thereof is roughly the same as that of the first embodiment, with the main difference being that in step one, when the raw materials are processed and prepared, aluminum hydroxide is not added to the raw materials required for preparation.

[0028] Comparative Example 2 Please refer to Figure 1-2 As shown, this embodiment provides a bending-resistant and environmentally friendly cable material specially used for medical equipment. The preparation method thereof is roughly the same as that of the first embodiment, with the main difference being that in step 2, when the raw materials are processed and prepared, antioxidants are not added to the raw materials required for preparation.

[0029] Comparative Example 3 Please refer to Figure 1-2 As shown, this embodiment provides a bending-resistant and environmentally friendly cable material specially used for medical equipment. The preparation method thereof is substantially the same as that of the first embodiment, with the main difference being that in step 2, the mixing temperature of the high-speed mixer is 105°C.

[0030] Test Trial: The cable materials obtained by processing in Examples 1, 2 and 3 are recorded as Example Groups 1 to 3, and the cable materials obtained by processing in Comparative Examples 1 to 3 are recorded as Comparative Groups 1 to 3. According to GB / T1040.1-2006 standard, the tensile strength and elongation at break of the cable materials of Example Groups 1 to 3 and Comparative Groups 1 to 3 are tested, and the relevant test data are recorded in Table 1.

[0031] Table 1: Test data record table

[0032] It can be seen from Table 1 that the cable material obtained by processing through example groups 1 to 3 has a tensile strength of ≥12.9MPa, which is higher than the standard 10MPa, and an elongation at break of ≥163%, which is higher than the standard 150%. It has a high tensile strength, a large elongation at break, and good softness, elasticity and ductility. Therefore, the cable material obtained by processing through embodiments one, two and three has ideal bending resistance and a small bending radius. It is not easy to break when the cable dedicated to medical equipment is bent with a small radius, which can ensure the protection effect of the internal cables, thereby extending the overall service life of the cable.

[0033] By adjusting the content of aluminum hydroxide and antioxidant, the tensile strength and elongation at break of the cable material can be improved. When the tensile strength and elongation at break of the cable material decrease, the bending resistance of the cable material decreases, and the bending radius increases. Compared with group 1, in which aluminum hydroxide was not added, the tensile strength and elongation at break of the cable material were significantly reduced. Compared with group 2, in which antioxidant was not added, the tensile strength and elongation at break of the cable material were reduced. Compared with group 3, the temperature during kneading of the raw materials was increased, and the tensile strength and elongation at break of the cable material decreased. The high temperature of kneading can affect the tensile strength and elongation at break of the cable material. In the present invention, aluminum hydroxide and an antioxidant are added during the raw material ratio, and the aluminum hydroxide and the antioxidant are fully mixed with other raw materials, and then the raw materials are kneaded, extruded, and pelletized to obtain pellets with high tensile strength and elongation at break; the kneading temperature is set during the high-speed kneading of the raw materials, thereby avoiding the interference of high temperature on the performance of the cable material, ensuring the stable performance of the cable material, and thus improving the bending resistance of the cable material. When the cable is bent with a small radius, the cable material wrapped outside is not easy to break, thereby ensuring the protection effect of the internal cable and reducing the damage caused by cable exposure and reduced insulation performance. It can reduce safety hazards and expand the scope of use of cable materials, making it easy to be widely used in the field of medical equipment. After the pellets are dehydrated and dried, humidity detection is carried out to adjust the humidity of the pellets to avoid excessive humidity of the pellets affecting subsequent storage and use. Calcium zinc stabilizer is used as a stabilizer for the preparation of cable materials in the raw materials to assist in the preparation of cable materials, so that the prepared cable materials have high flame retardancy and are halogen-free. The cables produced using this cable material are not easy to burn, which can prevent the spread of flames and the expansion of disasters. Since the product does not contain halogen, it can solve the secondary pollution in the combustion process and has excellent environmental protection effects.

[0034] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0035] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A kind of bending-resistant and environmentally friendly cable material specially used for medical equipment, characterized by: The invention is prepared from the following raw materials in parts by weight: 3-5 parts of silane coupling agent, 1-2 parts of cross-linking auxiliary agent, 2-3 parts of aluminum hydroxide 140FD, 1-3 parts of antioxidant and 6-10 parts of magnesium hydroxide.

2. According to the environmentally friendly bending-resistant cable material for medical equipment described in claim 1, it is characterized by: The following steps are also included: S1. Preliminary processing and batching of raw materials: screening antioxidants and magnesium hydroxide to remove internal impurities, and then weighing the silane coupling agent, cross-linking aid, aluminum hydroxide, antioxidant and magnesium hydroxide required for preparing the cable material according to the weight ratio to achieve the batching of the raw materials; S2, high-speed kneading: add the various raw materials in step S1 into the high-speed mixer in sequence, start the mixer to work for 10-20 minutes, and mix the raw materials evenly; S3, melt extrusion: after the raw materials are evenly mixed, the materials are concentrated and sent into a twin-screw extruder, and after melt blending and extrusion, the materials are extruded to form strips; S4, pelletizing and cooling: the strip material extruded in step S3 is sent into water for cooling. After the initial cooling, the extruded strip material is quickly pelletized by a pelletizer. The pelletized material is cooled and dried and then collected in a storage box.

3. According to claim 2, a special bending-resistant and environmentally friendly cable material for medical equipment, characterized in that: In step S2, the mixing temperature of the high-speed mixer is 55-75°C.

4. According to claim 2, a special bending-resistant and environmentally friendly cable material for medical equipment, characterized in that: In step S3, the temperature of the extruder is 170-200°C.

5. According to claim 2, a special bending-resistant and environmentally friendly cable material for medical equipment, characterized in that: In step S3, the diameter of the pellets after cutting is 2-5 mm.

6. According to claim 2, a special bending-resistant and environmentally friendly cable material for medical equipment, characterized in that: In the step S4, the following steps are also included when cooling and drying the pellets: S41, auxiliary feeding: start the power supply to make the centrifuge run idle, detect the rotating speed of the turntable to determine whether the centrifuge has a fault, and after passing the test, use circulating water to assist the movement of the pellets, and feed the pelletized pellets into the centrifugal dryer at a uniform speed; S42, dehydration and drying: the power of the centrifugal dryer is started again, the turntable drives the pellets to rotate at high speed, dehydrates the pellets, and completes the preliminary drying of the pellets. After the drying process, the pellets are taken out from the centrifugal dryer in a centralized manner; S43. Humidity detection: Use a temperature and humidity sensor to detect the humidity of the dried pellets. If the humidity is within the error range of the preset value, the pellets are placed in a storage box for storage. If the humidity of the pellets is higher than the preset value, a fan is used to perform secondary drying on the pellets until the humidity of the pellets is within the error range of the preset value.

7. According to claim 6, a special bending-resistant and environmentally friendly cable material for medical equipment, characterized in that: In the step S42, the rotating disk speed is 1200-1600 rpm, and the drying time is 5-12 seconds.

8. According to claim 6, a special bending-resistant and environmentally friendly cable material for medical equipment, characterized in that: In the step S43, when the pellets are dried by a fan, the drying time is 1-3 minutes.