Antibacterial polymer film material and preparation method thereof

By adding components such as modified chitosan antibacterial agent and nano-titanium dioxide into the polypropylene film, the problem of insufficient antibacterial performance of the polypropylene film is solved, and efficient antibacterial and mechanical performance improvement are achieved, which is suitable for food and medical fields.

CN118725459AInactive Publication Date: 2024-10-01JIANGSU PAKION MEDICAL MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410979080.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polypropylene films lack antibacterial properties and cannot effectively prevent bacterial adhesion and contamination, limiting their wide application in the food and medical fields.

Method used

The preparation method of antibacterial polymer film materials is adopted, including polypropylene, polyethylene terephthalate, compatibilizing aids, modified chitosan antibacterial agent, nanometer titanium dioxide and antibacterial glass powder, by adjusting the proportion of components and Process steps to improve the antibacterial properties and mechanical properties of the material.

Benefits of technology

The antibacterial properties, mechanical properties, thermal stability and weather resistance of the polymer film are significantly improved, while the cytotoxicity is reduced, the service life is extended, and the optical transparency is maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725459A_ABST
    Figure CN118725459A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of film materials, in particular to an antibacterial polymer film material and a preparation method thereof. The antibacterial polymer film material is specifically prepared from the following components in parts by weight: 68 to 87 parts of polypropylene, 32 to 41 parts of polyethylene glycol terephthalate, 15 to 30 parts of a compatible aid, 3 to 4 parts of a modified chitosan antibacterial agent, 8 to 10 parts of nano titanium dioxide, 1 to 3 parts of antibacterial glass powder and 0.5 to 1 part of an antioxidant. Amphipathic balance of chitosan is adjusted through hydrophobic acrylate and butylamine, and meanwhile, an intermediate product with good antibacterial property and oxidation resistance is grafted to obtain the modified chitosan antibacterial agent. The added nano titanium dioxide and antibacterial glass powder are cooperated to improve the antibacterial property, water solubility and biocompatibility of the antibacterial polymer film and reduce the cytotoxicity; meanwhile, the oxidation resistance, the mechanical property, the heat stability and the weather resistance of the antibacterial polymer film are improved through the cooperation of the antibacterial glass powder and the nano titanium dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of film materials, and in particular relates to an antibacterial polymer film material and a preparation method thereof. Background Art

[0002] As the mainstream packaging material in the current market, plastic packaging has been widely used in food, medical and other fields due to its light weight, high strength, water barrier and oil resistance. Polypropylene is a thermoplastic widely used in general applications. The polypropylene film made has excellent properties such as light weight, high transparency, good flatness, good rigidity, strong mechanical adaptability, good moisture resistance, good smoothness, high film making speed, uniform thickness, moisture resistance, oil resistance, heat resistance and cold resistance. However, the lack of antibacterial properties of polypropylene may limit its use because it cannot effectively prevent bacterial adhesion and contamination.

[0003] Therefore, in order to expand the application of polypropylene and give it antibacterial activity, a polymer film material with good antibacterial and mechanical properties is urgently needed. Summary of the invention

[0004] The object of the present invention is to provide an antibacterial polymer film material and a preparation method thereof, so as to solve the technical problems in the prior art.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: The technical solution provided by the present invention is as follows: In a first aspect, the present invention provides an antibacterial polymer film material, which specifically comprises the following components by weight: 68-87 parts of polypropylene, 32-41 parts of polyethylene terephthalate, 15-30 parts of a compatibility aid, 3-4 parts of a modified chitosan antibacterial agent, 8-10 parts of nano-titanium dioxide, 1-3 parts of antibacterial glass powder, and 0.5-1 part of an antioxidant.

[0006] By adopting the above technical solution, polyethylene terephthalate is added to improve the impact resistance and toughness of the polypropylene film, and by controlling the mass ratio of the two raw materials, the compatibility between the components is promoted, thereby improving the comprehensive performance of the polymer film material.

[0007] The compatibility aid includes at least one of sodium alginate, polyvinyl alcohol and polyethylene glycol.

[0008] By adopting the above technical solution, the surface activity of the compatibilizing agent can enhance the adsorption between nano-titanium dioxide, modified chitosan antibacterial agent and antibacterial glass powder and the matrix, thereby increasing stability and dispersibility, reducing material precipitation, and effectively improving the long-lasting antibacterial ability of the polymer film.

[0009] Preferably, the method for preparing the modified chitosan antibacterial agent comprises the following steps: S1: 100-200 g chitosan and 11.4-22.8 g 1,4-diazabicyclo[2.2.2]octane are added to 5-10 L water, stirred at 300-500 rpm for 20-30 min, 172-340 g functionalized polyethylene glycol is added, and the stirring is continued at 300-500 rpm at room temperature for 1.5-2.5 days, and then 5-7 L acetone is added for precipitation, filtered, and washed with acetone for 3-5 times to obtain functional chitosan; The structural formula of functional chitosan is as follows: In the above process, the amino groups of chitosan react with the double bonds of functionalized polyethylene glycol.

[0010] By adopting the above technical scheme, PEG has good biocompatibility, hydrophilicity and water solubility, and PEG functionalized with hydrophobic acrylate end is grafted onto the chitosan backbone, rather than directly connecting the hydrophobic group to the chitosan backbone, so as to improve the water solubility and biocompatibility of functional chitosan and reduce cytotoxicity. The butylamine grafted with PEG functionalized with hydrophobic acrylate end can enhance the cationic effect of chitosan; and synergistically improve the antibacterial activity of chitosan with the amphiphilic balance of functionalized chitosan.

[0011] S2: 50-100 g of functional chitosan was added to 0.94-2 L of N, N-dimethylformamide, and stirred at 50-60° C. for 25-35 min in a nitrogen atmosphere. After cooling to room temperature, 36.3-72 g of 2-[dodecylthio(thiocarbonyl)thio]-2-methylpropionic acid, 193-386 g of N, N'-dicyclohexylcarbodiimide and 7.5-15 g of 4-dimethylaminopyridine were added. The mixture was magnetically stirred at room temperature for 12-24 h, cooled in an ice bath for 0.5-1.5 h, and then vacuum filtered. 1-2 L of ether was added to the filtrate for precipitation, and the filter cake was washed with ether for 3-5 times to obtain grafted chitosan. The structural formula of grafted chitosan is as follows: In the above process, the carboxylic acid of 2-[dodecylthio(thiocarbonyl)thio]-2-methylpropionic acid reacts with the primary alcohol of chitosan to form an ester through the Steglich esterification reaction under the action of the catalyst 4-dimethylaminopyridine, and serves as the reaction site for the subsequent RAFT polymerization.

[0012] S3: Add 280-480g of the intermediate product, 20-40g of grafted chitosan, and 0.43-0.8g of azobisisobutyronitrile to 1.9-3.8L N,N-dimethylformamide, stir magnetically for 15-25min, react at 65-75°C in a nitrogen atmosphere for 16-20h, immerse the entire reaction in liquid nitrogen to quench the reaction, and after thawing, add 2-4L of acetone to the solution for precipitation, vacuum filter, wash the filter cake with acetone 3-5 times, and vacuum dry at 70-80°C for 12-20h to obtain a modified chitosan antibacterial agent.

[0013] The structural formula of modified chitosan antibacterial agent is as follows: The method for preparing the intermediate product comprises the following steps: 458-916 g of 4-vinylbenzyl chloride and 0.95-1.9 kg of triphenylphosphine are added to 5-10 L of acetone, and magnetically stirred for 36-54 h in a nitrogen atmosphere, and then cooled to room temperature. Then 7-15 L of petroleum ether is added, and the mixture is filtered. The filter cake is washed with petroleum ether for 3-5 times, and then vacuum dried at room temperature for 20-28 h to obtain an intermediate product.

[0014] The structural formula of the intermediate product is as follows: The method for preparing the functionalized polyethylene glycol comprises the following steps: Add 400-600 g of polyethylene glycol diacrylate to 2.5-3.8 L of water, stir for 15-25 min, then add 69.2-104 mL of butylamine and 1.5-2.2 L of N,N-dimethylformamide, stir magnetically at room temperature for 70-74 h, remove the solvent in vacuo, wash with ethyl acetate 3-5 times, dry in air for 10-14 h, and further dry under vacuum for 12-16 h to obtain functionalized polyethylene glycol.

[0015] The structural formula of functionalized polyethylene glycol is as follows: By adopting the above technical scheme, the intermediate product is a quaternary phosphate ionic liquid, which has a larger atomic radius and lower electronegativity of phosphorus atoms, so that it has stronger polarization performance, effective antibacterial activity, and a wide antibacterial range, and has good chemical stability and excellent weather resistance and oxidation resistance. After being grafted with functionalized chitosan, the solubility of the intermediate product can be improved, the dosage can be reduced, and the cytotoxicity can be reduced. The electrostatic interaction between the obtained modified chitosan antibacterial agent and the negatively charged bacterial cell membrane leads to cation-induced cracking, resulting in membrane structure rupture, organic matter leakage, and ultimately cell death. It has a long-lasting, low-toxicity and low-dose antibacterial effect; the modified chitosan antibacterial agent, as a macromolecule, can be used as a dispersant and stabilizer for nano-titanium dioxide and antibacterial glass powder in a polymer film, thereby reducing the agglomeration of nano-titanium dioxide and antibacterial glass powder, so that the nano-titanium dioxide and antibacterial glass powder can be more stably dispersed in the polymer film, prolonging the service life and exerting the maximum antibacterial effect.

[0016] Preferably, the relative molecular mass of the polyethylene glycol diacrylate is about 575 Da.

[0017] Preferably, the antioxidant includes at least one of 2,6-di-tert-butyl-p-methylphenol, 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene.

[0018] Preferably, the method for preparing the antibacterial glass powder comprises the following steps: 35-70g ZnO, 34-68g SiO2, 2-4g B2O3, 10-20g Na2CO3, 9-18g CaCO3 and 10-20g K2CO3 are mixed in a 3D mixer for 4-6h to obtain a mixture, and the mixture is transferred into a Pt crucible, placed in an electric furnace, heated to 1250-1350°C at a heating rate of 8-12°C / min, maintained for 0.5-1.5h, poured into a preheated graphite mold, annealed at 500-600°C for 0.5-1.5h, and then slowly cooled to room temperature to remove thermal residual stress, crushed by ball milling, and separated by an air classifier to obtain antibacterial glass powder.

[0019] By adopting the above technical scheme, ZnO, SiO2, B2O3, Na2CO3, CaCO3, and K2CO3 are used as precursor materials, and a zinc silicate antibacterial glass powder with ZnO as the main antibacterial component is obtained through a melt quenching process. The amorphous structure of the antibacterial glass powder gives it a large surface area, which is beneficial to the release of zinc ions. The large surface area and increased volume fraction can improve the physical and chemical mechanisms of the thermal stability of the polymer film. The presence of hydroxyl groups on the surface of the antibacterial glass powder can enhance the surface hydrophilicity of the polymer film material. Due to the formation of a hydration layer, the hydrophobic interaction between the surface and bacteria is reduced, effectively inhibiting the adhesion of bacteria, and synergistically enhancing the antibacterial properties of the polymer film material.

[0020] By adopting the above technical scheme, nano titanium dioxide has antibacterial properties, strong ultraviolet shielding ability, good chemical stability and thermal stability, and generates chemically active superoxide anion free radicals O through photocatalysis. 2- When encountering bacteria, the hydroxyl free radicals OH· directly attack the bacterial cell wall, cell membrane or components within the cell, causing the degradation of organic matter in the bacteria, thereby killing the bacteria and decomposing them. The photocatalytic effect of nano-titanium dioxide is long-lasting, which can effectively enhance the long-lasting antibacterial effect of the polymer film. The antibacterial effect of zinc oxide in the antibacterial glass powder is similar to that of nano-titanium dioxide, and it also performs antibacterial work through photocatalysis. It cooperates with nano-titanium dioxide to improve the antioxidant, antibacterial, weather resistance and thermal stability of the polymer film.

[0021] In a second aspect, the present invention further provides a method for preparing an antibacterial polymer film material, comprising the following steps: Step (1) 68-87 parts of polypropylene, 32-41 parts of polyethylene terephthalate, 15-30 parts of a compatibility aid, 3-4 parts of a modified chitosan antibacterial agent, 8-10 parts of nano titanium dioxide, 1-3 parts of antibacterial glass powder, and 0.5-1 part of an antioxidant are stirred and mixed at a speed of 150-250 rpm for 1.5-2.5 hours to obtain a mixed material; Step (2) placing the mixed material in a twin-screw extruder, stirring and mixing evenly, and then casting the mixed material on a casting machine to form an antibacterial polymer film material.

[0022] Preferably, the temperature of the twin-screw extruder from the feed port to the discharge port is: 180°C, 190°C, 200°C, 210°C, 200°C, 190°C respectively; the extrusion speed is 150-250r / min; the casting machine traction rate is 150-250m / min.

[0023] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. The present invention adjusts the amphiphilic balance of chitosan by hydrophobic acrylate and butylamine, and simultaneously grafts an intermediate product with good antibacterial and antioxidant properties to obtain a modified chitosan antibacterial agent, which cooperates with the added nano titanium dioxide and antibacterial glass powder to improve the antibacterial property, water solubility, biocompatibility and reduce cytotoxicity of the antibacterial polymer film; at the same time, the antibacterial glass powder and nano titanium dioxide are used to synergistically improve the antioxidant property, mechanical properties, thermal stability and weather resistance of the antibacterial polymer film.

[0024] 2. The antibacterial glass powder in the present invention has a large surface area that is conducive to the release of zinc ions. It is added to the substrate to reduce the inherent microbial sensitivity of polypropylene, effectively prevent bacterial adhesion and eliminate microorganisms, and has good antibacterial properties. It cooperates with nano-titanium dioxide to improve the antibacterial and antioxidant properties of the polymer film, while improving the thermal stability of the polymer film and maintaining its optical transparency. Due to the nucleation effect of the antibacterial glass powder, the introduction of the foreign body surface can reduce the energy barrier of primary nucleation, thereby increasing the crystallization rate of polypropylene and the degree of crystallinity. It cooperates with polyethylene terephthalate to improve the mechanical strength of the polymer film.

[0025] 3. The modified chitosan antibacterial agent added in the present invention firstly grafts butylamine-grafted hydrophobic acrylate-terminated functionalized PEG onto chitosan to improve the antibacterial property, water solubility, biocompatibility and reduce cytotoxicity of the functional chitosan, and then grafts the intermediate product with good antibacterial and antioxidant properties onto the functional chitosan to synergistically improve the antibacterial and antioxidant properties of the polymer film. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 It is a process flow chart of the preparation of the antibacterial polymer film material of the present invention; Figure 2 It is a line graph of the mechanical properties of the antibacterial polymer film material of the present invention; Figure 3 It is a bar graph of the antibacterial property of the antibacterial polymer film material of the present invention. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1 This embodiment discloses a method for preparing an intermediate product, comprising the following steps: 687 g of 4-vinylbenzyl chloride and 1.4 kg of triphenylphosphine were added to 7.5 L of acetone, and magnetically stirred for 48 h in a nitrogen atmosphere. The mixture was cooled to room temperature, and then 10.5 L of petroleum ether was added and filtered. The filter cake was washed four times with petroleum ether and then vacuum dried at room temperature for 24 h to obtain an intermediate product.

[0030] Example 2 This embodiment discloses a method for preparing functionalized polyethylene glycol, comprising the following steps: 500 g of polyethylene glycol diacrylate was added to 2.9 L of water, stirred for 20 min, then 86.6 mL of butylamine and 1.9 L of N,N-dimethylformamide were added, and magnetic stirring was carried out at room temperature for 72 h. After the solvent was removed in vacuo, it was washed with ethyl acetate 4 times, dried in air for 12 h, and further dried under vacuum for 14 h to obtain functionalized polyethylene glycol.

[0031] Example 3 This embodiment discloses a method for preparing a modified chitosan antibacterial agent, comprising the following steps: S1: 150 g chitosan and 17.1 g 1,4-diazabicyclo[2.2.2]octane were added to 7.5 L water, stirred at 400 rpm for 25 min, and then 258 g functionalized polyethylene glycol prepared in Example 2 was added, and the mixture was stirred at 400 rpm for 2 days at room temperature, and then 6 L acetone was added for precipitation, filtered, and washed with acetone for 4 times to obtain functional chitosan; S2: 75 g of functional chitosan was added to 1.4 L of N, N-dimethylformamide, and stirred at 55 ° C for 30 min in a nitrogen atmosphere. After cooling to room temperature, 54.5 g of 2-[dodecylthio(thiocarbonyl)thio]-2-methylpropionic acid, 290 g of N, N'-dicyclohexylcarbodiimide and 5.3 g of 4-dimethylaminopyridine were added, and magnetic stirring was performed at room temperature for 18 h. After cooling in an ice bath for 1 h, vacuum filtration was performed, 1.5 L of ether was added to the filtrate for precipitation, and the filter cake was washed with ether for 4 times to obtain grafted chitosan; S3: 380g of the intermediate product prepared in Example 1, 30g of grafted chitosan, and 0.6g of azobisisobutyronitrile were added to 2.9L N,N-dimethylformamide, and magnetically stirred for 20min. The mixture was reacted at 70°C in a nitrogen atmosphere for 18h. The entire reaction mixture was immersed in liquid nitrogen to quench the reaction. After thawing, 3L of acetone was added to the solution for precipitation. The mixture was vacuum filtered, and the filter cake was washed with acetone 4 times. The filter cake was vacuum dried at 75°C for 16h to obtain a modified chitosan antibacterial agent. Example 4 This embodiment discloses a method for preparing an antibacterial glass powder, comprising the following steps: 52.5g ZnO, 51g SiO2, 3g B2O3, 15g Na2CO3, 13.5g CaCO3 and 15g K2CO3 were mixed in a 3D mixer for 5h to obtain a mixture. The mixture was transferred into a Pt crucible, placed in an electric furnace, heated to 1300°C at a heating rate of 10°C / min, maintained for 1h, poured into a preheated graphite mold, annealed at 550°C for 1h, and then slowly cooled to room temperature to remove thermal residual stress. The mixture was crushed by ball milling and separated by an air classifier to obtain antibacterial glass powder.

[0032] Example 5 See also Figure 1 As shown, this embodiment discloses a method for preparing an antibacterial polymer film material, comprising the following steps: Step (1) 77.5 parts of polypropylene, 36.5 parts of polyethylene terephthalate, 22.5 parts of a compatibility aid, 3.5 parts of a modified chitosan antibacterial agent prepared in Example 3, 9 parts of nano titanium dioxide, 2 parts of an antibacterial glass powder prepared in Example 4, and 0.75 parts of an antioxidant are stirred and mixed at a speed of 200 rpm for 2 hours to obtain a mixed material; Step (2) placing the mixed material in a twin-screw extruder, stirring and mixing evenly, and then casting the mixed material on a casting machine to form an antibacterial polymer film material.

[0033] Among them, the compatibility aid is sodium alginate; the antioxidant is 2,6-di-tert-butyl-p-methylphenol; the temperature of the twin-screw extruder from the feed port to the discharge port are: 180°C, 190°C, 200°C, 210°C, 200°C, 190°C; the extrusion speed is 200r / min; the casting machine traction rate is 200m / min.

[0034] Example 6 See also Figure 1 As shown, this embodiment discloses a method for preparing an antibacterial polymer film material, comprising the following steps: Step (1) 68 parts of polypropylene, 41 parts of polyethylene terephthalate, 15 parts of a compatibility aid, 4 parts of a modified chitosan antibacterial agent prepared in Example 3, 8 parts of nano titanium dioxide, 3 parts of an antibacterial glass powder prepared in Example 4, and 0.5 parts of an antioxidant are stirred and mixed at a speed of 250 rpm for 1.5 hours to obtain a mixed material; Step (2) placing the mixed material in a twin-screw extruder, stirring and mixing evenly, and then casting the mixed material on a casting machine to form an antibacterial polymer film material.

[0035] Among them, the compatibilizer is polyvinyl alcohol; the antioxidant is 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; the temperature of the twin-screw extruder from the feed port to the discharge port is: 180°C, 190°C, 200°C, 210°C, 200°C, 190°C; the extrusion speed is 250r / min; the casting machine traction rate is 150m / min.

[0036] Example 7 See also Figure 1 As shown, this embodiment discloses a method for preparing an antibacterial polymer film material, comprising the following steps: Step (1) 87 parts of polypropylene, 32 parts of polyethylene terephthalate, 30 parts of a compatibility aid, 3 parts of a modified chitosan antibacterial agent prepared in Example 3, 10 parts of nano titanium dioxide, 1 part of an antibacterial glass powder prepared in Example 4, and 1 part of an antioxidant are stirred and mixed at a speed of 150 rpm for 2.5 hours to obtain a mixed material; Step (2) placing the mixed material in a twin-screw extruder, stirring and mixing evenly, and then casting the mixed material on a casting machine to form an antibacterial polymer film material.

[0037] Among them, the compatibilizer is polyethylene glycol; the antioxidant is 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene; the temperatures from the feed port to the discharge port of the twin-screw extruder are: 180°C, 190°C, 200°C, 210°C, 200°C, 190°C; the extrusion speed is 150r / min; the casting machine traction rate is 250m / min.

[0038] Example 8 See also Figure 1 As shown, this embodiment discloses a method for preparing an antibacterial polymer film material, comprising the following steps: Step (1) 70 parts of polypropylene, 38 parts of polyethylene terephthalate, 18 parts of a compatibility aid, 4 parts of a modified chitosan antibacterial agent prepared in Example 3, 8 parts of nano titanium dioxide, 3 parts of an antibacterial glass powder prepared in Example 4, and 0.6 parts of an antioxidant are stirred and mixed at a speed of 220 rpm for 1.8 hours to obtain a mixed material; Step (2) placing the mixed material in a twin-screw extruder, stirring and mixing evenly, and then casting the mixed material on a casting machine to form an antibacterial polymer film material.

[0039] Among them, the compatibility aid is sodium alginate; the antioxidant is 2,6-di-tert-butyl-p-methylphenol; the temperatures from the feed port to the discharge port of the twin-screw extruder are: 180°C, 190°C, 200°C, 210°C, 200°C, 190°C; the extrusion speed is 220r / min; the casting machine traction rate is 170m / min.

[0040] Example 9 See also Figure 1 As shown, this embodiment discloses a method for preparing an antibacterial polymer film material, comprising the following steps: Step (1) 85 parts of polypropylene, 34 parts of polyethylene terephthalate, 28 parts of a compatibility aid, 3 parts of a modified chitosan antibacterial agent prepared in Example 3, 10 parts of nano titanium dioxide, 1 part of an antibacterial glass powder prepared in Example 4, and 0.8 parts of an antioxidant were stirred and mixed at a speed of 170 rpm for 2.2 hours to obtain a mixed material; Step (2) placing the mixed material in a twin-screw extruder, stirring and mixing evenly, and then casting the mixed material on a casting machine to form an antibacterial polymer film material.

[0041] Among them, the compatibilizer is polyethylene glycol; the antioxidant is 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene; the temperatures from the feed port to the discharge port of the twin-screw extruder are: 180°C, 190°C, 200°C, 210°C, 200°C, 190°C; the extrusion speed is 170r / min; the casting machine traction rate is 220m / min.

[0042] Comparative Example 1 Comparative Example 1 Compared with Example 5, in the process of preparing the antibacterial polymer film material in Comparative Example 1, no modified chitosan antibacterial agent was added, and other conditions remained unchanged.

[0043] Comparative Example 2 Comparative Example 2 Compared with Example 5, in the process of preparing the antibacterial polymer film material in Comparative Example 2, zinc oxide is used instead of the antibacterial glass powder, and other conditions remain unchanged.

[0044] Experimental example The performance of the antibacterial polymer film materials prepared in Examples 5-9 and Comparative Examples 1-2 was tested. Tensile strength: tested in accordance with GB / T1040.2-2006 "Plastics-Determination of tensile properties"; antibacterial rate: tested in accordance with GB / T 31402-2015 "Plastics-Test method for antibacterial properties of plastic surfaces". Test bacteria: The bacteria are a mixture of Candida albicans ATCC10231, Staphylococcus aureus ATCC 6538, and Escherichia coli ATCC25922, and the three are added in the same proportion; Antibacterial time-effect test: The antibacterial rate of the obtained plastic film before and after accelerated aging is detected according to the aforementioned method. The accelerated aging test is as follows: the above antibacterial polymer film material is placed in a container at 70℃±3℃ and a freezer at -20℃±3℃ for 3 hours each. After 5 cycles, it is dried under ultraviolet irradiation at an ambient temperature of 22℃±3℃ for 24 hours; the test results are shown in Table 1: Table 1 It can be seen from Table 1 that the antibacterial polymer film materials prepared in Examples 5-9 have good mechanical properties and antibacterial properties. From the comparison between Comparative Example 1 and Example 5, it can be seen that in the process of preparing the antibacterial polymer film material, the modified chitosan antibacterial agent is added to improve the antibacterial property of the antibacterial polymer film material. From the comparison between Comparative Example 2 and Example 5, it can be seen that in the process of preparing the antibacterial polymer film material, the antibacterial glass powder is added to improve the antibacterial property and mechanical properties of the antibacterial polymer film material.

[0045] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

[0046] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. An antibacterial polymer film material, characterized in that: The antibacterial polymer film material specifically comprises the following components by weight: 68-87 parts of polypropylene, 32-41 parts of polyethylene terephthalate, 15-30 parts of a compatibility aid, 3-4 parts of a modified chitosan antibacterial agent, 8-10 parts of nano titanium dioxide, 1-3 parts of antibacterial glass powder, and 0.5-1 part of an antioxidant.

2. The antibacterial polymer film material according to claim 1, characterized in that: The compatibility aid includes at least one of sodium alginate, polyvinyl alcohol and polyethylene glycol.

3. The antibacterial polymer film material according to claim 1, characterized in that: The preparation method of the modified chitosan antibacterial agent comprises the following steps: S1: 100-200 g chitosan and 11.4-22.8 g 1,4-diazabicyclo[2.2.2]octane are added to 5-10 L water, stirred at 300-500 rpm for 20-30 min, 172-340 g functionalized polyethylene glycol is added, and the stirring is continued at 300-500 rpm at room temperature for 1.5-2.5 days, and then 5-7 L acetone is added for precipitation, filtered, and washed with acetone for 3-5 times to obtain functional chitosan; S2: 50-100 g of functional chitosan is added to 0.94-2 L of N,N-dimethylformamide, and stirred at 50-60° C. for 25-35 min in a nitrogen atmosphere. After cooling to room temperature, 36.3-72 g of 2-[dodecylthio(thiocarbonyl)thio]-2-methylpropionic acid, 193-386 g of N,N'-dicyclohexylcarbodiimide and 7.5-15 g of 4-dimethylaminopyridine are added, and magnetic stirring is performed at room temperature for 12-24 h. After cooling in an ice bath for 0.5-1.5 h, vacuum filtration is performed, 1-2 L of ether is added to the filtrate for precipitation, and the filter cake is washed with ether for 3-5 times to obtain grafted chitosan; S3: Add 280-480g of the intermediate product, 20-40g of grafted chitosan, and 0.43-0.8g of azobisisobutyronitrile to 1.9-3.8L N,N-dimethylformamide, stir magnetically for 15-25min, react at 65-75°C in a nitrogen atmosphere for 16-20h, immerse the entire reaction in liquid nitrogen to quench the reaction, and after thawing, add 2-4L of acetone to the solution for precipitation, vacuum filter, wash the filter cake with acetone 3-5 times, and vacuum dry at 70-80°C for 12-20h to obtain a modified chitosan antibacterial agent.

4. The antibacterial polymer film material according to claim 3, characterized in that: The method for preparing the intermediate product comprises the following steps: 458-916 g of 4-vinylbenzyl chloride and 0.95-1.9 kg of triphenylphosphine are added to 5-10 L of acetone, and magnetically stirred for 36-54 h in a nitrogen atmosphere, and then cooled to room temperature. Then 7-15 L of petroleum ether is added, and the mixture is filtered. The filter cake is washed with petroleum ether for 3-5 times, and then vacuum dried at room temperature for 20-28 h to obtain an intermediate product.

5. The antibacterial polymer film material according to claim 3, characterized in that: The method for preparing the functionalized polyethylene glycol comprises the following steps: Add 400-600 g of polyethylene glycol diacrylate to 2.5-3.8 L of water, stir for 15-25 min, then add 69.2-104 mL of butylamine and 1.5-2.2 L of N,N-dimethylformamide, stir magnetically at room temperature for 70-74 h, remove the solvent in vacuo, wash with ethyl acetate 3-5 times, dry in air for 10-14 h, and further dry under vacuum for 12-16 h to obtain functionalized polyethylene glycol.

6. The antibacterial polymer film material according to claim 1, characterized in that: The antioxidant includes at least one of 2,6-di-tert-butyl-p-methylphenol, 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene.

7. The antibacterial polymer film material according to claim 1, characterized in that: The method for preparing the antibacterial glass powder comprises the following steps: 35-70g ZnO, 34-68g SiO2, 2-4g B2O3, 10-20g Na2CO3, 9-18g CaCO3 and 10-20g K2CO3 are mixed in a 3D mixer for 4-6h to obtain a mixture, and the mixture is transferred into a Pt crucible, placed in an electric furnace, heated to 1250-1350°C at a heating rate of 8-12°C / min, maintained for 0.5-1.5h, poured into a preheated graphite mold, annealed at 500-600°C for 0.5-1.5h, and then slowly cooled to room temperature to remove thermal residual stress, crushed by ball milling, and separated by an air classifier to obtain antibacterial glass powder.

8. A method for preparing the antibacterial polymer film material according to any one of claims 1 to 7, characterized in that: The steps include: Step (1) 68-87 parts of polypropylene, 32-41 parts of polyethylene terephthalate, 15-30 parts of a compatibility aid, 3-4 parts of a modified chitosan antibacterial agent, 8-10 parts of nano titanium dioxide, 1-3 parts of antibacterial glass powder, and 0.5-1 part of an antioxidant are stirred and mixed at a speed of 150-250 rpm for 1.5-2.5 hours to obtain a mixed material; Step (2) placing the mixed material in a twin-screw extruder, stirring and mixing evenly, and then casting the mixed material on a casting machine to form an antibacterial polymer film material.

9. The method for preparing the antibacterial polymer film material according to claim 8, characterized in that: The temperatures of the twin-screw extruder from the feed port to the discharge port are 180°C, 190°C, 200°C, 210°C, 200°C, and 190°C respectively; the extrusion speed is 150-250r / min; and the traction rate of the casting machine is 150-250m / min.

Citation Information

Patent Citations

  • Antibacterial thermoplastic plastic composition and preparation method thereof

    CN103627197A

  • Oil-proof and antibacterial food packaging film

    CN109135209A

  • High polymer material with antibacterial function and preparation method thereof

    CN112980091A

  • Low-temperature-resistant polypropylene film and preparation method thereof

    CN115232402A

  • Antibacterial and antiviral plastic film as well as preparation method and application thereof