Environment-friendly oil seal material and preparation method thereof
By combining nitrile rubber, polyurethane, hydrogenated nitrile rubber and other materials with highly wear-resistant carbon black, diatomaceous earth and other components, and performing vulcanization treatment, a highly wear-resistant and environmentally friendly oil seal material is prepared, which solves the problem of existing oil seals. The problem of insufficient wear resistance of the material is achieved, and longer sealing performance and resistance to lubricants are achieved.
Patent Information
- Application Number
- CN202410926783.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-01
AI Technical Summary
The wear resistance of existing oil seal materials has not been qualitatively improved, which limits the use range and service life of oil seal materials.
Using a combination of nitrile rubber, polyurethane, hydrogenated nitrile rubber, high wear-resistant carbon black, calcium carbonate, diatomaceous earth, silica, sulfur, antioxidants, UV stabilizers, lubricants and antioxidants, through mixing, plastic Refining and vulcanization treatments are used to prepare highly wear-resistant and environmentally friendly oil seal materials.
The wear resistance and sealing performance of the oil seal material are improved, which can maintain a stable sealing effect in long-term use and have good tolerance to lubricating oil to prevent damage due to oil erosion.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of oil seal materials, in particular to an environmentally friendly oil seal material and a preparation method thereof. Background Art
[0002] Oil seals refer to general seals, which are used to seal lubricating oil. Oil seals are mechanical components used to seal grease. Their main function is to isolate the parts that need lubrication from the output parts in the transmission parts to prevent the lubricating oil from leaking. Therefore, this type of original part is called an oil seal. Oil seals are widely used in various industrial equipment, automobiles and other fields, and are one of the important components to ensure the normal operation of mechanical equipment.
[0003] However, most of the oil seal materials currently sold on the market have undergone special treatment, the main purpose of which is to give the oil seal materials higher wear resistance so that they can maintain a stable sealing effect during long-term use. However, the wear resistance of materials sold on the market has not been qualitatively improved, which has always limited the scope of use and service life of oil seal materials. Summary of the invention
[0004] The present invention aims at the problems existing in the prior art and discloses an environmentally friendly oil seal material and a preparation method thereof. The present invention adopts a combination of multiple components to prepare an oil seal material with high wear resistance.
[0005] The present invention is achieved in that:
[0006] An environmentally friendly oil seal material, characterized in that, in parts by mass, the oil seal material is prepared from the following components:
[0007] Nitrile rubber: 20-30 parts;
[0008] Polyurethane: 20-30 parts;
[0009] Hydrogenated nitrile rubber: 10-15 parts;
[0010] High wear-resistant carbon black: 3-8 parts;
[0011] Calcium carbonate: 2-5 parts;
[0012] Diatomaceous earth: 5-9 parts;
[0013] Silicon dioxide: 1-3 parts;
[0014] Sulfur: 2-3 parts;
[0015] Antioxidant: 1-2 parts;
[0016] UV stabilizer: 1-2 parts;
[0017] Lubricant: 1-2 parts;
[0018] Anti-aging agent: 1 to 2 parts.
[0019] Furthermore, in terms of parts by mass, the mass ratio of the nitrile rubber, polyurethane and hydrogenated nitrile rubber is 2:2:1.
[0020] Furthermore, in terms of parts by mass, the weight ratio of the antioxidant, the ultraviolet stabilizer, the lubricant and the anti-aging agent is 1:1:1:1.
[0021] Furthermore, the oil seal material is prepared from the following components in parts by mass:
[0022] Nitrile rubber: 26 parts;
[0023] Polyurethane: 26 parts;
[0024] Hydrogenated nitrile rubber: 13 parts;
[0025] High wear-resistant carbon black: 5 parts;
[0026] Calcium carbonate: 3 parts;
[0027] Diatomaceous earth: 7 parts;
[0028] Silicon dioxide: 2 parts;
[0029] Sulfur: 3 parts;
[0030] Antioxidants: 2 parts;
[0031] UV stabilizer: 2 parts;
[0032] Lubricant: 2 parts;
[0033] Anti-aging agent: 2 parts.
[0034] Furthermore, the preparation method of the environmentally friendly oil seal material is:
[0035] Step 1, mixing: weigh 20-30 parts of nitrile rubber, 20-30 parts of polyurethane, and 10-15 parts of hydrogenated nitrile rubber according to mass parts, mix the above materials, mix them evenly and set aside, stirring at a speed of 60-100r / min;
[0036] Step 2, plasticizing and molding: add 3-8 parts of high wear-resistant carbon black, 2-5 parts of calcium carbonate, 5-9 parts of diatomaceous earth, and 1-3 parts of silicon dioxide to the above-mentioned mixed materials, mix and plasticize again, the plasticizing temperature is: 150°C; the mixing time is: 30 minutes;
[0037] Step 3, vulcanization: add 2 to 3 parts of sulfur, 1 to 2 parts of antioxidant, 1 to 2 parts of UV stabilizer, 1 to 2 parts of lubricant, and 1 to 2 parts of antioxidant to the mixed material in step 2; perform vulcanization treatment at a temperature of 250°C, and the mixture is ready after vulcanization.
[0038] The beneficial effects of the present invention compared with the prior art are:
[0039] The present invention adopts a combination of nitrile rubber, polyurethane and hydrogenated nitrile rubber, and further adopts a combination of nitrile rubber and hydrogenated nitrile rubber, so that the oil seal material of the present invention combines the oil resistance of nitrile rubber with the heat resistance and oxidation resistance improved after hydrogenation. In the present invention, nitrile rubber, polyurethane and hydrogenated nitrile rubber are combined with high wear-resistant carbon black, calcium carbonate, diatomaceous earth and silicon dioxide to increase the hardness and wear resistance of the oil seal material.
[0040] The oil seal material of the present invention has good sealing performance, can effectively prevent the leakage of lubricating oil, and ensure the normal operation of mechanical equipment. The oil seal material of the present invention has high wear resistance and can maintain a stable sealing effect during long-term use. In addition, the oil seal material of the present invention has good tolerance to lubricating oil and will not be damaged by the erosion of oil, thereby ensuring the durability of the oil seal. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail by enumerating examples below. It should be noted that the specific implementation described here is only used to explain the present invention and is not used to limit the present invention.
[0042] Example 1
[0043] The preparation method of the environmentally friendly oil seal material disclosed in the present invention is:
[0044] Step 1, mixing: weigh 25 parts of nitrile rubber, 25 parts of polyurethane, and 12.5 parts of hydrogenated nitrile rubber according to mass parts, mix the above materials, mix them evenly and set aside, the stirring speed is 60-100r / min; the mass ratio between the nitrile rubber, polyurethane, and hydrogenated nitrile rubber is 2:2:1.
[0045] Step 2, plasticizing and molding: add 6 parts of high wear-resistant carbon black, 3 parts of calcium carbonate, 6 parts of diatomaceous earth, and 2 parts of silicon dioxide to the above-mentioned mixed materials, mix and plasticize again, the plasticizing temperature is: 150°C; the mixing time is: 30 minutes;
[0046] Step 3, vulcanization: add 2 parts of sulfur, 1 part of antioxidant, 1 part of UV stabilizer, 1 part of lubricant, and 1 part of antioxidant to the mixed material in step 2; perform vulcanization treatment at a temperature of 250°C, and the vulcanization is completed. The mass ratio of the antioxidant, UV stabilizer, lubricant, and antioxidant is 1:1:1:1.
[0047] Example 2
[0048] The preparation method of the environmentally friendly oil seal material disclosed in the present invention is:
[0049] Step 1, mixing: weigh 30 parts of nitrile rubber, 30 parts of polyurethane, and 15 parts of hydrogenated nitrile rubber according to mass parts, mix the above materials, mix them evenly and set aside, the stirring speed is 60-100r / min; the mass ratio between the nitrile rubber, polyurethane, and hydrogenated nitrile rubber is 2:2:1.
[0050] Step 2, plasticizing and molding: add 8 parts of high wear-resistant carbon black, 5 parts of calcium carbonate, 9 parts of diatomaceous earth and 3 parts of silicon dioxide to the above-mentioned mixed materials, mix and plasticize again, the plasticizing temperature is: 150°C; the mixing time is: 30 minutes;
[0051] Step 3, vulcanization: add 3 parts of sulfur, 2 parts of antioxidant, 2 parts of UV stabilizer, 2 parts of lubricant, and 2 parts of antioxidant to the mixed material in step 2; perform vulcanization treatment at a temperature of 250°C, and the vulcanization is completed. The mass ratio of the antioxidant, UV stabilizer, lubricant, and antioxidant is 1:1:1:1.
[0052] Example 3
[0053] The preparation method of the environmentally friendly oil seal material disclosed in the present invention is:
[0054] Step 1, mixing: weigh 20 parts of nitrile rubber, 20 parts of polyurethane, and 10 parts of hydrogenated nitrile rubber according to mass parts, mix the above materials, mix them evenly and set aside, the stirring speed is 60-100r / min; the mass ratio between the nitrile rubber, polyurethane, and hydrogenated nitrile rubber is 2:2:1.
[0055] Step 2, plasticizing and molding: add 3 parts of high wear-resistant carbon black, 2 parts of calcium carbonate, 5 parts of diatomaceous earth, and 1 part of silicon dioxide to the above-mentioned mixed materials, mix and plasticize again, the plasticizing temperature is: 150°C; the mixing time is: 30 minutes;
[0056] Step 3, vulcanization: add 2 parts of sulfur, 1 part of antioxidant, 1 part of UV stabilizer, 1 part of lubricant, and 1 part of antioxidant to the mixed material in step 2; perform vulcanization treatment at a temperature of 250°C, and the vulcanization is completed. The mass ratio of the antioxidant, UV stabilizer, lubricant, and antioxidant is 1:1:1:1.
[0057] Example 4
[0058] The preparation method of the environmentally friendly oil seal material disclosed in the present invention is:
[0059] Step 1, mixing: weigh 26 parts of nitrile rubber, 26 parts of polyurethane, and 13 parts of hydrogenated nitrile rubber according to mass parts, mix the above materials, mix them evenly and set aside, the stirring speed is 60-100r / min; the mass ratio between the nitrile rubber, polyurethane, and hydrogenated nitrile rubber is 2:2:1.
[0060] Step 2, plasticizing and molding: add 5 parts of high wear-resistant carbon black, 3 parts of calcium carbonate, 7 parts of diatomaceous earth, and 2 parts of silicon dioxide to the above-mentioned mixed materials, mix and plasticize again, the plasticizing temperature is: 150°C; the mixing time is: 30 minutes;
[0061] Step 3, vulcanization: add 3 parts of sulfur, 2 parts of antioxidant, 2 parts of UV stabilizer, 2 parts of lubricant, and 2 parts of antioxidant to the mixed material in step 2; perform vulcanization treatment at a temperature of 250°C, and the vulcanization is completed. The mass ratio of the antioxidant, UV stabilizer, lubricant, and antioxidant is 1:1:1:1.
[0062] Example 5
[0063] The preparation method of the environmentally friendly oil seal material disclosed in the present invention is:
[0064] Step 1, mixing: weigh 28 parts of nitrile rubber, 28 parts of polyurethane, and 14 parts of hydrogenated nitrile rubber according to mass parts, mix the above materials, mix them evenly and set aside, the stirring speed is 60-100r / min; the mass ratio between the nitrile rubber, polyurethane, and hydrogenated nitrile rubber is 2:2:1.
[0065] Step 2, plasticizing and molding: add 6 parts of high wear-resistant carbon black, 4 parts of calcium carbonate, 7 parts of diatomaceous earth and 1 part of silicon dioxide to the above-mentioned mixed materials, mix and plasticize again, the plasticizing temperature is: 150°C; the mixing time is: 30 minutes;
[0066] Step 3, vulcanization: add 3 parts of sulfur, 1 part of antioxidant, 1 part of UV stabilizer, 1 part of lubricant, and 1 part of antioxidant to the mixed material in step 2; perform vulcanization treatment at a temperature of 250°C, and the vulcanization is completed. The mass ratio of the antioxidant, UV stabilizer, lubricant, and antioxidant is 1:1:1:1.
[0067] Example 6
[0068] The preparation method of the environmentally friendly oil seal material disclosed in the present invention is:
[0069] Step 1, mixing: weigh 22 parts of nitrile rubber, 22 parts of polyurethane, and 11 parts of hydrogenated nitrile rubber according to mass parts, mix the above materials, mix them evenly and set aside, the stirring speed is 60-100r / min; the mass ratio between the nitrile rubber, polyurethane, and hydrogenated nitrile rubber is 2:2:1.
[0070] Step 2, plasticizing and molding: add 3-8 parts of high wear-resistant carbon black, 2-5 parts of calcium carbonate, 5-9 parts of diatomaceous earth, and 1-3 parts of silicon dioxide to the above-mentioned mixed materials, mix and plasticize again, the plasticizing temperature is: 150°C; the mixing time is: 30 minutes;
[0071] Step 3, vulcanization: add 2 parts of sulfur, 2 parts of antioxidant, 2 parts of UV stabilizer, 2 parts of lubricant, and 2 parts of antioxidant to the mixed material in step 2; perform vulcanization treatment at a temperature of 250°C, and the vulcanization is completed. The mass ratio of the antioxidant, UV stabilizer, lubricant, and antioxidant is 1:1:1:1.
[0072] Example 7
[0073] The preparation method of the environmentally friendly oil seal material disclosed in the present invention is:
[0074] Step 1, mixing: weigh 28 parts of nitrile rubber, 28 parts of polyurethane, and 14 parts of hydrogenated nitrile rubber according to mass parts, mix the above materials, mix them evenly and set aside, the stirring speed is 60-100r / min; the mass ratio between the nitrile rubber, polyurethane, and hydrogenated nitrile rubber is 2:2:1.
[0075] Step 2, plasticizing and molding: add 7 parts of high wear-resistant carbon black, 3 parts of calcium carbonate, 9 parts of diatomaceous earth and 3 parts of silicon dioxide to the above mixed materials, mix and plasticize again, the plasticizing temperature is: 150; ℃ mixing time: 30 minutes;
[0076] Step 3: Vulcanization: Add 2.5 parts of sulfur, 1.5 parts of antioxidant, 1.5 parts of UV stabilizer, 1.5 parts of lubricant, and 1.5 parts of antioxidant to the mixed material in step 2; vulcanize at a temperature of 250°C until vulcanization is complete. The mass ratio of the antioxidant, UV stabilizer, lubricant, and antioxidant is 1:1:1:1.
[0077] The oil seal material in the above embodiment was tested for performance, and the results are shown in the following table:
[0078] Elongation at break % Tensile strength MPa Impact rebound Example 1 185 15.0 44 Example 2 173 15.6 46 Example 3 190 16.0 45 Example 4 220 14.7 50 Example 5 194 15.1 48 Example 6 188 15.2 47 Example 7 210 15.3 46
[0079] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principle of the present invention, and these improvements should also be regarded as within the protection scope of the present invention.
Claims
1. An environmentally friendly oil seal material, characterized in that: The oil seal material is prepared from the following components in parts by mass: Nitrile rubber: 20-30 parts; Polyurethane: 20-30 parts; Hydrogenated nitrile rubber: 10-15 parts; High wear-resistant carbon black: 3-8 parts; Calcium carbonate: 2-5 parts; Diatomaceous earth: 5-9 parts; Silicon dioxide: 1-3 parts; Sulfur: 2-3 parts; Antioxidant: 1-2 parts; UV stabilizer: 1-2 parts; Lubricant: 1-2 parts; Anti-aging agent: 1 to 2 parts.
2. The environmentally friendly oil seal material according to claim 1, characterized in that: Calculated by weight, the weight ratio of the nitrile rubber, polyurethane and hydrogenated nitrile rubber is 2:2:
1.
3. The environmentally friendly oil seal material according to claim 1, characterized in that: Calculated by weight, the weight ratio of the antioxidant, the ultraviolet stabilizer, the lubricant and the anti-aging agent is 1:1:1:
1.
4. The environmentally friendly oil seal material according to claim 1, characterized in that: The oil seal material is prepared from the following components in parts by mass: Nitrile rubber: 26 parts; Polyurethane: 26 parts; Hydrogenated nitrile rubber: 13 parts; High wear-resistant carbon black: 5 parts; Calcium carbonate: 3 parts; Diatomaceous earth: 7 parts; Silicon dioxide: 2 parts; Sulfur: 3 parts; Antioxidants: 2 parts; UV stabilizer: 2 parts; Lubricant: 2 parts; Anti-aging agent: 2 parts.
5. The environmentally friendly oil seal material according to claim 1, characterized in that: The preparation method of the environmentally friendly oil seal material is as follows: Step 1, mixing: weigh 20-30 parts of nitrile rubber, 20-30 parts of polyurethane, and 10-15 parts of hydrogenated nitrile rubber according to mass parts, mix the above materials, mix them evenly and set aside, and the stirring speed is 60-100r / min; Step 2, plasticizing and molding: add 3-8 parts of high wear-resistant carbon black, 2-5 parts of calcium carbonate, 5-9 parts of diatomaceous earth, and 1-3 parts of silicon dioxide to the above-mentioned mixed materials, mix and plasticize again, the plasticizing temperature is: 150; ℃ mixing time: 30 minutes; Step 3, vulcanization: add 2 to 3 parts of sulfur, 1 to 2 parts of antioxidant, 1 to 2 parts of UV stabilizer, 1 to 2 parts of lubricant, and 1 to 2 parts of antioxidant to the mixed material in step 2; perform vulcanization treatment at a temperature of 250°C, and the mixture is ready after vulcanization.