Electrolytic adhesive containing stable polymer and preparation method thereof

The stable polymer electrolytic adhesive prepared by graft copolymerization solves the problem that the existing electrolytic adhesive is prone to precipitation of anions and cations after voltage is applied, and better chemical and thermal stability is achieved, ensuring that The long-term effectiveness of electronic devices and are not prone to contamination.

CN118956301APending Publication Date: 2024-11-15ZHEJIANG ZHONGTE CHEM CO LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202411355094.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing electrolytic adhesive containing ionic liquids is prone to precipitation after voltage is applied, resulting in electrical corrosion, unstable adhesive properties and contamination of electronic devices.

Method used

The stable polymer electrolytic adhesive prepared by graft copolymerization method is introduced by copolymerizing acrylic monomers, ionic liquids and liquid crystal monomers, and anionic ions and liquid crystal monomers are added to form a network structure to increase heat. Stability and chemical stability.

Benefits of technology

It achieves better viscosity reduction effect after power-on and does not easily retain residual glue on the surface, enhances chemical stability and thermal stability, avoids the weakening of the energy-on viscosity reduction effect of ion precipitation, and ensures the long-term effectiveness and difficulty of electronic devices. pollute.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956301A_ABST
    Figure CN118956301A_ABST
Patent Text Reader

Abstract

The invention discloses an electrolytic adhesive containing a stable polymer and a preparation method thereof, and belongs to the technical field of electronic manufacturing, the electrolytic adhesive is prepared from the following raw materials in parts by weight: 1 part of a polymer, 0.01-0.15 part of a cross-linking agent and 0.0001-0.1 part of an anticorrosive agent; the polymer is obtained by direct block copolymerization of an acrylic monomer, an ionic liquid and a liquid crystal monomer and simultaneously contains anions, cations and the liquid crystal monomer; the electrolytic adhesive containing the stable polymer prepared by the invention has relatively large initial stripping force, relatively small stripping force after voltage is applied, and relatively good stability in a humid and hot environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic manufacturing, and in particular relates to an electrolytic adhesive containing a stable polymer and a preparation method thereof. Background Art

[0002] Acrylic adhesives are widely used in packaging, automobile manufacturing, electrical and other fields due to their good chemical resistance and excellent adhesion. Electronic devices need to be easily recycled, peeled off and protected during production, transportation and application, so ionic liquids with thermal stability and conductivity are widely used in the field of adhesive material technology.

[0003] When a certain voltage is applied to the electrolytic adhesive coating containing ionic liquid, anions and cations undergo redox reactions, the adhesive bonding force is weakened and it is easy to peel off. However, anions and cations in this type of electrolytic adhesive are easy to precipitate, which can easily cause problems such as electrical corrosion, unstable adhesive properties and contamination of electronic devices, thereby affecting the use and protection of electronic devices. Summary of the invention

[0004] To solve the above problems, the object of the present invention is to provide an electrolytic adhesive containing a stable polymer and a preparation method thereof.

[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions: An electrolytic adhesive containing a stable polymer, composed of the following raw materials, in parts by weight: 1 part of polymer, 0.01-0.15 parts of a cross-linking agent, and 0.0001-0.1 parts of an anticorrosive agent; The polymer is a polymer containing anionic, cationic and liquid crystal monomers obtained by direct block copolymerization of acrylic monomers, ionic liquids and liquid crystal monomers.

[0006] The cross-linking agent is toluene diisocyanate, diglycidyl aniline or polycarbodiimide resin.

[0007] The anticorrosive agent is polycarbodiimide resin, alkyl phosphate, benzotriazole derivative or triethylamine.

[0008] The polymer is prepared according to the following method: Under nitrogen protection, ionic liquid, acrylic acid, acrylic monomer and liquid crystal monomer are added to an organic solvent, stirred and dissolved, and then one-third of an oil-soluble azo initiator is added thereto, reacted at 80-90°C for 2-3 hours, cooled to 70-80°C, and continued to react for 2-3 hours to obtain a reaction liquid, and the remaining oil-soluble azo initiator is continued to be added to the obtained reaction liquid, reacted at 70-80°C for 5-8 hours, and then cooled to 25-30°C to obtain a polymer.

[0009] The mass ratio of the ionic liquid, acrylic acid, acrylic acid monomer, liquid crystal monomer, organic solvent and oil-soluble azo initiator is 1:0.5-1:5-10:0.1-0.5:10-20:0.0001-0.005.

[0010] The ionic liquid is 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium fluoromethanesulfonyl imide, 1-butyl-3-methylimidazolium dicyanamide, 1-hexyl-3-methylimidazolium bistrifluoromethanesulfonyl imide, 1-allyl-3-butylimidazolium bistrifluoromethanesulfonyl imide or 1-vinyl-3-butylimidazolium bistrifluoromethanesulfonyl imide.

[0011] The acrylic monomer is acrylamide, methyl acrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, lauryl acrylate, isobornyl acrylate, acrylonitrile, methyl methacrylate, pentaerythritol triacrylate, hydroxypropyl acrylate, 2-ethylhexyl acrylate or N,N-dimethylaniline.

[0012] The liquid crystal monomer is 4-cyanobiphenyl, 4,4-dihydroxybiphenyl, biphenyl diphenol, 4'-methyl-2-cyanobiphenyl, 4'-hexylbiphenyl-4-carbonitrile, 4'-heptylbiphenyl-4-carbonitrile or 4-(3-butenyloxy)benzoic acid 4-methoxyphenyl ester.

[0013] The organic solvent is ethyl acetate, n-butyl acetate, toluene, benzene, xylene, cyclohexane, dichloromethane, acetone, butanone or ether.

[0014] The oil-soluble azo initiator is azobisisobutyronitrile, azobisisoheptanenitrile or dimethyl 2,2'-azobisisobutyrate.

[0015] The method for preparing the electrolytic adhesive containing a stable polymer comprises the following steps: In parts by weight, 1 part of polymer, 0.01-0.15 parts of cross-linking agent and 0.0001-0.1 parts of anticorrosive agent are added into a reactor, stirred and mixed evenly to obtain an electrolytic adhesive containing a stable polymer.

[0016] Compared with the prior art, the present invention has the following advantages: The electrolytic adhesive containing a stable polymer of the present invention adopts a graft copolymerization method, and an acrylic monomer, an ionic liquid and a liquid crystal monomer undergo a copolymerization reaction at a certain temperature to obtain a polymer containing anions, cations and liquid crystal monomers at the same time. The introduction of anions and cations makes the polymer have more directional mobile charges, has a better viscosity reduction effect after power is applied, and is not easy to leave residual adhesive on the surface when peeled off; the introduction of liquid crystal monomers makes the polymer have stronger chemical stability, is more resistant to humid and hot environments and chemical corrosion, is not easy to seep out after long-term storage, and will not cause electrical corrosion to the adhered electronic devices, while avoiding the problem of weakening of the viscosity reduction effect of power application caused by ion precipitation after long-term storage.

[0017] The electrolytic adhesive containing a stable polymer of the present invention is prepared by adding a cross-linking agent, which can generate bridge bonds between polymer molecules to form a network structure, effectively improve the thermal stability of the electrolytic adhesive, and make it have a larger initial bonding force, so that the adhesive layer and the surface of the adherend are fully bonded; the acrylic acid monomer in the polymer promotes the cross-linking property, increases the cross-linking force and reduces the cohesive force, and can effectively inhibit the generation of residual adhesive when the adhesive layer on the surface of the adherend is peeled off, thereby reducing the pollution and electrical corrosion of the adhered surface of the electronic device. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is the structural formula of the polymer prepared in Example 1 of the present invention; Figure 2 is the structural formula of the polymer prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0019] In order to better understand the technical solution of the present invention, the above content of the present invention is further described in detail below through specific implementation methods in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above content of the present invention belong to the scope of the present invention.

[0020] Example 1 Preparation of polymer: Under nitrogen protection, 15 g of 1-vinyl-3-butylimidazole bis(trifluoromethanesulfonyl)imide salt, 7.5 g of acrylic acid, 75 g of isooctyl acrylate and 1.5 g of 4-(3-butenyloxy)benzoic acid 4-methoxyphenyl ester were added to 150 g of ethyl acetate, stirred and dissolved, and then 0.005 g of azobisisobutyronitrile was added thereto. The mixture was reacted at 80° C. for 2 h, cooled to 70° C., and continued to react for 2 h to obtain a reaction solution. 0.01 g of azobisisobutyronitrile was continued to be added to the obtained reaction solution. After reacting at 70° C. for 5 h, the mixture was cooled to 25° C. to obtain a polymer.

[0021] Preparation of electrolytic adhesive containing stabilizing polymer: 100 g of polymer, 1 g of polycarbodiimide resin and 0.01 g of triethylamine were added into a reactor, stirred and mixed evenly to obtain an electrolytic adhesive containing a stable polymer.

[0022] Example 2 Preparation of polymer: Under nitrogen protection, 15 g of 1-allyl-3-butylimidazole bistrifluoromethanesulfonyl imide salt, 9 g of acrylic acid, 100 g of isooctyl acrylate and 3 g of 4-(3-butenyloxy)benzoic acid 4-methoxyphenyl ester were added to 180 g of toluene, stirred and dissolved, and then 0.009 g of azobisisoheptanitrile was added thereto, and the mixture was reacted at 85° C. for 2.5 h, cooled to 75° C., and continued to react for 2.5 h to obtain a reaction solution, and 0.018 g of azobisisoheptanitrile was continued to be added to the obtained reaction solution, and the mixture was reacted at 75° C. for 6.5 h, and then cooled to 26° C. to obtain a polymer.

[0023] Preparation of electrolytic adhesive containing stabilizing polymer: 100 g of polymer, 5 g of diglycidyl aniline and 2.5 g of alkyl phosphate were added into a reactor and stirred to mix evenly to obtain an electrolytic adhesive containing a stable polymer.

[0024] Example 3 Preparation of polymer: Under nitrogen protection, 15 g of 1-ethyl-3-methylimidazolium fluoromethanesulfonyl imide salt, 11 g of acrylic acid, 105 g of lauryl acrylate and 4.5 g of 4,4-dihydroxybiphenyl were added to 230 g of acetone, stirred and dissolved, and then 0.01 g of dimethyl 2,2'-azobisisobutyrate was added thereto, reacted at 88°C for 2.7 h, cooled to 76°C, and continued to react for 2.4 h to obtain a reaction solution, and 0.02 g of dimethyl 2,2'-azobisisobutyrate was continued to be added to the obtained reaction solution, reacted at 75°C for 7 h, and then cooled to 28°C to obtain a polymer.

[0025] Preparation of electrolytic adhesive containing stabilizing polymer: 100 g of polymer, 10 g of toluene diisocyanate and 5 g of polycarbodiimide resin were added into a reactor, stirred and mixed evenly to obtain an electrolytic adhesive containing a stable polymer.

[0026] Example 4 Preparation of polymer: Under nitrogen protection, 15 g of 1-hexyl-3-methylimidazole bistrifluoromethanesulfonyl imide salt, 13.5 g of acrylic acid, 120 g of methyl methacrylate and 6 g of 4'-hexylbiphenyl-4-carbonitrile were added to 270 g of cyclohexane, stirred and dissolved, and then 0.02 g of 2,2'-azobisisobutyric acid dimethyl ester was added thereto, and the mixture was reacted at 85°C for 2 h, cooled to 75°C, and the reaction was continued for 2.5 h to obtain a reaction solution, and 0.04 g of 2,2'-azobisisobutyric acid dimethyl ester was continued to be added to the obtained reaction solution, and the mixture was reacted at 78°C for 7.5 h, and then cooled to 27°C to obtain a polymer.

[0027] Preparation of electrolytic adhesive containing stabilizing polymer: 100 g of the polymer, 12 g of toluene diisocyanate and 8 g of a benzotriazole derivative were added into a reactor, and stirred and mixed evenly to obtain an electrolytic adhesive containing a stable polymer.

[0028] Example 5 Preparation of polymer: Under nitrogen protection, 15 g of 1-ethyl-3-methylimidazolium tetrafluoroborate, 15 g of acrylic acid, 150 g of 2-ethylhexyl acrylate and 7.5 g of biphenyldiphenol were added to 300 g of xylene, stirred and dissolved, and then 0.025 g of azobisisobutyronitrile was added thereto, and the mixture was reacted at 90°C for 3 h, cooled to 80°C, and the reaction was continued for 3 h to obtain a reaction solution, and 0.05 g of azobisisobutyronitrile was continued to be added to the obtained reaction solution, and the mixture was reacted at 80°C for 8 h, and then cooled to 30°C to obtain a polymer.

[0029] Preparation of electrolytic adhesive containing stabilizing polymer: 100 g of polymer, 15 g of polycarbodiimide resin and 10 g of benzotriazole derivative were added into a reactor, stirred and mixed evenly to obtain an electrolytic adhesive containing a stable polymer.

[0030] 100 g of Y1410 (acrylic resin solution), 15 g of 1-vinyl-3-butylimidazole bis(trifluoromethanesulfonyl)imide salt, 1.5 g of 4-(3-butenyloxy)benzoic acid 4-methoxyphenyl ester, 1 g of polycarbodiimide resin and 0.01 g of triethylamine were added into a reactor, stirred and mixed evenly to obtain an electrolytic adhesive.

[0031] The electrolytic adhesive containing stable polymer prepared in Examples 1 to 5 and the electrolytic adhesive prepared in Comparative Example 1 were diluted with ethyl acetate to form an adhesive solution with a mass concentration of 50%, and then the adhesive solution was evenly coated on a polyester film to form a single-sided adhesive film with a thickness of 38 μm, and baked in an oven at 90°C for 5 minutes to prepare an electrolytic adhesive sample with a thickness of 30 μm. The obtained electrolytic adhesive sample was made into a sheet of 10 mm × 150 mm in size, and it was attached to the metal layer of a PET film with a metal layer to prepare an adhesive sheet.

[0032] The separator on the PET side of the adhesive sheet with a substrate was peeled off, and the adhesive sheet was attached to the center of the stainless steel plate as an adherend, and pressed back and forth with a roller three times. It was left at 23°C for 30 minutes to obtain a joint body comprising a stainless steel plate / electrically peelable adhesive sheet / film with a metal layer (electrically conductive substrate).

[0033] The obtained joint bodies were subjected to performance tests, including the measurement of ionic liquid leakage (normal temperature), initial peeling force before voltage application, peeling force after voltage application, and peeling force after voltage application after wet heat storage.

[0034] Determination of ionic liquid seepage (normal temperature): At normal temperature (24°C), apply a voltage of 10V to the adhesive layer of the obtained joint sample for 10 seconds and then peel it off. Rinse the surface of the stainless steel plate from which the adhesive layer has been peeled off with 1 mL of methanol to obtain a cleaning solution. Heat the cleaning solution to remove the methanol, and vacuum dry the residue at normal temperature for more than 48 hours. Dissolve the obtained solid component with an ACN:H2O (90:10) solution, and vortex stir for 2 to 3 minutes to completely dissolve the solid component. Filter the obtained solution through a 0.2μm PTFE filter. Analyze the filtrate using HPLC to measure the ionic liquid seepage (normal temperature) (mg / cm 2 ).

[0035] 180 。 Peeling force measurement: Peeling method: 180° peeling, peeling speed: 300 mm / min, peeling temperature: 23°C, applied voltage: 30 V, applied time: 15 s, wet heat storage conditions: 60°C, 90% RH, wet heat storage time: 500 h, peeling force reduction rate (%) = {1-(peeling force after voltage application / initial peeling force)}×100. The test results are shown in Table 1.

[0036] Table 1 Performance parameters of electrolytic adhesive

[0037] It can be seen from the results in Table 1 that the amount of ion liquid seepage of the electrolytic adhesive containing a stable polymer prepared by the present invention at room temperature is significantly less than the amount of ion seepage of the electrolytic adhesive prepared by conventional mixing and stirring in Comparative Example 1. The product prepared by the present invention has stability, a large initial bonding force and a small bonding force after power-on, and the bonding force of the applied voltage after wet heat storage can still be fully reduced. Compared with Comparative Example 1 in which the adhesive is prepared by mixing, the amount of ion seepage of the electrolytic adhesive containing a stable polymer of the present invention is stably lower than the amount of ion seepage in the comparative example. It can be seen that the electrolytic adhesive containing a stable polymer of the present invention has a high bonding force before applying a voltage and an ultra-low viscosity after applying a voltage, so that the target material can be firmly adhered to the substrate and easily peeled off after power-on, and no residual glue will be left on the surface of the adherend; anions and cations are not easy to seep out at room temperature, and the stability is strong, which ensures long-term effectiveness while not easily causing electrical corrosion to the adherend and polluting the adherend.

[0038] Although the above describes the specific implementation methods of the present invention, it does not limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.

Claims

1. An electrolytic adhesive containing a stable polymer, characterized in that: The composition is composed of the following raw materials in parts by weight: 1 part of polymer, 0.01-0.15 parts of cross-linking agent and 0.0001-0.1 parts of anticorrosive agent; The polymer is obtained by directly block copolymerizing acrylic monomers, ionic liquids and liquid crystal monomers, and contains anionic, cationic and liquid crystal monomers at the same time.

2. The electrolytic adhesive containing a stable polymer as claimed in claim 1, characterized in that: The cross-linking agent is toluene diisocyanate, diglycidyl aniline or polycarbodiimide resin.

3. The electrolytic adhesive containing a stable polymer as claimed in claim 1, characterized in that: The anticorrosive agent is polycarbodiimide resin, alkyl phosphate, benzotriazole derivative or triethylamine.

4. The electrolytic adhesive containing a stable polymer as claimed in claim 1, characterized in that: The polymer is prepared according to the following method: Under nitrogen protection, ionic liquid, acrylic acid, acrylic acid monomer and liquid crystal monomer are added to an organic solvent, stirred and dissolved, and then one-third of an oil-soluble azo initiator is added thereto, reacted at 80-90°C for 2-3 hours, cooled to 70-80°C, and continued to react for 2-3 hours to obtain a reaction liquid, and the remaining oil-soluble azo initiator is continued to be added to the obtained reaction liquid, reacted at 70-80°C for 5-8 hours, and then cooled to 25-30°C to obtain a polymer.

5. The electrolytic adhesive containing a stable polymer as claimed in claim 4, characterized in that: The mass ratio of the ionic liquid, acrylic acid, acrylic acid monomer, liquid crystal monomer, organic solvent and oil-soluble azo initiator is 1:0.5-1:5-10:0.1-0.5:10-20:0.0001-0.

005.

6. The electrolytic adhesive containing a stable polymer as claimed in claim 4, characterized in that: The ionic liquid is 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium fluoromethanesulfonyl imide, 1-butyl-3-methylimidazolium dicyanamide, 1-hexyl-3-methylimidazolium bistrifluoromethanesulfonyl imide, 1-allyl-3-butylimidazolium bistrifluoromethanesulfonyl imide or 1-vinyl-3-butylimidazolium bistrifluoromethanesulfonyl imide.

7. The electrolytic adhesive containing a stable polymer as claimed in claim 4, characterized in that: The acrylic monomer is acrylamide, methyl acrylate, ethyl acrylate, butyl acrylate, isooctyl acrylate, lauryl acrylate, isobornyl acrylate, acrylonitrile, methyl methacrylate, pentaerythritol triacrylate, hydroxypropyl acrylate, 2-ethylhexyl acrylate or N,N-dimethylaniline.

8. The electrolytic adhesive containing a stable polymer as claimed in claim 4, characterized in that: The liquid crystal monomer is 4-cyanobiphenyl, 4,4-dihydroxybiphenyl, biphenyl diphenol, 4'-methyl-2-cyanobiphenyl, 4'-hexylbiphenyl-4-carbonitrile, 4'-heptylbiphenyl-4-carbonitrile or 4-(3-butenyloxy)benzoic acid 4-methoxyphenyl ester.

9. The electrolytic adhesive containing a stable polymer as claimed in claim 4, characterized in that: The organic solvent is ethyl acetate, n-butyl acetate, toluene, benzene, xylene, cyclohexane, dichloromethane, acetone, butanone or ether; the oil-soluble azo initiator is azobisisobutyronitrile, azobisisoheptanenitrile or 2,2'-dimethyl azobisisobutyrate.

10. The method for preparing the electrolytic adhesive containing a stable polymer according to claim 1, characterized in that: The following steps are involved: In parts by weight, 1 part of polymer, 0.01-0.15 parts of cross-linking agent and 0.0001-0.1 parts of anticorrosive agent are added into a reactor, stirred and mixed evenly to obtain an electrolytic adhesive containing a stable polymer.

Citation Information

Cited By

  • Electroinduced viscosity-reducing glue as well as preparation method and application thereof

    CN119432236A

  • Reworkable thermal visbreaking foam tape and preparation method thereof

    CN119662151A

  • Electrolytic adhesive and adhesive tape and preparation method thereof

    CN119823677A

  • Block copolymer and preparation method thereof, electrolytic viscose and electrolytic viscose film

    CN122404719A

  • A block copolymer, a method for preparing the same, an electrolytic adhesive, and an electrolytic adhesive film