Additive containing alkyl borate and amino siloxane, anti-ionizing radiation aromatic polyester material and preparation method of anti-ionizing radiation aromatic polyester material
By using alkyl borate and amino siloxane additives in aromatic polyester materials, a fully saturated chain structure radiation-resistant additive is formed, which solves the problem that aromatic polyester materials are prone to embrittlement and yellowing under high ionizing radiation. It solves the problem of change and achieves improved mechanical properties and enhanced radiation toughness under high radiation doses.
Patent Information
- Application Number
- CN202410973759.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
AI Technical Summary
Aromatic polyester materials are prone to radiation embrittlement and radiation yellowing under high ionizing radiation. Traditional anti-radiation agents cannot effectively solve the problem, but instead aggravate the embrittlement and yellowing of the material.
An additive formula containing alkyl borate ester and amino siloxane is used as an aromatic polyester material resistant to ionizing radiation. By mixing alkyl borate ester with amino siloxane and aromatic polyester material, it is formed The radiation-resistant additive system with a fully saturated chain structure avoids aromatic hydrocarbon units and unsaturated olefin units, improving the radiation resistance of the material.
The mechanical strength and toughness of aromatic polyester materials are maintained or improved under high radiation doses, radiation embrittlement and yellowing are avoided, and material solidification caused by excessive radiation self-crosslinking is significantly alleviated, which has good industrial application prospects.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of radiation-resistant modification of materials, and in particular to an additive containing alkyl borate and aminosiloxane, an aromatic polyester material resistant to ionizing radiation and a preparation method thereof. Background Art
[0002] When plastics and other organic polymers are exposed to ionizing radiation such as high-energy electromagnetic waves, high-energy ion currents, and high-energy electron beams, the original molecular chains will be broken by high-energy impacts, forming free radicals or ionized fragment end groups. Then, these broken chain links tend to be mainly radiolytic or mainly cross-linked, depending on the chemical structure properties. In most cases, the continuous accumulation of high radiation doses will eventually cause the overall polymer material to tend to be radiolytic, showing adverse consequences such as radiation embrittlement and radiation yellowing of the material on a macro scale. At present, the widely used radiation disinfection of imported and exported goods, radiation sterilization of medical supplies, and nuclear power plant cable equipment all encounter the ionizing radiation hazards of plastics and other polymer parts or packaging materials. Therefore, the development of radiation-resistant formulas for plastics and other polymer materials has practical significance and economic value.
[0003] Aromatic polyesters are common materials in general-purpose plastics. The main problem they face in ionizing radiation is that due to the rigidity of the benzene ring units, radiation will cause excessive self-crosslinking, resulting in radiation embrittlement of this type of material. Traditional benzene-containing anti-radiation additives cannot overcome this contradiction, but instead aggravate the radiation yellowing and radiation embrittlement caused by the presence of aromatic units in the additives.
[0004] Based on this, the present invention provides an anti-radiation additive formulation system which does not contain aromatic units, has a molecular structure mainly composed of fully saturated CC or CO units, and has long-chain alkyl or alkoxy units with soft chain segments. Summary of the invention
[0005] The present invention aims to provide a fully saturated chain, high boiling point, easy-to-mix anti-radiation additive system to address the shortcomings of common aromatic hydrocarbon-containing anti-radiation agents that are prone to radiation yellowing and radiation embrittlement under high ionizing radiation doses. Compared with other traditional anti-radiation formulations, this formulation system does not have the disadvantage of radiation yellowing, and can maintain or improve the mechanical strength and toughness of aromatic polyester materials under a radiation dose of several hundred kGy.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0007] An additive is applicable to a formulation system of aromatic polyester for resisting ionizing radiation, and the additive comprises alkyl borate and aminosiloxane.
[0008] As a possible implementation mode, further, the aromatic polyester is a polycarboxylate having a benzene ring functional group structure in the molecular chain, such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polybutylene terephthalate adipate (PBAT) and other polyesters containing aromatic hydrocarbon structures.
[0009] As a possible implementation manner, further, the alkyl borate is a borate compound whose side group contains only saturated alkyl groups and whose alkyl carbon chain length is more than four carbon atoms, such as tributyl borate, tripentyl borate, trihexyl borate, and other alkyl borates.
[0010] As a possible implementation mode, further, the aminosiloxane is an organic silicon compound having a fully saturated molecular chain, an amino group at one end of the molecule and an alkoxy silicon structure at the other end, such as 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, etc.
[0011] The invention also provides an aromatic polyester material resistant to ionizing radiation, comprising aromatic polyester and the above additive.
[0012] As a possible implementation manner, further, the amount of the alkyl borate added is 0.1% to 10% relative to the total weight of the feed; the amount of the aminosiloxane added is 0.1% to 10% relative to the total weight of the feed.
[0013] Furthermore, the ionizing radiation resistant aromatic polyester material does not contain aromatic hydrocarbon structure and unsaturated olefin unit; the ionizing radiation resistant aromatic polyester material can withstand a processing temperature below about 300 degrees.
[0014] The present invention provides a method for preparing the above-mentioned aromatic polyester material resistant to ionizing radiation, characterized in that it comprises the following steps:
[0015] 1) Pre-drying the aromatic polyester raw material for standby use;
[0016] 2) adding alkyl borate and aminosiloxane to the dried pure aromatic polyester raw material and stirring to mix well;
[0017] 3) adding the mixed material to a melting device such as an internal mixer or a screw extruder, and mixing it at the internal mixing temperature of the pure raw material of the aromatic polyester to be processed until it is uniform;
[0018] 4) The material after the banburying in step 3) is crushed and then re-granulated to obtain an aromatic polyester modified composite material.
[0019] As a possible implementation, further, in step 2), the alkyl borate and the aminosiloxane are added separately to the pure aromatic polyester raw material, or the alkyl borate and the aminosiloxane are pre-mixed and then added to the pure aromatic polyester raw material.
[0020] As a possible implementation method, further, additives in an amount less than 3-5% can be added to the aromatic polyester raw material at one time for mixing, and the excess amount of additives needs to be added gradually in the subsequent mixing and kneading process.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0022] 1) The molecular chemical structure of the aromatic polyester material formula provided by the present invention does not contain aromatic hydrocarbon groups such as benzene rings, which fundamentally avoids the problems of radiation yellowing of traditional aromatic hydrocarbon anti-radiation agents and the volatility of olefin additives.
[0023] 2) The formula of the present invention has a high boiling point and low volatility, which can reduce air pollution during the processing process. At the same time, it can significantly alleviate the radiation curing brittleness of aromatic polyesters caused by excessive radiation self-crosslinking and benzene ring rigidity, and can maintain or even improve the mechanical rigidity and toughness of aromatic polyester materials under a radiation dose of several hundred kGy, taking into account the radiation resistance requirements of aromatic polyesters in terms of rigidity or toughness under high ionizing radiation dose scenarios, and has excellent industrial application prospects. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The present invention provides an additive, an aromatic polyester material resistant to ionizing radiation and a preparation method thereof, wherein the aromatic polyester material resistant to ionizing radiation comprises an additive suitable for an aromatic polyester anti-ionizing radiation formulation system and an aromatic polyester; wherein the aromatic polyester is any polycarboxylate containing a benzene ring functional group structure, such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polybutylene terephthalate adipate (PBAT) and other polyesters containing aromatic hydrocarbon structures.
[0026] Additives suitable for aromatic polyester anti-ionizing radiation formulation systems include alkyl borate and aminosiloxane. Among them, alkyl borate is a borate compound in which any side group contains only saturated alkyl groups and the alkyl carbon chain length is more than four carbon atoms, such as tributyl borate, tripentyl borate, etc.; aminosiloxane is an organic silicon compound in which any molecular chain is a fully saturated bond, and one end of the molecule contains an amine group and the other end contains an alkoxy silicon structure, such as 3-aminopropyl triethoxysilane, N-(2-aminoethyl)-3-aminopropyl trimethoxysilane, etc.
[0027] The above-mentioned additive compound molecules do not contain any aromatic structure or any unsaturated olefin units. According to the specific ingredients of the formula, the additive compound itself can withstand processing processes such as mixing or injection molding at a temperature range of about 300 degrees or below.
[0028] The preparation method of the aromatic polyester material resistant to ionizing radiation specifically comprises the following steps:
[0029] 1) The aromatic polyester raw material is first dried in a drying equipment such as a blast dryer at 60-90°C for 1-4 hours for use. If it is not used immediately after drying, the polyester raw material is sealed in a dry state at 30-40°C. If it is stored openly, it needs to be dried again before use;
[0030] 2) Add the additives in a weight percentage relative to the total feed, wherein the addition amount of alkyl borate is 0.1% to 10%, and the addition amount of aminosiloxane is 0.1% to 10%; mix the additives with the polyester pellets dried in the above step 1) and stir evenly. The alkyl borate and aminosiloxane can be added to the pure aromatic polyester raw material separately, or the alkyl borate and aminosiloxane can be mixed evenly in advance and then added to the pure aromatic polyester raw material. The additives less than about 3% to 5% can be mixed at one time, and the excess additives need to be added gradually during the subsequent mixing and kneading process.
[0031] 3) The mixed material in the above step 2) is put into a mixing equipment such as an internal mixer for internal mixing. The internal mixing temperature is set to the melting temperature of the aromatic pure raw material. The internal mixing time is 5 to 30 minutes, during which the remaining additives can be added successively.
[0032] 4) The raw materials after mixing are taken out and crushed by a plastic crusher and other equipment, and then re-granulated to obtain the final granular radiation-resistant composite material, which can be used as the masterbatch of various plastic products for anti-ionizing radiation purposes. It has good anti-ionizing radiation performance and can be used alone or blended with other plastics.
[0033] Example 1
[0034] Take 98% of PBAT (polybutylene terephthalate adipate) masterbatch (weight percentage relative to the total feed, the following percentages have the same meaning), dry it in a blast dryer at 80 degrees for 2 hours, cool it down to 30-40 degrees and take it out. Mix two additives: 1% tributyl borate and 1% 3-aminopropyl triethoxysilane with the dried PBAT masterbatch. Then put the mixture into a mixer and mix it at 150°C for 5-10 minutes. After the mixing is completed, take it out and put it into a plastic crusher for crushing. Put the crushed mixture into a twin-screw extruder for re-granulation. The temperature of each zone of the extruder is 130-180°C and the speed is 40-80r / min.
[0035] The radiation-resistant composite masterbatch finally obtained in this embodiment was injected into a dumbbell-shaped mechanical test sample to test the change of the formula on the radiation resistance of the polyester masterbatch. The test conditions were: the electron accelerator energy was 10 MeV, the temperature was room temperature (25°C), and the ambient atmosphere was exposed to ordinary air. The radiation resistance of the sample is as follows:
[0036] When the electron beam radiation dose increases from 0 kGy to 100 kGy, the tensile strength of the pure PBAT sample in the non-added group increases from about 22 MPa before irradiation to 23.5 MPa after irradiation (self-crosslinking by bulk radiation); but the tensile elongation at break decreases from about 700% before irradiation to about 630% after irradiation (radiation embrittlement); the tensile strength of the composite sample of the present embodiment increases from 24 MPa before irradiation to 27 MPa after irradiation, and the elongation at break increases from about 660% before irradiation to about 720% after irradiation (radiation toughening).
[0037] When the electron beam radiation dose increases from 0 kGy to 300 kGy, the tensile strength of the pure PBAT sample in the non-additive group increases from 22 MPa to 23 MPa (bulk radiation self-crosslinking), but the tensile elongation at break decreases from about 700% to about 560% (radiation embrittlement); the sample of the composite material of this embodiment increases from 24 MPa to about 27 MPa, and the elongation at break increases from about 660% to 680% (radiation toughening).
[0038] This compounding ratio achieves the goal of keeping the PBAT polyester material in this example within the range of high radiation doses below 300 kGy, while increasing the radiation-resistant rigidity (tensile strength) and toughness (elongation at break) of the sample.
[0039] Example 2
[0040] The preparation process of the radiation-resistant composite material is the same as that in Example 1, and PBAT polyester is still used as the main raw material, but the ratio is different. PBAT is taken at 98.9%, and the additive formula ratio is changed to: 3-aminopropyltriethoxysilane is added at 1%, and tributyl borate is added at 0.1%. The same electron beam irradiation conditions as in Example 1 are adopted.
[0041] When the electron beam radiation dose increases from 0kGy to 50kGy, the tensile strength of the composite sample with this ratio increases slightly from 24MPa to 25MPa, and the tensile elongation at break increases sharply from 660% to 750%.
[0042] When the electron beam radiation dose increases from 0 kGy to 100 kGy, the tensile strength of the composite sample with this ratio increases slightly from 24 MPa to 25.5 MPa, and the tensile elongation at break increases slightly from 660% to 670%;
[0043] When the electron beam radiation dose increases from 0 kGy to 300 kGy, the tensile strength of the composite sample with this ratio slightly decreases from 24 MPa to 23.5 MPa, and the tensile elongation at break slightly decreases from 660% to 645%;
[0044] The comprehensive radiation resistance performance of this ratio is not as good as that of Example 1 in the full radiation dose range, but it can significantly enhance the radiation toughness of the sample below a radiation dose of 50 kGy (the elongation at break after radiation is significantly improved) under the condition of less additive usage. At the same time, the radiation resistance rigidity of the composite polyester material remains basically unchanged within the high radiation dose range compared to the pure polyester material without additives, and the radiation embrittlement is significantly alleviated.
[0045] Example 3
[0046] The preparation process of the radiation-resistant composite material is the same as that in Example 1, and PBAT polyester is still used as the main masterbatch, but the ratio is different. PBAT is taken at 98.9%, and the additive formula ratio is changed to: 0.1% of 3-aminopropyltriethoxysilane is added, and 1% of tributyl borate is added. The same electron beam irradiation conditions as in Example 1 are adopted.
[0047] When the electron beam radiation dose increases from 0 kGy to 100 kGy, the tensile strength of the composite sample with this ratio remains unchanged at about 22 MPa, and the tensile elongation at break increases from 650% to 680%;
[0048] When the electron beam radiation dose increases from 0 kGy to 300 kGy, the tensile strength of the composite sample with this ratio increases from 22 MPa to 25.5 MPa, and the tensile elongation at break increases from 650% to 760%.
[0049] The main advantage of this compounding ratio is that it can simultaneously improve the radiation resistance rigidity and toughness of the composite sample within the range of high radiation doses above 100KGy, especially it can greatly improve the radiation resistance toughness (tensile elongation at break) of the composite sample under high radiation dose conditions.
[0050] In summary, for the two types of additives involved in the present invention, for the polyester masterbatch PBAT, the main function of alkyl borate is radiation toughening, and the main function of aminosiloxane is radiation enhancement. The focus of additive feeding can be adjusted for different aromatic polyester masterbatches according to actual needs.
[0051] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An additive, It is characterized in that The additive is suitable for a formulation system for aromatic polyester to resist ionizing radiation, and comprises alkyl borate and aminosiloxane.
2. The polyester raw material according to claim 1, It is characterized in that The aromatic polyester is a polycarboxylate having a benzene ring functional group structure in its molecular chain.
3. The additive according to claim 1, It is characterized in that The alkyl borate is a borate compound in which the side group contains only a straight-chain or branched saturated alkyl group, and the alkyl carbon chain contains four or more carbon atoms.
4. The additive according to claim 1, It is characterized in that The aminosiloxane is an organic silicon compound with a fully saturated bond in the molecular chain, an amino group at one end of the molecule and an alkoxy silicon structure at the other end.
5. An aromatic polyester material resistant to ionizing radiation, It is characterized in that The invention comprises an aromatic polyester and the additives according to claims 1 to 4.
6. The ionizing radiation-resistant aromatic polyester material according to claim 5, It is characterized in that The addition amount of the alkyl borate is 0.1% to 10% relative to the total weight of the raw materials; the addition amount of the aminosiloxane is 0.1% to 10% relative to the total weight of the raw materials.
7. The ionizing radiation-resistant aromatic polyester material according to claim 5, It is characterized in that The anti-ionizing radiation additive does not contain aromatic hydrocarbon structure or unsaturated olefin unit; the anti-ionizing radiation aromatic polyester and additive composite material can withstand processing temperature below 300 degrees.
8. A method for preparing the ionizing radiation resistant aromatic polyester material according to any one of claims 5 to 7, It is characterized in that The steps include: 1) Pre-drying the aromatic polyester raw material for standby use; 2) adding alkyl borate and aminosiloxane to the dried pure aromatic polyester raw material and stirring to mix well; 3) Add the mixed material to the melting equipment to be processed into 10000 pure raw materials of aromatic polyester Mix at the internal mixing temperature until uniform; 4) The material after the banburying in step 3) is crushed and then re-granulated to obtain an aromatic polyester modified composite material.
9. The method for preparing the ionizing radiation resistant aromatic polyester material according to claim 8, It is characterized in that In step 2), the alkyl borate and the aminosiloxane are added to the pure aromatic polyester raw material separately, or the alkyl borate and the aminosiloxane are pre-mixed and then added to the pure aromatic polyester raw material.
10. The method for preparing the ionizing radiation resistant aromatic polyester material according to claim 8, It is characterized in that Additives in an amount less than about 3-5% can be added to the aromatic polyester raw material at one time for mixing, and more additives need to be added in succession during the subsequent mixing and kneading process.