Antistatic nylon plastic and preparation method thereof

By blending epoxidized polyaniline and aminated silver powder with nylon, a conductive network is constructed, which solves the problem of reduced performance of antistatic nylon plastics, improves antistatic and antibacterial properties, and enhances overall performance.

CN118725558AInactive Publication Date: 2024-10-01SUZHOU SAIRONG CONSTITUTION&DECORATION ENG CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410767678.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing antistatic nylon plastics have reduced antistatic properties due to compatibility and migration problems, poor impact properties and tensile properties, and need to add a large amount of antistatic agents with polar components to cause internal pore problems.

Method used

Epoxidized polyaniline and aminated silver powder are blended with modified nylon, grafted with conductive groups to build a conductive network, combined with lubricants and antioxidants, and extruded and granulated to form antistatic nylon plastic.

Benefits of technology

Significantly improves the antistatic and antibacterial properties of nylon plastic, improves conductivity, enhances the overall performance of the plastic, reduces the amount of antistatic agent used, and avoids compatibility and pore problems.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an antistatic nylon plastic and a preparation method thereof, and relates to the technical field of plastics. The preparation method comprises the following steps: polymerizing 4-(aminomethyl)-3-chloroaniline to form a conductive polyaniline compound, carrying out ring-opening and ring-closing reaction on aminomethyl and epoxy chloropropane to form epoxidized polyaniline, and carrying out blending modification on the epoxidized polyaniline, aminated silver powder and nylon to obtain the conductive silver / nylon composite material. The group of the epoxidized polyaniline is subjected to chemical end-capping and coupling chain extension reaction with the carboxyl-terminated group and amino-terminated group of the nylon, so that the conductive group is grafted into the molecular chain of the nylon, the conductivity of the nylon is greatly improved, and the antistatic capacity of the nylon plastic is further improved; the silver powder is modified by N, N-dimethyl aminopropyl (triethoxy) silane, so that the dispersity of the silver powder is greatly improved, the silver powder is further uniformly dispersed in nylon, a conductive network is constructed by the silver powder and conductive polyaniline, and the antistatic property of the nylon plastic is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastics, in particular to an antistatic nylon plastic and a preparation method thereof. Background Art

[0002] In the prior art, antistatic agents are usually blended with nylon for modification, thereby giving the modified nylon plastic particles antistatic properties. However, there are generally compatibility and mobility problems; and in order to produce antistatic properties, a conductive network needs to be formed inside the plastic particles, so generally a large amount of antistatic agents needs to be added. Since antistatic agents generally contain polar components, when a large amount of antistatic agents are introduced, there are firstly agglomeration problems caused by compatibility, and secondly, there are internal pore problems caused by polar components, which reduces the interface effect between the antistatic agent and nylon, thereby causing the impact and tensile properties of the plastic particles to decrease. Summary of the invention

[0003] The purpose of the present invention is to provide an antistatic nylon plastic and a preparation method thereof to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: an antistatic nylon plastic, wherein the antistatic nylon plastic is made of modified nylon, a lubricant and an antioxidant.

[0005] Furthermore, the modified nylon is prepared from nylon PA66, epoxidized polyaniline and amination silver powder.

[0006] Furthermore, the epoxidized polyaniline is prepared by polymerizing 4-(aminomethyl)-3-chloroaniline and then reacting it with epichlorohydrin for ring opening and ring closing reactions.

[0007] Furthermore, the amination silver powder is prepared from silver powder and 3-N,N-dimethylaminopropyl (triethoxy) silane.

[0008] A method for preparing antistatic nylon plastic comprises the following preparation steps:

[0009] (1) 4-(aminomethyl)-3-chloroaniline and hydrochloric acid are mixed in a mass ratio of 1:12-13, stirred to dissolve, stirred in an ice water bath at 60 rpm for 50 min, and then an aqueous ammonium persulfate solution is added, wherein the mass ratio of 4-(aminomethyl)-3-chloroaniline to ammonium persulfate is 1:0.03-0.05, and the reaction is continued for 24 h. The filter cake is washed with hydrochloric acid until the filtrate is colorless, and then washed with double distilled water for 4-6 times, and then dried at 65° C. for 24 h to obtain a polyaniline compound;

[0010] (2) A polyaniline compound and anhydrous ethanol are mixed in a ratio of 3.5 to 4.4 g:50 mL, and under a nitrogen atmosphere, 0.01 to 0.1 times the mass of the polyaniline compound is added with benzyltriethylammonium chloride, the temperature is raised to 65° C., 3.5 to 4.0 times the mass of the polyaniline compound is added with epichlorohydrin and 9 to 10 times the mass of the polyaniline compound is added with anhydrous ethanol, and the reaction is continued for 30 minutes, and then a 40% sodium hydroxide aqueous solution is added, the temperature is lowered to 50° C., and the reaction is continued for 1 to 1.5 hours, and the filtrate is collected by suction, and the liquid is separated by extraction with toluene, and the upper layer is collected, and then dried with anhydrous magnesium sulfate for 2 to 4 hours, and the filtrate is collected by suction, and dried to constant weight at 50° C. and a vacuum degree of -0.06 MPa to obtain epoxidized polyaniline;

[0011] (3) 3-N,N-dimethylaminopropyl (triethoxy) silane, anhydrous ethanol and deionized water are mixed uniformly, and the pH is adjusted to 3-4 with acetic acid to obtain a silane solution; the silane solution is added to a 10% by mass silver powder / ethanol dispersion, 3-N,N-dimethylaminopropyl (triethoxy) silane accounts for 1-7% by mass of the silver powder, ultrasonic dispersion is performed at 30kHz for 2h, the supernatant is removed by centrifugation, and the mixture is placed in an oven at 150°C for dehydration for 2h, and then ultrasonically cleaned with 90°C water and anhydrous ethanol at 30kHz for 30min, and dried in an oven at 80°C for 24h to obtain an amination silver powder;

[0012] (4) mixing nylon PA66, epoxidized polyaniline, and amide silver powder in a mass ratio of 100:2-8:2-8, and extruding and granulating the mixture at 260-285° C. through a twin-screw extruder to obtain modified nylon;

[0013] (5) The modified nylon, lubricant and antioxidant are mixed in a mass ratio of 30:1-2:1-3 and extruded and granulated at 190-225° C. to obtain an antistatic nylon plastic.

[0014] Furthermore, the concentration of hydrochloric acid in step (1) is 0.5 to 2 mol / L.

[0015] Furthermore, the concentration of the ammonium persulfate aqueous solution in step (1) is 0.1 to 0.3 g / mL.

[0016] Furthermore, in step (2), the mass ratio of the polyaniline compound to sodium hydroxide is 1:1.5-2.0.

[0017] Furthermore, in step (3), the ratio of 3-N,N-dimethylaminopropyl (triethoxy) silane, anhydrous ethanol and deionized water is 2g:95mL:5mL.

[0018] Furthermore, the lubricant in step (5) is at least one of talc, polyethylene wax and calcium stearate; and the antioxidant is one or more of hindered phenol antioxidant 1010, antioxidant 1098 and phosphite.

[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0020] The invention adopts epoxidized polyaniline, amide silver powder and nylon for blending and modification to obtain modified nylon with antistatic and antibacterial properties, and then extrude and granulate to form nylon plastic.

[0021] The present invention first polymerizes 4-(aminomethyl)-3-chloroaniline to form a conductive polyaniline compound, then uses aminomethyl and epichlorohydrin to perform ring-opening and ring-closing reactions to form epoxidized polyaniline, and then blends and modifies the epoxidized polyaniline with amination silver powder and nylon. The groups of epoxidized polyaniline react with the terminal carboxyl groups and terminal amino groups of nylon to undergo chemical end-capping and coupling chain extension reactions, thereby allowing the conductive groups to be grafted into the nylon molecular chain, greatly improving the conductive properties of the nylon itself, and further improving the antistatic ability of the nylon plastic. The silver powder is subjected to 3-N,N- The dimethylaminopropyl (triethoxy) silane modification treatment greatly improves the dispersibility of silver powder, which is then evenly dispersed inside the nylon and constructs a conductive network together with conductive polyaniline to improve the antistatic properties of nylon plastics. At the same time, the excellent antibacterial properties of the silver powder itself can also improve the antibacterial properties of nylon plastics. In addition, the chlorine group of epoxidized polyaniline and the dimethylamine of the amination silver powder form a quaternary ammonium structure, which works together with the silver powder to improve the antibacterial properties of nylon plastics. At the same time, the cationization of the quaternary ammonium structure can also greatly improve the antistatic properties of nylon plastics. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe the method in detail. The test methods for various indicators of the nylon plastics prepared in the following examples are as follows:

[0024] Antistatic: The plastics prepared in the examples and comparative examples were injection molded into sheets. Referring to GB / T1410, a 10 cm × 10 cm × 1 mm sheet was taken and its volume resistivity was measured using a volume surface resistivity meter at a temperature of 23°C and a relative humidity of 33%.

[0025] Example 1

[0026] (1) 4-(aminomethyl)-3-chloroaniline and 0.5 mol / L hydrochloric acid were mixed in a mass ratio of 1:12, stirred to dissolve, and then stirred in an ice water bath at 60 rpm for 50 min, and then 0.1 g / mL of ammonium persulfate aqueous solution was added, and the mass ratio of 4-(aminomethyl)-3-chloroaniline to ammonium persulfate was 1:0.03. The reaction was continued for 24 h, and then filtered, and the filter cake was washed with hydrochloric acid until the filtrate was colorless, and then washed with double distilled water for 4 times, and then dried at 65° C. for 24 h to obtain a polyaniline compound;

[0027] (2) A polyaniline compound and anhydrous ethanol were mixed in a ratio of 3.5 g:50 mL, and under a nitrogen atmosphere, 0.01 times the mass of the polyaniline compound was added with benzyltriethylammonium chloride, the temperature was raised to 65° C., 3.5 times the mass of the polyaniline compound was added with epichlorohydrin and 9 times the mass of the polyaniline compound was added with anhydrous ethanol, and the reaction lasted for 30 minutes. Then, a 40% sodium hydroxide aqueous solution was added, and the mass ratio of the polyaniline compound to the sodium hydroxide was 1:1.5. The temperature was lowered to 50° C., and after the reaction lasted for 1 hour, the filtrate was filtered out, and the liquid was separated by extraction with toluene. The upper layer was taken, and then dried with anhydrous magnesium sulfate for 2 hours. The filtrate was filtered out, and dried to constant weight at 50° C. and a vacuum degree of -0.06 MPa to obtain epoxidized polyaniline;

[0028] (3) 3-N,N-dimethylaminopropyl (triethoxy) silane, anhydrous ethanol and deionized water are mixed in a ratio of 2g:95mL:5mL, and the pH is adjusted to 3 with acetic acid to obtain a silane solution; the silane solution is added to a silver powder / ethanol dispersion having a mass fraction of 10%, wherein the 3-N,N-dimethylaminopropyl (triethoxy) silane accounts for 1% of the mass fraction of the silver powder, and the dispersion is ultrasonically dispersed at 30kHz for 2h, the supernatant is removed by centrifugation, and the mixture is placed in an oven at 150°C for dehydration for 2h, and then ultrasonically cleaned with 90°C water and anhydrous ethanol at 30kHz for 30min, and dried in an oven at 80°C for 24h to obtain an amination silver powder;

[0029] (4) mixing nylon PA66, epoxidized polyaniline and amide silver powder in a mass ratio of 100:2:2, and extruding and granulating the mixture at 260-285° C. through a twin-screw extruder to obtain modified nylon;

[0030] (5) Modified nylon, talcum powder and hindered phenol antioxidant 1010 are mixed in a mass ratio of 30:1:1 and extruded and granulated at 190-225° C. to obtain antistatic nylon plastic.

[0031] Example 2

[0032] (1) 4-(aminomethyl)-3-chloroaniline and 1.2 mol / L hydrochloric acid were mixed in a mass ratio of 1:12.5, stirred to dissolve, and then stirred in an ice water bath at 60 rpm for 50 min, and then 0.2 g / mL of ammonium persulfate aqueous solution was added, and the mass ratio of 4-(aminomethyl)-3-chloroaniline to ammonium persulfate was 1:0.04. The reaction was continued for 24 h, and then filtered, and the filter cake was washed with hydrochloric acid until the filtrate was colorless, and then washed with double distilled water for 5 times, and then dried at 65° C. for 24 h to obtain a polyaniline compound;

[0033] (2) A polyaniline compound and anhydrous ethanol were mixed in a ratio of 4.0 g:50 mL, and under a nitrogen atmosphere, 0.08 times the mass of the polyaniline compound was added with benzyltriethylammonium chloride, the temperature was raised to 65° C., 3.8 times the mass of the polyaniline compound was added with epichlorohydrin and 9.5 times the mass of the polyaniline compound was added with anhydrous ethanol, and the reaction lasted for 30 min. Then, a 40% sodium hydroxide aqueous solution was added, and the mass ratio of the polyaniline compound to the sodium hydroxide was 1:1.6. The temperature was lowered to 50° C., and the reaction lasted for 1.2 h. The filtrate was filtered and separated by extraction with toluene, the upper layer was taken, and then dried with anhydrous magnesium sulfate for 3 h. The filtrate was filtered and dried to constant weight at 50° C. and a vacuum degree of -0.06 MPa to obtain epoxidized polyaniline;

[0034] (3) 3-N,N-dimethylaminopropyl (triethoxy) silane, anhydrous ethanol and deionized water were mixed in a ratio of 2g:95mL:5mL, and the pH was adjusted to 3.5 with acetic acid to obtain a silane solution; the silane solution was added to a silver powder / ethanol dispersion with a mass fraction of 10%, 3-N,N-dimethylaminopropyl (triethoxy) silane accounting for 4% of the mass fraction of the silver powder, and ultrasonic dispersion was performed at 30kHz for 2h, and the supernatant was removed by centrifugation, and the mixture was placed in an oven at 150°C for dehydration for 2h, and then ultrasonically cleaned with 90°C water and anhydrous ethanol at 30kHz for 30min, and dried in an oven at 80°C for 24h to obtain an amination silver powder;

[0035] (4) Nylon PA66, epoxidized polyaniline, and amide silver powder are uniformly mixed in a mass ratio of 100:5:5, and extruded and granulated at 260-285° C. using a twin-screw extruder to obtain modified nylon;

[0036] (5) Modified nylon, polyethylene wax and antioxidant 1098 are mixed in a mass ratio of 30:1.5:2 and extruded and granulated at 190-225° C. to obtain antistatic nylon plastic.

[0037] Example 3

[0038] (1) 4-(aminomethyl)-3-chloroaniline and 2 mol / L hydrochloric acid were mixed in a mass ratio of 1:13, stirred to dissolve, and then stirred in an ice water bath at 60 rpm for 50 min, and then 0.3 g / mL of ammonium persulfate aqueous solution was added, and the mass ratio of 4-(aminomethyl)-3-chloroaniline to ammonium persulfate was 1:0.05. The reaction was continued for 24 h, and then filtered, and the filter cake was washed with hydrochloric acid until the filtrate was colorless, and then washed with double distilled water for 6 times, and then dried at 65° C. for 24 h to obtain a polyaniline compound;

[0039] (2) A polyaniline compound and anhydrous ethanol were mixed in a ratio of 4.4 g:50 mL, and under a nitrogen atmosphere, 0.1 times the mass of the polyaniline compound was added with benzyltriethylammonium chloride, the temperature was raised to 65° C., 4.0 times the mass of the polyaniline compound was added with epichlorohydrin and 10 times the mass of the polyaniline compound was added with anhydrous ethanol, and the reaction lasted for 30 minutes. Then, a 40% sodium hydroxide aqueous solution was added, and the mass ratio of the polyaniline compound to sodium hydroxide was 1:2.0. The temperature was lowered to 50° C., and the reaction lasted for 1.5 hours. The filtrate was filtered and separated by extraction with toluene, the upper layer was taken, and then dried with anhydrous magnesium sulfate for 4 hours. The filtrate was filtered and dried to constant weight at 50° C. and a vacuum degree of -0.06 MPa to obtain epoxidized polyaniline;

[0040] (3) 3-N,N-dimethylaminopropyl (triethoxy) silane, anhydrous ethanol and deionized water were mixed in a ratio of 2g:95mL:5mL, and the pH was adjusted to 4 with acetic acid to obtain a silane solution; the silane solution was added to a silver powder / ethanol dispersion with a mass fraction of 10%, 3-N,N-dimethylaminopropyl (triethoxy) silane accounting for 7% of the mass fraction of the silver powder, and ultrasonic dispersion was performed at 30kHz for 2h, and the supernatant was removed by centrifugation, and the mixture was placed in an oven at 150°C for dehydration for 2h, and then ultrasonically cleaned with 90°C water and anhydrous ethanol at 30kHz for 30min, and dried in an oven at 80°C for 24h to obtain an amination silver powder;

[0041] (4) Nylon PA66, epoxidized polyaniline, and amide silver powder are uniformly mixed in a mass ratio of 100:8:8, and extruded and granulated at 260-285° C. using a twin-screw extruder to obtain modified nylon;

[0042] (5) Modified nylon, calcium stearate and phosphite are mixed in a mass ratio of 30:2:3 and extruded and granulated at 190-225° C. to obtain antistatic nylon plastic.

[0043] Comparative Example 1

[0044] The difference between Comparative Example 1 and Example 2 is that epichlorohydrin is not added, and the remaining steps are the same as Example 2.

[0045] Comparative Example 2

[0046] The difference between Comparative Example 2 and Example 2 is that 4-(aminomethyl)-3-chloroaniline is not added, and the remaining steps are the same as Example 2.

[0047] Comparative Example 3

[0048] The difference between Comparative Example 3 and Example 2 is that the silver powder is not subjected to 3-N,N-dimethylaminopropyl (triethoxy) silane modification treatment, and the remaining steps are the same as Example 2.

[0049] Comparative Example 4

[0050] The difference between Comparative Example 4 and Example 2 is that no amide silver powder is added, and the remaining steps are the same as Example 2.

[0051] Effect example

[0052] Table 1 below shows the performance analysis results of the nylon plastics of Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.

[0053] Table 1

[0054] Volume resistivity (Ω·cm) Example 1 <![CDATA[0.53×10 6 ]]> Example 2 <![CDATA[0.51×10 6 ]]> Example 3 <![CDATA[0.51×10 6 ]]> Comparative Example 1 <![CDATA[0.63×10 6 ]]> Comparative Example 2 <![CDATA[0.82×10 6 ]]> Comparative Example 3 <![CDATA[0.61×10 6 ]]> Comparative Example 4 <![CDATA[0.72×10 6 ]]>

[0055] The invention first polymerizes 4-(aminomethyl)-3-chloroaniline to form a conductive polyaniline compound, then uses aminomethyl to react with epichlorohydrin to perform ring-opening and ring-closing reactions, thereby forming epoxidized polyaniline, which is then mixed with amination silver powder and nylon for modification. The groups of the epoxidized polyaniline react with the terminal carboxyl groups and terminal amino groups of the nylon for chemical termination and coupling chain extension reactions, thereby allowing the conductive groups to be grafted into the nylon molecular chain, greatly improving the conductive performance of the nylon itself, thereby improving the antistatic ability of the nylon plastic, and the silver powder is modified by 3-N,N-dimethylaminopropyl (triethoxy) silane, thereby greatly improving the dispersibility of the silver powder, thereby uniformly dispersing the silver powder inside the nylon, and constructing a conductive network together with the conductive polyaniline, thereby improving the antistatic property of the nylon plastic, and in addition, the chlorine groups of the epoxidized polyaniline and the dimethylamine of the amination silver powder form a quaternary ammonium structure, and the cationization thereof can also greatly improve the antistatic property of the nylon plastic.

[0056] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. An antistatic nylon plastic, characterized in that: The antistatic nylon plastic is prepared from modified nylon, lubricant and antioxidant.

2. The antistatic nylon plastic according to claim 1, characterized in that: The modified nylon is prepared from nylon PA66, epoxidized polyaniline and amination silver powder.

3. The antistatic nylon plastic according to claim 2, characterized in that: The epoxidized polyaniline is prepared by polymerizing 4-(aminomethyl)-3-chloroaniline and then reacting it with epichlorohydrin for ring opening and ring closing reactions.

4. The antistatic nylon plastic according to claim 2, characterized in that: The amination silver powder is prepared from silver powder and 3-N,N-dimethylaminopropyl (triethoxy) silane.

5. A method for preparing antistatic nylon plastic, characterized in that: The method comprises the following preparation steps: (1) 4-(aminomethyl)-3-chloroaniline and hydrochloric acid are mixed in a mass ratio of 1:12-13, stirred to dissolve, stirred in an ice water bath at 60 rpm for 50 min, and then an aqueous ammonium persulfate solution is added, wherein the mass ratio of 4-(aminomethyl)-3-chloroaniline to ammonium persulfate is 1:0.03-0.05, and the reaction is continued for 24 h. The filter cake is washed with hydrochloric acid until the filtrate is colorless, and then washed with double distilled water for 4-6 times, and then dried at 65° C. for 24 h to obtain a polyaniline compound; (2) A polyaniline compound and anhydrous ethanol are mixed in a ratio of 3.5 to 4.4 g:50 mL, and under a nitrogen atmosphere, 0.01 to 0.1 times the mass of the polyaniline compound is added with benzyltriethylammonium chloride, the temperature is raised to 65° C., 3.5 to 4.0 times the mass of the polyaniline compound is added with epichlorohydrin and 9 to 10 times the mass of the polyaniline compound is added with anhydrous ethanol, and the reaction is continued for 30 minutes, and then a 40% sodium hydroxide aqueous solution is added, the temperature is lowered to 50° C., and the reaction is continued for 1 to 1.5 hours, and the filtrate is collected by suction, and the liquid is separated by extraction with toluene, and the upper layer is collected, and then dried with anhydrous magnesium sulfate for 2 to 4 hours, and the filtrate is collected by suction, and dried to constant weight at 50° C. and a vacuum degree of -0.06 MPa to obtain epoxidized polyaniline; (3) 3-N,N-dimethylaminopropyl (triethoxy) silane, anhydrous ethanol and deionized water are mixed uniformly, and the pH is adjusted to 3-4 with acetic acid to obtain a silane solution; the silane solution is added to a 10% by mass silver powder / ethanol dispersion, 3-N,N-dimethylaminopropyl (triethoxy) silane accounts for 1-7% by mass of the silver powder, ultrasonic dispersion is performed at 30kHz for 2h, the supernatant is removed by centrifugation, and the mixture is placed in an oven at 150°C for dehydration for 2h, and then ultrasonically cleaned with 90°C water and anhydrous ethanol at 30kHz for 30min, and dried in an oven at 80°C for 24h to obtain an amination silver powder; (4) mixing nylon PA66, epoxidized polyaniline, and amide silver powder in a mass ratio of 100:2-8:2-8, and extruding and granulating the mixture at 260-285° C. through a twin-screw extruder to obtain modified nylon; (5) The modified nylon, lubricant and antioxidant are mixed in a mass ratio of 30:1-2:1-3 and extruded and granulated at 190-225° C. to obtain an antistatic nylon plastic.

6. The method for preparing an antistatic nylon plastic according to claim 5, characterized in that: The concentration of hydrochloric acid in step (1) is 0.5-2 mol / L.

7. The method for preparing an antistatic nylon plastic according to claim 5, characterized in that: The concentration of the ammonium persulfate aqueous solution in step (1) is 0.1-0.3 g / mL.

8. The method for preparing an antistatic nylon plastic according to claim 5, characterized in that: The mass ratio of the polyaniline compound to sodium hydroxide in step (2) is 1:1.5-2.

0.

9. The method for preparing an antistatic nylon plastic according to claim 5, characterized in that: In step (3), the ratio of 3-N,N-dimethylaminopropyl (triethoxy) silane, anhydrous ethanol and deionized water is 2g:95mL:5mL.

10. The method for preparing an antistatic nylon plastic according to claim 5, characterized in that: In step (5), the lubricant is at least one of talc, polyethylene wax and calcium stearate; and the antioxidant is one or more of hindered phenol antioxidant 1010, antioxidant 1098 and phosphite.

Citation Information

Patent Citations

  • Acidified polyaniline-doped conductive nylon material and preparation method thereof

    CN109401289A

  • Antistatic ABS (Acrylonitrile Butadiene Styrene) composite plastic particle and preparation method thereof

    CN115975334A

  • ABS (Acrylonitrile Butadiene Styrene) antistatic plastic based on graphene modification and preparation process thereof

    CN117844167A