Tanshinone-reducing eucalyptus folic acid hydromagnesite composite material as well as preparation method and application thereof

Through the co-hybridization of nortanshinone and eucalyptol with hydromagnesite, the problem of hydromagnesite's poor dispersion and easy combustion in a low-polarity matrix is ​​solved, forming nortanshinone-eucalyptol with high mechanical and thermal stability. Hydromagnesite composite materials realize multiple functional and environmentally friendly industrial applications.

CN118725415APending Publication Date: 2024-10-01JIANGXI GUANGYUAN CHEM +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964463.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the application of traditional natural hydromagnesite, there are excessive surface polarities, easy moisture absorption, agglomeration, and stress defects caused by agglomeration. In addition, traditional surface modifiers are costly, complicated to prepare, difficult to degrade, and are dispersed in low-polarity matrices. Polyolefin elastomers have poor performance and are easy to burn.

Method used

Nortanshinone and eucalyptol are co-hybridized with hydromagnesite, and through modification and dispersion, a nortanshinone-eucalyptol hydromagnesite composite material is formed, which reduces the surface polarity of hydromagnesite and improves its dispersion and functionality.

Benefits of technology

Significantly reduces oil absorption value, improves mechanical and thermal stability, reduces dielectric loss, forms a core-shell structure, is suitable for large-scale industrial production, enhances flame retardant properties, and improves the application of natural products in industrial materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725415A_ABST
    Figure CN118725415A_ABST
Patent Text Reader

Abstract

The invention provides a tanshinone-reducing eucalyptus folic acid hydromagnesite composite material as well as a preparation method and application thereof, and belongs to the technical field of natural product reconstruction. The preparation method comprises the following steps: combining a natural product eucalyptus folic acid with natural hydromagnesite powder to obtain eucalyptus folic acid hydromagnesite, and then co-hybridizing the natural product nortanshinone and the eucalyptus folic acid hydromagnesite to obtain the hydromagnesite composite material jointly modified by the nortanshinone and the eucalyptus folic acid. Wherein the natural product nortanshinone contains a large number of aromatic rings and heterocyclic rings and belongs to a typical large conjugated structure, hydroxyl groups on a molecular structure of the natural product eucalyptus folic acid are shielded by methyl groups, the whole structure shows relatively low polarity and aromaticity, and the natural product nortanshinone and the eucalyptus folic acid are mutually complementary and jointly modified in structure, so that the natural product nortanshinone has a relatively high activity. Hydroxyl groups on the surface of natural hydromagnesite can be greatly shielded, the surface polarity of the hydromagnesite is reduced, the comprehensive performance of the hydromagnesite is effectively improved, and the defects of traditional silane in the aspects of functionality, cost performance, production and preparation processes, difficulty in degradation and the like are effectively overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of natural product reconstruction, and in particular to a nortanshinone-eucalyptol hydromagnesite composite material and a preparation method and application thereof. Background Art

[0002] The reconstruction of all-natural products is a typical form of functional material construction. In particular, the use of sustainably renewable natural products for functional organic combination is a key proposition of long-term evolution. The reconstruction of natural products can effectively enhance the functionality of the final product and is also one of the efficient means to effectively reduce carbon emissions. Natural hydromagnesite is a typical mineral of traditional natural inorganic mineral powder. It is widely used in strengthening organic polymer materials. However, it has major performance defects, especially excessive surface polarity, high hydroxyl content, easy moisture absorption and agglomeration during subsequent storage, and easy agglomeration during actual use, causing stress defects. Traditional synthetic surface modifiers are not only costly and complicated in preparation, but also difficult to degrade after failure, have single functions, and have limited enhancement effects. Solutions are urgently needed. Summary of the invention

[0003] The object of the present invention is to provide a nortanshinone-based eucalyptol hydromagnesite composite material and a preparation method and application thereof. The composite material not only has a good core-shell structure, a low oil absorption value, and a high renewability, but also can well promote carbonization, mechanical enhancement, improve thermal stability, and reduce dielectric loss, so as to solve the problem that polyolefin elastomer alloys are easy to burn and natural mineral powders have poor dispersibility in a low-polarity (or non-polar) matrix.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing a nortanshinone-eucalyptol hydromagnesite composite material, comprising the following steps:

[0006] The eucalyptol acid, hydromagnesite and the first solvent are mixed and modified to obtain eucalyptol acidified hydromagnesite;

[0007] The eucalyptol hydromagnesite is mixed with a dispersant to disperse the mixture, thereby obtaining a eucalyptol hydromagnesite dispersion;

[0008] mixing nortanshinone with a second solvent to obtain a nortanshinone solution;

[0009] The eucalyptol acidified hydromagnesite dispersion is mixed with a nortanshinone solution for hybridization to obtain a nortanshinone-based eucalyptol acidified hydromagnesite composite material.

[0010] Preferably, the median particle size D of the hydromagnesite is 50The particle size is 1.0-4.8 μm; the dosage ratio of eucalyptus acid to hydromagnesite is 0.1-5.0 mol:10 kg.

[0011] Preferably, the first solvent includes one of ethanol, methanol, ethylene glycol, N,N-dimethylformamide, ethyl acetate and propanol.

[0012] Preferably, the modification includes a first reaction and a second reaction performed sequentially, wherein the temperature of the first reaction is 90-130°C, the time is 0.2-3.5h, and the stirring rate is 500-1600r / min; the temperature of the second reaction is 1-10°C, the time is 0.1-2.0h, and the stirring rate is 300-1000r / min.

[0013] Preferably, the dispersant is a mixture of a first alcohol and water, the first alcohol is one or more of methanol, ethanol, propanol, 1,2-propylene glycol, isopropanol, ethylene glycol and 1,3-propylene glycol, and the volume ratio of the first alcohol to water is 1:1 to 100;

[0014] The dispersion rate is 800-2000 rpm, the time is 0.2-3.6 hours, and the concentration of the eucalyptol hydromagnesite dispersion is 1-20M.

[0015] Preferably, the second solvent is a mixed solution of a second alcohol and water, the second alcohol is one or more of methanol, ethanol, propanol, 1,2-propylene glycol, isopropanol, ethylene glycol and 1,3-propylene glycol, and the volume ratio of the second alcohol to water is 1 to 50:1;

[0016] The temperature of mixing the nortanshinone and the second solvent is 40-60° C.; the concentration of the nortanshinone solution is 1-10M.

[0017] Preferably, the usage ratio of nortanshinone to eucalyptol hydromagnesite is 1-5 mol:10 kg.

[0018] Preferably, the hybridization temperature is 50-99° C. and the time is 0.5-6.5 h.

[0019] The present invention provides a nortanshinone-based eucalyptol hydromagnesite composite material prepared by the preparation method described in the above technical scheme.

[0020] The present invention provides application of the nortanshinone-eucalyptol hydromagnesite composite material described in the above technical solution in a thermoplastic elastomer alloy masterbatch.

[0021] The present invention provides a method for preparing a composite material of nortanshinone-eucalyptol hydromagnesite, wherein the natural product eucalyptol and natural hydromagnesite powder are first combined to form eucalyptol hydromagnesite, and then the natural product nortanshinone and eucalyptol hydromagnesite are co-hybridized to obtain a composite material of hydromagnesite co-modified with nortanshinone and eucalyptol. Among them, the natural product nortanshinone contains a large number of aromatic rings and heterocycles, and belongs to a typical large conjugated structure. The natural product eucalyptol, the hydroxyl groups on its molecular structure have been shielded by methyl groups, and the overall structure presents lower polarity and aromaticity. Through the mutual complementation and co-modification of the two in structure, the hydroxyl groups on the surface of natural hydromagnesite can be greatly shielded, and its surface polarity can be reduced, and its comprehensive performance can be effectively improved, and the defects of traditional silane in functionality, cost performance, production and preparation process, and non-degradability can be effectively compensated.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) In terms of powder modification, the present invention provides a composite material of nortanshinone-eucalyptol hydromagnesite, wherein eucalyptol is an important plant extract and drug intermediate, which is widely present in eucalyptus, has a wide source and is renewable. Another type of nortanshinone belongs to a natural flavonoid product (extracted from the Chinese herbal medicine Salvia miltiorrhiza), is a colorless crystalline powder, has important applications in the field of biomedicine (anti-oxidation, anti-inflammatory, etc.), is typically green and environmentally friendly, has a wide source and is degradable. The two are successively combined with natural hydromagnesite to form a coating layer, which is a typical reconstruction of natural products and natural mineral powders, and can significantly reduce the surface energy of natural mineral powders, which is reflected in the significant improvement in oil absorption value, surface polarity and contact angle. At the same time, it can give the composite material multiple functionalities, which is in line with the current concept of low-carbon, environmentally friendly and sustainable development. The present invention is expected to enhance the depth and breadth of application of natural products in the upgrading and modification of the surface performance of traditional industrial powders through simple and efficient reconstruction of natural products, enhance their application value, and modify natural inorganic mineral powders in a targeted manner.

[0024] (2) In terms of functionality, the natural hydromagnesite mineral in the prepared nortanshinone-based eucalyptol hydromagnesite composite material has good flame retardant and smoke suppression properties. The surface is modified and hybridized with eucalyptol and nortanshinone. Both contain aromatic rings, especially nortanshinone contains large conjugated aromatic rings and polycyclic heterocycles. During the combustion process, it can quickly form carbon and attach to the MgO ceramic precursor product to form a reinforced physical barrier layer that can resist heat flow, mass flow, and air flow, effectively fixing the molecular chain fragments in the condensed phase, thereby significantly increasing the amount of residual carbon. In addition, eucalyptol and nortanshinone are beneficial to improving the quality of residual carbon (promoting the formation of crystalline carbon layer). , because eucalyptol and nortanshinone are both low-polarity aromatic compounds, they can effectively reduce the surface polarity of natural hydromagnesite, thereby achieving effective dispersion in low-polarity or non-polar thermoplastic elastomer alloys, and are not prone to stress defects, effectively enhancing the mechanical properties of thermoplastic elastomers. The composite material can act as a physical entanglement point in the polymer matrix, effectively inhibiting the slip and rotation of the molecular chain and enhancing its thermal stability. In addition, because the composite material is better filled and fills the gaps between the molecular chains, it can effectively reduce the energy consumption of the dielectric in the process of converting electrical energy to thermal energy per unit time, that is, the dielectric loss tangent angle tanδ decreases significantly, reducing heat loss;

[0025] (3) In terms of actual production and application, the surface energy of the nortanshinone-eucalyptol hydromagnesite composite material prepared by the present invention is low, the oil absorption value is significantly reduced, and the adsorption effect on processing is greatly reduced, which is conducive to reducing the subsequent processing cost. A core-shell structure composite material composed of organic functional molecules and inorganic mineral powders can be obtained through a simple two-step method. The preparation process is simple and easy, the process is green and environmentally friendly, and there is no complicated process. The raw materials are widely available and are all industrial grade, suitable for large-scale industrial production, and have great application potential. The composite material product is white or off-white, which will not cause trouble to the coloring of the matrix. The obtained composite material can greatly promote the application of natural products in industrial materials, and can better optimize the surface structure of traditional inorganic mineral powders and expand the scope of application. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The schematic diagram of the process for preparing the nortanshinone-based eucalyptol hydromagnesite composite material of the present invention;

[0027] Figure 2 This is a particle size distribution diagram of the nortanshinone-eucalyptol hydromagnesite composite material Nts-Ea-HM prepared in Example 1;

[0028] Figure 3 This is the SEM image of the nortanshinone-eucalyptol hydromagnesite composite material Nts-Ea-HM prepared in Example 1. DETAILED DESCRIPTION

[0029] like Figure 1 As shown, the present invention provides a method for preparing a nortanshinone-based eucalyptol hydromagnesite composite material, comprising the following steps:

[0030] The eucalyptol acid, hydromagnesite and the first solvent are mixed and modified to obtain eucalyptol acidified hydromagnesite;

[0031] The eucalyptol hydromagnesite is mixed with a dispersant to disperse the mixture, thereby obtaining a eucalyptol hydromagnesite dispersion;

[0032] mixing nortanshinone with a second solvent to obtain a nortanshinone solution;

[0033] The eucalyptol acidified hydromagnesite dispersion is mixed with a nortanshinone solution for hybridization to obtain a nortanshinone-based eucalyptol acidified hydromagnesite composite material.

[0034] In the present invention, unless otherwise specified, the required raw materials or reagents are commercially available products well known to those skilled in the art.

[0035] The invention mixes eucalyptol, hydromagnesite and a first solvent, performs modification, and obtains eucalyptol acidified hydromagnesite.

[0036] In the present invention, eucalyptol and nortanshinone are both commercially available products.

[0037] In the present invention, the eucalyptol (3,4,5-trimethoxybenzoic acid) is a natural benzoic acid product derived from eucalyptus extract, and its chemical structure is shown in Formula I, and its molecular formula is C 10 H 12 O 5 , the relative molecular mass is 212.20;

[0038]

[0039] In the present invention, the median particle size D of the hydromagnesite is 50 Preferably, it is 1.0-4.8 μm, more preferably 2.3 μm; the usage ratio of eucalyptus acid to hydromagnesite is preferably 0.1-5.0 mol:10 kg, more preferably 1-2 mol:10 kg.

[0040] In the present invention, the first solvent preferably includes one of ethanol, methanol, ethylene glycol, N,N-dimethylformamide, ethyl acetate and propanol.

[0041] The present invention preferably dissolves eucalyptus acid in a first solvent, performs a first mixing, and obtains a eucalyptus acid solution; places hydromagnesite in a high-speed stirrer, performs high-speed stirring, adds the eucalyptus acid solution to the hydromagnesite powder, heats the high-speed stirrer to perform a first reaction, cools to room temperature after completion, and then cools down to perform a second reaction.

[0042] In the present invention, the first mixing time is preferably 0.5 to 8.5 h, more preferably 3 to 5.5 h, the stirring rate is preferably 100 to 1200 rpm, more preferably 600 to 800 rpm, the temperature is preferably room temperature (25° C.), and the concentration of the eucalyptus acid solution is preferably 1 to 20 M, more preferably 1 to 10 M.

[0043] In the present invention, the stirring rate of the high-speed stirring is preferably 100-900 r / min, more preferably 500-800 r / min, and the temperature of the hydromagnesite is preferably 40-80°C, more preferably 50-60°C.

[0044] Before adding the eucalyptus acid solution, the eucalyptus acid solution is preferably heated to 35-70°C, more preferably 50-60°C. The adding method is preferably spraying, and the spraying rate is preferably 1-100 mL / min, more preferably 50-80 mL / min.

[0045] In the present invention, the modification includes a first reaction and a second reaction carried out sequentially, wherein the temperature of the first reaction is 90-130°C, more preferably 100-110°C, the time is 0.2-3.5h, more preferably 1.0-2.0h, and the stirring rate is 500-1600r / min, more preferably 800-1200r / min; the temperature of the second reaction is 1-10°C, more preferably 5-8°C, the time is 0.1-2.0h, more preferably 1-1.5h, and the stirring rate is 300-1000r / min, more preferably 600-800r / min.

[0046] After completing the modification, the present invention preferably removes dust and dries the obtained product in sequence to obtain eucalyptol hydromagnesite; the dust removal is preferably placing the reaction product in a cyclone separator with a power of 100 to 800 W, more preferably 400 to 600 W, a rotation speed of 500 to 1800 r / min, more preferably 600 to 1000 r / min, and an air inlet rate of 8 to 16 m / s, more preferably 10 to 12 m / s; the drying method is preferably static drying, the drying temperature is preferably 80 to 120 ° C, more preferably 90 to 100 ° C, the time is preferably 10 to 72 h, more preferably 24 to 42 h, and the power is preferably 800 to 2200 W, more preferably 1000 to 1500 W.

[0047] The invention mixes the eucalyptol hydromagnesite with a dispersant and disperses the mixture to obtain a eucalyptol hydromagnesite dispersion.

[0048] In the present invention, the dispersant is preferably a mixture of a first alcohol and water, and the first alcohol is preferably one or more of methanol, ethanol, propanol, 1,2-propylene glycol, isopropanol, ethylene glycol and 1,3-propylene glycol. When the first alcohol is two or more of the above alcohols, they are preferably mixed in equal volumes; the volume ratio of the first alcohol to water is preferably 1:1-100, more preferably 1:20-50.

[0049] In the present invention, the dispersion rate is preferably 800-2000 rpm, more preferably 1000-1500 rpm, the time is preferably 0.2-3.6 h, more preferably 1.8-3.0 h, and the concentration of the eucalyptol hydromagnesite dispersion is preferably 1-20 M, more preferably 1-15 M, and further preferably 10 M.

[0050] The present invention mixes nortanshinone with a second solvent to obtain a nortanshinone solution; and mixes the eucalyptol acidified hydromagnesite dispersion with the nortanshinone solution for hybridization to obtain a nortanshinone-based eucalyptol acidified hydromagnesite composite material.

[0051] The nortanshinone used in the present invention is a salvia miltiorrhiza extract with an aromatic ring / aromatic heterocycle, the structure of which is shown in Formula II, and the molecular formula is C 17 H 12 O 4 , the relative molecular mass is 280.27.

[0052]

[0053] In the present invention, the second solvent is preferably a mixed solution of a second alcohol and water, and the second alcohol is preferably one or more of methanol, ethanol, propanol, 1,2-propylene glycol, isopropanol, ethylene glycol and 1,3-propylene glycol. When the second alcohol is two or more of the above alcohols, they are preferably mixed in equal volumes; the volume ratio of the second alcohol to water is preferably 1 to 50:1, more preferably 20 to 30:1.

[0054] In the present invention, the temperature of mixing the nortanshinone and the second solvent is 40-60°C, more preferably 45-55°C, and further preferably 50°C, the time is preferably 0.5-6.0h, more preferably 1-3h, the ultrasonic power is preferably 5-80kHz, more preferably 40-60kHz, the stirring mode of mixing is preferably dissolving while mechanically stirring, and the mechanical stirring rate is preferably 600-1800rpm, more preferably 800-1000rpm; the concentration of the nortanshinone solution is preferably 1-10M, more preferably 3-5M.

[0055] In the present invention, the usage ratio of nortanshinone to eucalyptol hydromagnesite is preferably 1-5 mol:10 kg, more preferably 2-3 mol:10 kg.

[0056] When the molar mass ratio of tanshinone to eucalyptol hydromagnesite is lower than 1 mol:10kg, the amount of tanshinone agglomerated on the surface of natural hydromagnesite powder may be limited, making it difficult to further modify and shield the natural hydromagnesite powder, and the polarity of the natural hydromagnesite powder may be difficult to further decrease, resulting in limited degradation of the overall performance. When the molar mass ratio of tanshinone to eucalyptol hydromagnesite is higher than 5 mol:10kg, tanshinone may be over-enriched on the surface of natural hydromagnesite, loosely stacked, or even multiple powder particles may be wrapped together, resulting in peeling due to friction between molecular chains during processing, thereby affecting the overall performance of the composite material.

[0057] The present invention preferably heats the temperature to the hybridization temperature, adds the nortanshinone solution to the eucalyptol hydromagnesite dispersion during the heating process, and after the addition is completed, continues stirring for hybridization; the heating rate is preferably 1°C / min to 10°C / h; the addition rate is preferably 1 drop / 3s to 6 drops / s, more preferably 2 drops / s.

[0058] In the present invention, the hybridization temperature is 50-99° C., more preferably 71° C., the time is 0.5-6.5 h, more preferably 3.5 h, and the stirring rate is preferably 300-1200 rpm, more preferably 900 rpm.

[0059] During the hybridization process, nortanshinone is accumulated on the surface of eucalyptol hydromagnesite through the physical electrostatic adsorption effect, forming a secondary coating on the hydromagnesite.

[0060] After the hybridization is completed, the present invention preferably performs suction filtration, centrifugal washing, flash drying and low-temperature cooling in sequence to obtain a nortanshinone-eucalyptol hydromagnesite composite material (Nts-Ea-HM).

[0061] In the present invention, the suction filtration is preferably to place the reaction product under -0.09MPa to -0.08MPa (more preferably -0.085MPa) for suction filtration, the filter paper is a slow filter paper, the number of layers is 1 to 3, the suction filtration power is 100 to 1000W, more preferably 500W, and a mixed solution of alcohol and purified water is used for washing during the suction filtration process. The type of alcohol is the same as the first alcohol, and the volume ratio of alcohol to purified water is 1:1 to 20, more preferably 1:10, and the suction filtration is repeated 1 to 5 times; the centrifugation is preferably to place the composite material obtained by suction filtration in a centrifuge tube for centrifugal washing, and the reagent used for centrifugation is preferably a mixture of alcohol and purified water. The alcohol is preferably methanol or ethanol, the volume ratio of the alcohol to purified water is 1:1-90, more preferably 1:40, the solid content is 50-500 g / L, more preferably 200 g / L, the centrifugal speed is 3000-12000 rpm, more preferably 8000 rpm, the centrifugal time is 0.1-1.2 h, more preferably 0.6 h, and the centrifugal temperature is preferably 5-15 ° C, more preferably 10 ° C; the flash drying temperature is 100-150 ° C, more preferably 130 ° C, the drying time is 0.1-0.8 h, more preferably 0.4 h, and the drying air volume is 300-1000 m 3 / h, more preferably 600m 3 / h; the low-temperature cooling is preferably placing the powder obtained by flash drying in a high-speed stirrer for rotation cooling, the stirring temperature is 1-10°C, more preferably 5°C, the stirring rate is 300-1200rpm, more preferably 900rpm, and the stirring time is 0.5-12h, more preferably 6h.

[0062] The present invention provides a nortanshinone-based eucalyptol hydromagnesite composite material prepared by the preparation method described in the above technical scheme.

[0063] The median particle size (D 50 ) is 1.0 to 5.0 μm, and more preferably 2.5 μm.

[0064] The present invention provides an application of the nortanshinone-based eucalyptol hydromagnesite composite material described in the above technical solution in a thermoplastic elastomer alloy masterbatch; the thermoplastic elastomer alloy is preferably LDPE / TPE. The nortanshinone-based eucalyptol hydromagnesite composite material provided by the present invention can be used as a functional filler in a thermoplastic elastomer masterbatch, which can not only promote the carbonization of the elastomer alloy, provide flame retardancy and smoke suppression, but also improve thermal stability and reduce dielectric loss, and in addition, can effectively improve mechanical strength.

[0065] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0066] Example 1

[0067] (1) Dissolve 212.2 g of eucalyptus acid in ethanol and stir for 5.5 h at a stirring rate of 600 rpm and a stirring temperature of room temperature (25° C.) to obtain a solution 1, wherein the concentration of the solution 1 is controlled to be 10 M;

[0068] (2) 10 kg of natural hydromagnesite (median particle size D 50 2.3 μm) was placed in a high-speed stirrer at a stirring rate of 500 r / min and a powder temperature of 60°C. The temperature of solution 1 was raised to 50°C and added to the natural hydromagnesite powder by spraying, and the spraying rate was controlled to be 50 mL / min. The amount ratio of eucalyptus acid to natural hydromagnesite was 1 mol: 10 kg. After the addition was completed, the temperature was raised to 110°C and the stirring rate was controlled to be 1200 r / min. The mixture was mixed for 2.0 h. After the mixture was cooled to room temperature, the mixture was stirred at a low temperature (5°C) for 1.0 h and a stirring rate of 600 r / min. The obtained product was placed in a cyclone separator for dust removal at a power of 400 W, a rotation speed of 1000 r / min and an air inlet rate of 12 m / s. The mixture was then allowed to stand and dried at a drying temperature of 100°C, a drying time of 42 h and a drying power of 1500 W to obtain eucalyptus acidified hydromagnesite.

[0069] (3) 840.9 g of nortanshinone was dissolved in a mixed solution of ethanol and purified water, wherein the volume ratio of ethanol to purified water was 20:1, and the solution was dissolved while being mechanically stirred at a mechanical stirring rate of 1000 rpm, a stirring time of 3.0 h, an ultrasonic power of 40 kHz, and a temperature of 50° C. to obtain a solution 2, and the concentration of the solution 2 was controlled to be 3 M;

[0070] (4) 10 kg of the obtained eucalyptus acidified hydromagnesite was stirred and dispersed in a mixed solution of ethanol and purified water, wherein the volume ratio of ethanol to purified water was 1:50, the dispersion rate was 1000 rpm, and the dispersion time was 1.8 h to obtain dispersion 3, the concentration of dispersion 3 was controlled to be 10 M, and the temperature was raised to 71° C. at a heating rate of 30° C. / h. During the heating process, solution 2 was added dropwise to dispersion 3 at a dropping rate of 2 drops / s until the dropping was completed, and stirring was continued for 3.5 h, and the stirring rate was controlled to 900 rpm. The product after the reaction was completed was placed at -0.085 MPa for suction filtration. The filter paper is slow filter paper with 2 layers and the filtration power is 500W. During the filtration process, a mixed solution of ethanol and purified water is used for washing. The volume ratio of ethanol to purified water is 1:10. The filtration is repeated 3 times. The product obtained by filtration is placed in a centrifuge tube for centrifugal washing. The reagent used for centrifugation is a mixed solution of ethanol and purified water. The volume ratio of ethanol to purified water is 1:40, the solid content is 200g / L, the centrifugal speed is 8000rpm, the centrifugal time is 0.6h, and the centrifugal temperature is 10℃. Then flash drying is carried out at a temperature of 130℃, a drying time of 0.4h, and a drying air volume of 600m 3 / h; the powder obtained by flash drying was placed in a high-speed mixer for rotation cooling, the stirring temperature was 5°C, the stirring rate was 900rpm, and the stirring time was 6h to obtain a nortanshinone-based eucalyptol hydromagnesite composite material (Nts-Ea-HM, median particle size (D 50 ) is 2.5 μm), wherein the dosage ratio of nortanshinone to eucalyptol hydromagnesite is 3 mol:10 kg.

[0071] Example 2

[0072] (1) Dissolve 21.2 g of eucalyptus acid in ethylene glycol, stir for 0.5 h, at a stirring rate of 1200 rpm, at a stirring temperature of room temperature (25° C.), to obtain solution 1, wherein the concentration of solution 1 is controlled to be 1 M;

[0073] (2) 10 kg of natural hydromagnesite (median particle size D 502.3 μm) was placed in a high-speed stirrer at a stirring rate of 100 r / min, and the powder temperature was controlled at 40°C. The temperature of solution 1 was raised to 35°C, and added to the natural hydromagnesite powder by spraying, and the spraying rate was controlled to be 1 mL / min. The amount ratio of eucalyptus acid to natural hydromagnesite was 0.1 mol: 10 kg. After the addition was completed, the temperature was raised to 90°C, the stirring rate was controlled to 500 r / min, and mixed for 3.5 h. After the addition was completed, the mixture was cooled to room temperature, and then stirred at a low temperature (1°C) for 0.1 h, and the stirring rate was 300 r / min. The obtained product was placed in a cyclone separator for dust removal, with a power of 100 W, a rotation speed of 500 r / min, and an air inlet rate of 8 m / s, and then dried at a drying temperature of 80°C, a drying time of 72 h, and a drying power of 800 W to obtain eucalyptus acidified hydromagnesite;

[0074] (3) dissolving 280.3 g of nortanshinone in a mixed solution of ethylene glycol and purified water, wherein the volume ratio of ethylene glycol to purified water is 1:1, dissolving while mechanically stirring, the mechanical stirring rate is 600 rpm, the stirring time is 6.0 h, the ultrasonic power is 5 kHz, the temperature is 40° C., to obtain solution 2, and the concentration of solution 2 is controlled to be 1 M;

[0075] (4) 10 kg of the obtained eucalyptus acidified hydromagnesite was stirred and dispersed in a mixture of ethylene glycol and purified water, wherein the volume ratio of ethylene glycol to purified water was 1:1, the dispersion rate was 800 rpm, and the dispersion time was 3.6 h to obtain dispersion 3, and the concentration of dispersion 3 was controlled to be 1 M. The temperature was then raised to 50° C. at a heating rate of 10° C. / h. During the heating process, solution 2 was added dropwise to dispersion 3 at a dropping rate of 1 drop / 3 s until the dropping was completed, and stirring was continued for 0.5 h, and the stirring rate was controlled to be 1200 rpm. After the reaction was completed, the product was placed under -0.08 MPa for 3 hours. Filtration, the filter paper is slow filter paper, the number of layers is 1, the filtration power is 100W, and a mixed solution of ethylene glycol and purified water is used for washing during the filtration process. The volume ratio of ethylene glycol to purified water is 1:1, and the filtration is repeated once; the product obtained by filtration is placed in a centrifuge tube for centrifugal washing, the reagent used is a mixed solution of ethanol and purified water, the volume ratio of ethanol solution to purified water is 1:1, the solid content is 50g / L, the centrifugal speed is 3000rpm, the centrifugal time is 1.2h, and the centrifugal temperature is 5℃; then flash drying is performed at a temperature of 100℃, a drying time of 0.8h, and a drying air volume of 300m 3 / h; the powder obtained by flash drying was placed in a high-speed mixer for rotation cooling, the stirring temperature was 1°C, the stirring rate was 300rpm, and the stirring time was 12h to obtain the nortanshinone-based eucalyptol hydromagnesite composite material Nts-Ea-HM (median particle size (D 50) is 2.5 μm), wherein the dosage ratio of nortanshinone to eucalyptol hydromagnesite is 1 mol:10 kg.

[0076] Example 3

[0077] (1) 1.06 kg of eucalyptus acid was dissolved in methanol and stirred for 8.5 h at a stirring rate of 100 rpm and a stirring temperature of room temperature (25° C.) to obtain solution 1, wherein the concentration of solution 1 was controlled to be 20 M;

[0078] (2) 10 kg of natural hydromagnesite (median particle size D 50 2.3 μm) was placed in a high-speed stirrer, the stirring rate was 900 r / min, the powder temperature was controlled to 80°C, the temperature of solution 1 was raised to 70°C, and it was added to the natural hydromagnesite powder by spraying, and the spraying rate was controlled to be 100 mL / min, wherein the amount ratio of eucalyptus acid to natural hydromagnesite was 5 mol: 10 kg, after the addition was completed, the temperature was raised to 130°C, the stirring rate was controlled to be 1600 r / min, and mixed for 0.2 h, and then cooled to room temperature, and then stirred at a low temperature (10°C) for 2.0 h, the stirring rate was 1000 r / min, and the obtained product was placed in a cyclone separator for dust removal, the power was 800 W, the speed was 1800 r / min, the air inlet rate was 16 m / s, and then it was left to dry, the drying temperature was 120°C, the drying time was 10 h, and the drying power was 2200 W, to obtain eucalyptus acidified hydromagnesite;

[0079] (3) dissolving 1.4 kg of nortanshinone in a mixed solution of methanol and purified water, wherein the volume ratio of methanol to purified water is 50:1, dissolving while mechanically stirring, the mechanical stirring rate is 1800 rpm, the stirring time is 0.5 h, the ultrasonic power is 80 kHz, the temperature is 50° C., to obtain solution 2, and the concentration of solution 2 is controlled to be 5 M;

[0080] (4) 10 kg of the obtained eucalyptus acidified hydromagnesite was stirred and dispersed in a mixture of ethanol and purified water, wherein the volume ratio of ethanol to purified water was 1:100, the dispersion rate was 2000 rpm, and the dispersion time was 0.2 h to obtain dispersion 3, and the concentration of dispersion 3 was controlled to be 20 M. Then, the temperature was raised to 99° C. at a heating rate of 1° C. / min. During the heating process, solution 2 was added dropwise to dispersion 3 at a dropping rate of 6 drops / s until the dropping was completed. Stirring was continued for 6.5 h, and the stirring rate was controlled to 300 rpm. The product after the reaction was placed under -0.09 MPa for Filtration, the filter paper is slow filter paper, the number of layers is 3, the filtration power is 1000W, and the mixed solution of methanol and purified water is used for washing during the filtration process. The volume ratio of methanol to purified water is 1:20, and the filtration is repeated 5 times; the product obtained by filtration is placed in a centrifuge tube for centrifugation, the reagent used is a mixed solution of ethanol and purified water, the volume ratio of ethanol to purified water is 1:90, the solid content is 500g / L, the centrifugal rate is 12000rpm, the centrifugal time is 0.1h, and the centrifugal temperature is 15℃; then flash drying is carried out at a temperature of 150℃, a drying time of 0.1h, and a drying air volume of 1000m 3 / h; the powder obtained by flash drying was placed in a high-speed mixer for rotation cooling, the stirring temperature was 10°C, the stirring rate was 1200rpm, and the stirring time was 0.5h to obtain the nortanshinone-based eucalyptol hydromagnesite composite material Nts-Ea-HM (median particle size (D 50 ) is 2.5 μm), wherein the dosage ratio of nortanshinone to eucalyptol hydromagnesite is 5 mol:10 kg.

[0081] Comparative Example 1

[0082] The steps (1) and (2) are the same as those in Example 1;

[0083] (3) 106.1 g of nortanshinone was fully dissolved in a mixed solution of ethanol and purified water, wherein the volume ratio of ethanol to purified water was 20:1, and the solution was dissolved while being mechanically stirred at a mechanical stirring rate of 1000 rpm for 3.0 h, an ultrasonic power of 40 kHz, and a temperature of 60° C. to obtain a solution 2, wherein the concentration of the solution 2 was controlled to be 3 M;

[0084] (4) 10 kg of the obtained eucalyptus acidified hydromagnesite was stirred and dispersed in a mixture of ethanol and purified water, the volume ratio of ethanol to purified water was 1:50, the dispersion rate was 1000 rpm, the dispersion time was 1.8 h, and the dispersion solution 3 was obtained. The concentration of the dispersion solution 3 was controlled to be 10 M, and then the temperature was increased to 71° C. at a heating rate of 30° C. / h. During the heating process, the solution 2 was added dropwise to the dispersion solution 3 at a dropping rate of 2 drops / s until the dropping was completed. The stirring was continued for 3.5 h, and the stirring rate was controlled to 900 rpm. The product after the reaction was placed under -0.085 MPa for extraction The filter paper is a slow filter paper with 2 layers and a filtration power of 500W. During the filtration process, a mixed solution of ethanol and purified water is used for washing, and the volume ratio of ethanol to purified water is 1:10, which is repeated 3 times. The product obtained by filtration is placed in a centrifuge tube for centrifugal washing. The reagent used is a mixed solution of ethanol and purified water, and the volume ratio of ethanol to purified water is 1:40. The solid content is controlled to be 200g / L, the centrifugal speed is 8000rpm, the centrifugal time is 0.6h, and the centrifugal temperature is 10℃. Then flash drying is carried out at a temperature of 130℃, a drying time of 0.4h, and a drying air volume of 600m 3 / h; the powder obtained by flash drying was placed in a high-speed mixer for rotation cooling, the stirring temperature was 5°C, the stirring rate was 900rpm, and the stirring time was 6.0h to obtain the nortanshinone-based eucalyptol hydromagnesite composite material Nts-Ea-HM (median particle size (D 50 ) is 2.5 μm), wherein the dosage ratio of nortanshinone to eucalyptol hydromagnesite is 0.5 mol:10 kg.

[0085] Comparative Example 2

[0086] The steps (1) and (2) are the same as those in Example 1;

[0087] (3) dissolving 2.8 kg of nortanshinone in a mixed solution of ethanol and purified water, wherein the volume ratio of ethanol to purified water is 20:1, and dissolving while mechanically stirring at a mechanical stirring rate of 1000 rpm for 3.0 h, an ultrasonic power of 40 kHz, and a temperature of 50° C. to obtain a solution 2, wherein the concentration of the solution 2 is controlled to be 10 M;

[0088] (4) 10 kg of the obtained eucalyptus acidified hydromagnesite was stirred and dispersed in a mixture of ethanol and purified water, the volume ratio of ethanol to purified water was 1:50, the dispersion rate was 1000 rpm, the dispersion time was 1.8 h, and the dispersion 3 was obtained. The concentration of the dispersion 3 was controlled to be 10 M, and then the temperature was increased to 71 ° C at a heating rate of 30 ° C / h. During the heating process, the solution 2 was added to the dispersion 3 in a dropwise manner, and the drop rate was 2 drops / s until the drop addition was completed. Stirring was continued for 3.5 h, and the stirring rate was controlled to 900 rpm. The product after the reaction was placed under -0.085 MPa for Filtration, the filter paper is slow filter paper, the number of layers is 2, the filtration power is 500W, and the mixed solution of ethanol and purified water is used for washing during the filtration process. The volume ratio of ethanol to purified water is 1:10, and the filtration is repeated 3 times; the product obtained by filtration is placed in a centrifuge tube, the reagent used is a mixed solution of ethanol and purified water, the volume ratio of ethanol to purified water is 1:40, the solid content is controlled to be 200g / L, the centrifugal speed is 8000rpm, the centrifugal time is 0.6h, and the centrifugal temperature is 10℃; then flash drying is carried out, the temperature is 130℃, the drying time is 0.4h, and the drying air intake is 600m 3 / h; the powder obtained by flash drying was placed in a high-speed mixer for rotation cooling, the stirring temperature was 5°C, the stirring rate was 900rpm, and the stirring time was 6.0h to obtain the nortanshinone-based eucalyptol hydromagnesite composite material Nts-Ea-HM (median particle size (D 50 ) is 2.5 μm), wherein the dosage ratio of nortanshinone to eucalyptol hydromagnesite is 10 mol:10 kg.

[0089] Comparative Example 3

[0090] The natural hydromagnesite mineral powder (median particle size D 50 2.3 μm) was used as Comparative Example 3, which was not modified.

[0091] Characterization and performance testing

[0092] 1) By Figure 2 It can be seen from the particle size distribution diagram that the particle size distribution of the nortanshinone-eucalyptol hydromagnesite composite material Nts-Ea-HM prepared in Example 1 is relatively uniform, presenting a single peak, and concentrated around 2.8 μm.

[0093] 2) Figure 3 This is a SEM image of the nortanshinone-based eucalyptol hydromagnesite composite material Nts-Ea-HM prepared in Example 1. Figure 3 It can be seen that the powder surface is relatively rough, with a variety of irregular substances dispersed more evenly, and the overall surface is relatively continuous, with a better modification effect.

[0094] 3) The activation rate, oil absorption value and contact angle test were performed on the nortanshinone-based eucalyptol hydromagnesite composite material Nts-Ea-HM prepared in Examples 1 to 3, the nortanshinone-based eucalyptol hydromagnesite composite material Nts-Ea-HM in Comparative Examples 1 to 3, and the unmodified natural hydromagnesite powder. The test results are shown in Table 1:

[0095] Activation rate: The dry powder is tested by weighing method;

[0096] Oil absorption value: tested in accordance with DB / T5211.15-2014 standard.

[0097] Contact angle: The contact angle of the sample was measured using a contact angle meter.

[0098] Table 1 Test results of particle size, specific surface area and oil absorption value of powders used in Examples 1 to 3 and Comparative Examples 1 to 3

[0099] Case Activation rate / % Oil absorption value (mL / 100g) Contact angle (°) Example 1 94.7 25 109.2 Example 2 90.2 27 95.5 Example 3 93.1 26 101.3 Comparative Example 1 32.1 35 35.2 Comparative Example 2 67.2 33 75.1 Comparative Example 3 18.3 39 25.4

[0100] As can be seen from Table 1, compared with Examples 1 to 3 and Comparative Example 3, the activation rate of the hydromagnesite composite material Nts-Ea-HM modified with multilayers of nortanshinone and eucalyptol has increased significantly, and on the other hand, the oil absorption value has decreased significantly, indicating that after modification with the two natural products, the surface polarity of the composite material has decreased significantly. At the same time, the contact angle test results show that after modification with multiple layers of natural products, the composite material has been transformed from a hydrophilic powder to a hydrophobic powder, and the adsorption of processing aids has been suppressed, which helps to greatly reduce the processing cost in the polymer composite material; further compared with Comparative Examples 1 to 3, when the added natural product is not within the appropriate range, when it is too low, the modification effect is general, and the coating effect on the inner core natural hydromagnesite is limited. When it is too high, too much nortanshinone may wrap multiple Tianshui magnesite mineral particles together, causing passive aggregation of particles and increase in particle size. It can be seen that modifying natural mineral powders with a suitable proportion of low-polarity natural products can improve the activation rate and contact angle of natural hydromagnesite and significantly reduce its oil absorption value. The improvement of these properties is conducive to the dispersion and application of such composite materials in low-polarity or non-polar matrices.

[0101] 4) The nortanshinone-based eucalyptol hydromagnesite composite material Nts-Ea-HM prepared in Examples 1 to 3 and Comparative Examples 1 to 3 and the unmodified natural hydromagnesite powder were added to the thermoplastic elastomer alloy (LDPE / TPE 50 parts / 50 parts, wherein LDPE is Sinopec 2624H and TPE is Suzhou Hongshuo J5835). Specifically, the material was first plasticized in an internal mixer for 15 minutes, and DOP (dioctyl phthalate, 3 parts), paraffin (5 parts) and the nortanshinone-based eucalyptol hydromagnesite composite material Nts-Ea-HM (20 parts) or natural hydromagnesite (20 parts) prepared in different cases were added successively for mixing, mixed at 160° C. for 6 minutes, and placed in a flat vulcanizer at 165° C. for 10 minutes, a pressure of 10 MPa, and cold pressed for 5 to 10 minutes to make the corresponding standard sample for performance testing.

[0102] Mechanical properties test: in accordance with GB / T1040-2004, test temperature 23±2℃.

[0103] Melt index: tested in accordance with GB / T3682-2000, the experimental temperature is 190℃.

[0104] Thermogravimetric analysis test: room temperature to 600°C in nitrogen atmosphere, heating rate 10°C / min.

[0105] Oxygen index test: GB / T2406-1993.

[0106] Dielectric property test: Thin discs (thickness 1mm, diameter 20mm) were fully coated with conductive silver paste at room temperature and tested with a broadband dielectric constant tester.

[0107] The results are shown in Table 2 below:

[0108] Table 2 Performance test results of composite materials prepared from different powders in Examples 1 to 3 and Comparative Examples 1 to 3

[0109]

[0110] It can be seen from Table 2 that with the introduction of the nortanshinone-eucalyptol hydromagnesite composite material Nts-Ea-HM, the mechanical properties of the LDPE / TPE composite material increased significantly, which indicates that the composite material can effectively enhance the mechanical properties of the thermoplastic elastomer. At the same time, it also confirms from another aspect that the introduction of these two natural products can effectively improve the compatibility of the composite material in low-polarity or non-polar thermoplastic elastomer alloys. In terms of processing performance, after the introduction of the two natural products, the fluidity of the LDPE / TPE composite material increased to a certain extent, indicating that the two can be bonded between the molecular chains. It helps the slip and flow of molecular chains, and is suitable for improving the extrusion fluidity and mold filling capacity of LDPE / TPE. In terms of thermal stability, after adding a suitable proportion of Nts-Ea-HM composite materials, the residual carbon rate of the composite materials at 600°C increased significantly, indicating that the introduction of the two natural products can effectively promote the carbonization of the composite materials, and the carbonization amount increased significantly, from 15.3% to 38.6%. In terms of combustion performance, after the introduction of the composite material Nts-Ea-HM, the limiting oxygen index of the composite material increased significantly, from 16.8% to 30.6%, from flammable materials to flame-retardant materials, typically improving its flame retardant effect. This may be because the outer layer of nortanshinone and eucalyptol modified the natural hydromagnesite, which can significantly improve the synergistic flame retardant effect of the core and the shell, which is specifically reflected in the rapid aromatic ring carbonization of the outer layer and the dehydration condensation of the inner core, forming a flame-retardant and refractory MgO ceramic precursor skeleton, and the outer aromatic carbon layer attached to it to form a hybrid carbon layer, which effectively improves the barrier of the condensed carbon layer to heat flow, air flow and mass flow, strengthens the flame retardant effect of the condensed phase, and the apparent oxygen The index is significantly improved. In terms of dielectric loss, with the introduction of Nts-Ea-HM, it can better fill the gaps in the molecular chains and effectively fill the gaps between the molecular chains. A tighter physical entanglement structure is formed between the molecular chains and the powder, which reduces the heat loss and the dielectric loss also shows a downward trend. However, when the molar mass ratio of nordanshinone on the surface of the composite material and the natural hydromagnesite inside is not appropriate, the mechanical properties of the LDPE / TPE thermoplastic elastomer alloy are limited. This may be because when the surface nordanshinone When the ratio of ketone to internal natural hydromagnesite is too low or too high, the modification effect of nortanshinone on natural hydromagnesite is limited. When it is too low, the surface shielding effect is poor. When it is too high, multiple natural hydromagnesite powder particles may be wrapped together, resulting in physical aggregation and physical loose adsorption stacking, which are easily peeled off during processing, and may also become stress defects when stretched by external forces, ultimately affecting the mechanical properties of LDPE / TPE thermoplastic elastomer alloys; at the same time, the processing fluidity will also be affected, and the reduction in compatibility has a very limited effect on improving the processing fluidity (Comparative Examples 1-3); in addition, in terms of residual carbon rate, due to the difficulty in effectively forming a good internal and external synergistic carbonization effect, the carbonization amount at 600°C decreases significantly. In terms of combustion performance, the decrease in physical barrier properties leads to a decrease in carbonization quality, and the lack of quantity also leads to limited condensed phase flame retardant effect, and the final oxygen index decreases significantly. Finally, in terms of dielectric loss, the inappropriate proportion of nortanshinone leads to an increase in the gap between the molecular chain and the powder, affecting the material polarity and increasing the dielectric loss. .

[0111] The above results show that the successive introduction of tanshinone and eucalyptol can improve the performance of natural hydromagnesite powder in mechanical properties, processing fluidity, residual carbon rate, limiting oxygen index and tanδ. Making full use of the low-polarity multi-conjugated natural products and rationally reconstructing them can make the tanshinone-based eucalyptol hydromagnesite composite material Nts-Ea-HM have better dispersibility and compatibility in the LDPE / TPE thermoplastic elastomer alloy matrix, which has a good effect on improving the various properties of the composite material.

[0112] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a nortanshinone-eucalyptol hydromagnesite composite material, comprising the following steps: The eucalyptol acid, hydromagnesite and the first solvent are mixed and modified to obtain eucalyptol acidified hydromagnesite; The eucalyptol hydromagnesite is mixed with a dispersant to disperse the mixture, thereby obtaining a eucalyptol hydromagnesite dispersion; mixing nortanshinone with a second solvent to obtain a nortanshinone solution; The eucalyptol acidified hydromagnesite dispersion is mixed with a nortanshinone solution for hybridization to obtain a nortanshinone-based eucalyptol acidified hydromagnesite composite material.

2. The preparation method according to claim 1, characterized in that: The median particle size D of the hydromagnesite 50 The particle size is 1.0-4.8 μm; the dosage ratio of eucalyptus acid to hydromagnesite is 0.1-5.0 mol:10 kg.

3. The preparation method according to claim 1, characterized in that: The first solvent includes one of ethanol, methanol, ethylene glycol, N,N-dimethylformamide, ethyl acetate and propanol.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The modification includes a first reaction and a second reaction carried out sequentially, wherein the temperature of the first reaction is 90-130°C, the time is 0.2-3.5h, and the stirring rate is 500-1600r / min; the temperature of the second reaction is 1-10°C, the time is 0.1-2.0h, and the stirring rate is 300-1000r / min.

5. The preparation method according to claim 1, characterized in that: The dispersant is a mixture of a first alcohol and water, wherein the first alcohol is one or more of methanol, ethanol, propanol, 1,2-propylene glycol, isopropanol, ethylene glycol and 1,3-propylene glycol, and the volume ratio of the first alcohol to water is 1:1 to 100; The dispersion rate is 800-2000 rpm, the time is 0.2-3.6 hours, and the concentration of the eucalyptol hydromagnesite dispersion is 1-20M.

6. The preparation method according to claim 1, characterized in that: The second solvent is a mixed solution of a second alcohol and water, the second alcohol is one or more of methanol, ethanol, propanol, 1,2-propylene glycol, isopropanol, ethylene glycol and 1,3-propylene glycol, and the volume ratio of the second alcohol to water is 1 to 50:1; The temperature of mixing the nortanshinone and the second solvent is 40-60° C.; the concentration of the nortanshinone solution is 1-10M.

7. The preparation method according to claim 1, characterized in that: The usage ratio of nortanshinone to eucalyptol hydromagnesite is 1-5 mol:10 kg.

8. The preparation method according to claim 1 or 7, characterized in that: The hybridization temperature is 50-99° C., and the hybridization time is 0.5-6.5 h.

9. The nortanshinone-eucalyptol hydromagnesite composite material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the nortanshinone-eucalyptol hydromagnesite composite material according to claim 9 in thermoplastic elastomer alloy masterbatch.