Method for improving compatibility of desulfurized rubber modified asphalt

By using the synergistic effect of rare earth stearate and linoleic acid in desulfurized rubber-modified asphalt, the problem of insufficient compatibility of modified asphalt is solved, the high-temperature stability and low-temperature crack resistance of the material are significantly improved, and the material is simplified. process and reduces phase separation.

CN118725591APending Publication Date: 2024-10-01TIANJIN CHENGJIAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410841630.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing modified asphalt materials have deficiencies in compatibility, especially the low rubber content and poor construction ease. Moreover, the introduced third component may produce toxic gases during the reaction process or affect the high and low temperatures of the material. Performance and durability.

Method used

Using the synergistic effect of rare earth stearate and linoleic acid, by adding rare earth stearate and linoleic acid to the desulfurized rubber modified asphalt, the compatibility is improved through the mixing and shearing process, and the phase separation phenomenon is significantly reduced.

Benefits of technology

Significantly improves the compatibility of devulcanized rubber-modified asphalt, enhances high-temperature stability, rutting resistance and low-temperature crack resistance, reduces total heat absorption, and simplifies the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725591A_ABST
    Figure CN118725591A_ABST
Patent Text Reader

Abstract

The invention provides a method for improving the compatibility of desulfurized rubber modified asphalt, which adopts rare earth stearate and linoleic acid to synergistically improve the compatibility of desulfurized rubber modified asphalt, and comprises the following steps: firstly, adding linoleic acid into desulfurized rubber, uniformly stirring at room temperature, standing for 2 hours, then heating matrix asphalt to 165-175 DEG C in a reaction tank, and stirring for 2 hours; adding the desulfurized rubber and the rare earth stearate into a reaction tank, and shearing at the shearing rate of 3000r / min for 30-50 minutes, so as to obtain the desulfurized rubber modified asphalt. The method is simple in process, the purpose of remarkably reducing the phase separation phenomenon can be achieved, and the compatibility improvement effect is remarkable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of modified asphalt, and in particular to a method for improving the compatibility of desulfurized rubber modified asphalt. Background Art

[0002] The application of rubber asphalt pavement can not only improve the road performance, but also solve the problem of recycling waste tires. Although rubber asphalt road materials have advantages in high temperature stability, low temperature crack resistance, fatigue performance and anti-aging performance, there are still problems such as low rubber content, poor construction and workability. Among them, compatibility is the core problem restricting rubber modified asphalt. At present, the main method to improve the compatibility of rubber modified asphalt is to introduce a third component, but it also faces some problems, such as the introduction of components The reaction process will produce toxic gases, or have a negative impact on the high temperature and low temperature performance and durability of the modified asphalt. Summary of the invention

[0003] The purpose of the present invention is to provide a method for improving the compatibility of desulfurized rubber modified asphalt, using rare earth stearate and linoleic acid to synergistically improve the compatibility of desulfurized rubber modified asphalt. The method has a simple process, can achieve the purpose of significantly reducing the phase separation phenomenon, and has a significant compatibility improvement effect.

[0004] The technical solution adopted by the present invention is: a method for improving the compatibility of desulfurized rubber modified asphalt, the desulfurized rubber modified asphalt includes the following components in parts by weight: 100 parts of base asphalt, 25-100 parts of desulfurized rubber, 2-16 parts of linoleic acid, 0.2-2.4 parts of rare earth stearate, and the rare earth stearate is a mixture of one or both of cerium stearate and lanthanum stearate.

[0005] A method for improving the compatibility of desulfurized rubber modified asphalt comprises the following steps:

[0006] Step 1: Accurately weigh each component;

[0007] Step 2, adding linoleic acid to the devulcanized rubber, stirring evenly at room temperature, and letting it stand for 2 hours;

[0008] Step three, heating the base asphalt to 165-175° C. in a reaction tank, adding the desulfurized rubber and rare earth stearate obtained in step two into the reaction tank for shearing for 30-50 minutes at a shear rate of 3000 r / min to obtain desulfurized rubber modified asphalt.

[0009] The sol content of the devulcanized rubber is greater than 70%.

[0010] The devulcanized rubber is a granular material produced by extrusion granulation.

[0011] The present invention has the following positive effects compared with the prior art:

[0012] 1. Rare earth stearate can reduce the total heat absorption of desulfurized rubber modified asphalt, significantly reduce the phase separation phenomenon, and the addition of rare earth stearate can improve the high temperature stability and anti-rutting performance of desulfurized rubber modified asphalt.

[0013] 2. Linoleic acid increases the light components of modified asphalt and provides active functional groups. It contains unsaturated carbon-carbon double bonds and carboxyl active groups that can react chemically or physically adsorb with the functional groups on the surface of rubber particles and the active functional groups in asphalt, increasing the adhesion and interaction between them, thereby improving the compatibility between rubber particles and matrix asphalt. In addition, the addition of linoleic acid improves the low-temperature crack resistance and deformation resistance of desulfurized rubber modified asphalt.

[0014] 3. Rare earth stearate and linoleic acid are used to synergistically improve the compatibility of desulfurized rubber modified asphalt. The process is simple and the effect is significant. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Attached Figure 1 This is an optical microscope image of the desulfurized rubber modified asphalt of Example 3.

[0016] Attached Figure 2 This is an optical microscope image of the desulfurized rubber modified asphalt of the comparative example. DETAILED DESCRIPTION

[0017] The present invention will be further explained below in conjunction with specific implementation modes. It should be understood that the following specific implementation modes are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0018] Example 1: A method for improving the compatibility of desulfurized rubber modified asphalt, the steps are as follows:

[0019] Step 1, weighing a certain weight of base asphalt, desulfurized rubber, linoleic acid, and cerium stearate, wherein the physical indicators of the base asphalt are: needle penetration (25°C) is 68.9 mm, softening point is 48.9°C, ductility (5°C) is 20.45 cm, dynamic viscosity (135°C) is 241 Pa·s, the sol content of desulfurized rubber is 72%, and the weight ratio of the base asphalt, desulfurized rubber, linoleic acid and cerium stearate is controlled to be 100:50:4:0.5;

[0020] Step 2, adding the weighed linoleic acid to the devulcanized rubber, stirring evenly at room temperature, and letting it stand for 2 hours;

[0021] Step three, heating the base asphalt to 165° C. in a reaction tank, adding the desulfurized rubber and cerium stearate obtained in step two into the reaction tank for shearing for 35 minutes at a shear rate of 3000 r / min to obtain desulfurized rubber modified asphalt.

[0022] The desulfurized rubber modified asphalt prepared in Example 1 was subjected to adhesion test and solubility test. The adhesion performance between modified asphalt and aggregate was evaluated by boiling method. The specific method is as follows: select stones with a shape similar to that of a cube, bind them with iron wire and then dry them. Then, heat the modified asphalt to a flowable state, immerse the stones, ensure that the asphalt completely covers the stones, lift and hang them on the iron frame, and record the mass of the modified asphalt before and after coating. Solubility test method: Place glass fiber filter paper at the bottom of a clean Gooch crucible. Next, weigh 2 mg of modified asphalt sample, gradually add 100 ml of trichloroethylene until the sample is completely dissolved, cover the bottle cap and let it stand at room temperature for at least 15 minutes. Then, transfer all insolubles to the crucible, and use a solvent to wash the filter paper until the filtrate becomes colorless and transparent. Finally, calculate the percentage of soluble components in the modified asphalt.

[0023] Example 2: A method for improving the compatibility of desulfurized rubber modified asphalt. The steps are as follows:

[0024] Step 1, weighing a certain mass of base asphalt, desulfurized rubber, linoleic acid, and lanthanum stearate, the properties of the base asphalt and the desulfurized rubber are the same as those in Example 1, and controlling the weight ratio of the base asphalt, desulfurized rubber, linoleic acid, and lanthanum stearate to be 100:50:6:0.5;

[0025] Step 2, adding the weighed linoleic acid to the devulcanized rubber, stirring evenly at room temperature, and letting it stand for 2 hours;

[0026] Step three, heating the base asphalt to 165° C. in a reaction tank, adding the desulfurized rubber and lanthanum stearate obtained in step two into the reaction tank for shearing for 40 minutes at a shear rate of 3000 r / min to obtain desulfurized rubber modified asphalt.

[0027] The adhesion test and solubility test were performed on Example 2 using the same test method as Example 1. The test results are shown in Table 1.

[0028] Example 3: A method for improving the compatibility of desulfurized rubber modified asphalt. The steps are as follows:

[0029] Step 1, weighing a certain mass of base asphalt, desulfurized rubber, linoleic acid, and cerium stearate, the properties of the base asphalt and the desulfurized rubber are the same as those in Example 1, and controlling the weight ratio of the base asphalt, desulfurized rubber, linoleic acid, and cerium stearate to be 100:50:6:1;

[0030] Step 2, adding the weighed linoleic acid to the devulcanized rubber, stirring evenly at room temperature, and letting it stand for 2 hours;

[0031] Step 3: heat the base asphalt to 165° C. in a reaction tank, add the desulfurized rubber and cerium stearate obtained in step 2 into the reaction tank and shear for 40 minutes at a shear rate of 3000 r / min to obtain desulfurized rubber modified asphalt;

[0032] The adhesion test and solubility test were performed on Example 3. The test methods were the same as those of Example 1. The test results are shown in Table 1.

[0033] An optical microscope test was performed on Example 3. Under an optical microscope, a small amount of sample was melted and placed on both sides of a glass slide, and a magnification of 200 times was selected to observe the distribution morphology of the modified asphalt. The test results are shown in the attached figure.

[0034] Comparative Example: A method for improving the compatibility of desulfurized rubber modified asphalt. The steps are as follows.

[0035] Step 1, weighing a certain mass of base asphalt and desulfurized rubber, controlling the weight ratio between the base asphalt and the desulfurized rubber to be 100:50, and the properties of the base asphalt and the desulfurized rubber are the same as those in Example 1.

[0036] Step 2: heating the base asphalt to 165° C. in a reaction tank, adding the desulfurized rubber into the reaction tank and shearing for 40 min at a shear rate of 3000 r / min to obtain desulfurized rubber modified asphalt;

[0037] The comparative example was subjected to adhesion test and solubility test, the test method was the same as that of Example 1, and the test results are shown in Table 1.

[0038] The comparative example was subjected to an optical microscope test using the same test method as in Example 3. The test results are shown in the accompanying drawings.

[0039] Table 1 Compatibility parameters of desulfurized rubber modified asphalt prepared in the examples of the present invention and the comparative examples

[0040] sample Peeling rate (%) Solubility (%) Example 1 10.08 96.5 Example 2 5.27 99.5 Example 3 3.62 99.8 Comparative Example 19.76 84.5

[0041] By comparing the data in Table 1, it can be seen that compared with the comparative example, the peeling rate of Examples 1, 2, and 3 is greatly reduced, and the solubility is greatly increased. From the data in the table, it can be clearly concluded that the addition of linoleic acid and cerium stearate significantly improves the compatibility between desulfurized rubber and stearate. After the water boiling test, partial peeling occurred on the surface of the modified asphalt, that is, the modified asphalt film on the surface of the aggregate peeled off. The lower the peeling rate, the better the compatibility of desulfurized rubber and cerium stearate. There is a phase separation between desulfurized rubber and asphalt in large amounts. The addition of linoleic acid and rare earth stearate increases the solubility of desulfurized rubber in asphalt, indicating that the force between desulfurized rubber and asphalt molecules is enhanced and the compatibility is improved. Rare earth stearate can reduce the total heat absorption of desulfurized rubber modified asphalt and significantly reduce the phase separation phenomenon. Linoleic acid increases the light components of the modified asphalt and provides active functional groups. It contains unsaturated carbon-carbon double bonds and carboxyl active groups that can chemically react or physically adsorb with the functional groups on the surface of rubber particles and the active functional groups in asphalt, increasing the adhesion and interaction between them.

[0042] It can also be clearly observed from the accompanying drawings that Figure 2 ) The flake-shaped desulfurized rubber is unevenly dispersed in the asphalt, the surface voids of the modified asphalt are large, the desulfurized rubber particles are aggregated and irregular in shape, and phase separation occurs. Figure 1 ) due to the addition of devulcanized rubber and cerium stearate, the devulcanized rubber particles become uniform in size and evenly distributed, and no obvious aggregation or large areas appear.

[0043] The present invention has been described in detail above through embodiments, but the contents described are only preferred implementation examples of the present invention and cannot be considered to limit the scope of implementation of the embodiments of the present invention. The protection scope of the embodiments of the present invention is defined by the claims. Anyone who utilizes the technical solutions described in the embodiments of the present invention, or who, inspired by the technical solutions of the embodiments of the present invention, designs similar technical solutions within the essence and protection scope of the embodiments of the present invention to achieve the above-mentioned technical effects, or who makes equal changes and improvements to the scope of application, shall still be included in the protection scope of the patent covered by the embodiments of the present invention.

Claims

1. A method for improving the compatibility of desulfurized rubber modified asphalt, It is characterized in that The desulfurized rubber modified asphalt comprises the following components in parts by weight: 100 parts of base asphalt, 25-100 parts of desulfurized rubber, 2-16 parts of linoleic acid, and 0.2-2.4 parts of rare earth stearate, wherein the rare earth stearate is a mixture of one or both of cerium stearate and lanthanum stearate. The method for improving the compatibility of desulfurized rubber modified asphalt comprises the following steps: step 1, accurately weighing each component; step 2, adding linoleic acid to the desulfurized rubber, stirring evenly at room temperature, and letting it stand for 2 hours; step 3, heating the base asphalt to 165-175° C. in a reaction tank, adding the desulfurized rubber and rare earth stearate obtained in step 2 to the reaction tank for shearing for 30-50 minutes at a shear rate of 3000 rpm to obtain desulfurized rubber modified asphalt.

2. The method for improving the compatibility of desulfurized rubber modified asphalt according to claim 1, It is characterized in that The sol content of the devulcanized rubber is greater than 70%.

3. The method for improving the compatibility of desulfurized rubber modified asphalt according to claim 1, It is characterized in that The devulcanized rubber is a granular material produced by extrusion granulation.