Fly ash-based antistatic powder and epoxy coating prepared from same

By loading nano-tin dioxide on fly ash and carrying out silane modification, the problems of high cost and insufficient electrostatic performance of existing antistatic fillers are solved, and a low-cost, green and environmentally friendly antistatic coating is prepared with good electrostatic properties. Performance and results of epoxy coating applications.

CN118725629AInactive Publication Date: 2024-10-01TAIYUAN UNIVERSITY OF TECHNOLOGY

Patent Information

Application Number
CN202410979022.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing antistatic fillers have problems such as dark color, easy oxidation, high cost and easy agglomeration. It is difficult to effectively reduce the electrostatic hazards of polymer materials, and the efficient utilization of fly ash has not been fully developed.

Method used

Nanoscale tin dioxide is loaded onto the surface of micron-scale fly ash using a hydrothermal method to prepare an antistatic composite powder, which is modified with silane and mixed with an epoxy emulsion to form a fly ash-based antistatic epoxy coating. A low-cost, green and environmentally friendly electrostatic performance improvement is achieved.

Benefits of technology

The prepared fly ash-based antistatic powder and coating have excellent antistatic properties, low cost, reduced volume resistivity, comply with national antistatic coating standards, and have important application significance for composite antistatic fillers and epoxy coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725629A_ABST
    Figure CN118725629A_ABST
Patent Text Reader

Abstract

The invention discloses fly ash-based antistatic powder and an epoxy coating prepared from the same, and belongs to the field of mineral material processing. The preparation method comprises the following steps: firstly, loading nanoscale stannic oxide onto the surface of micron-sized fly ash by adopting a hydrothermal method to prepare antistatic composite powder capable of being used as filler, then carrying out organic modification on the composite powder by adopting silane to obtain modified composite powder, mixing the modified composite powder with an epoxy emulsion and an auxiliary agent according to a certain proportion, and curing by a curing agent to obtain the antistatic fly ash composite material. The fly ash-based antistatic epoxy coating is obtained. The fly ash-based composite powder prepared by the invention has the advantages of good antistatic performance, low cost and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to fly ash-based antistatic powder, epoxy coating prepared therefrom and a preparation method thereof, and belongs to the field of mineral material processing. Background Art

[0002] With the expansion of industrial production and the acceleration of urbanization, various insulators such as PVC, rubber, plastic and other polymers are widely used. Fires and explosions caused by the lack of current conduction properties on their surfaces are frequent. The best solution is to apply antistatic coatings on the surfaces of these formed polymer materials to reduce their resistivity. Antistatic fillers are an important component of antistatic coatings, but there are always various limitations when using single fillers, such as dark color, easy oxidation, high cost, easy agglomeration, etc. The development of green and economical antistatic composite fillers is of great significance to solving the hazards of polymer static electricity.

[0003] As one of the solid wastes after coal combustion, the output of fly ash has always been high. The environmental pollution caused by the accumulation of a large amount of fly ash and the depletion of other mineral resources have accelerated the utilization and research and development of fly ash. Fly ash is generally spherical in structure, and its main components are silicon oxide and aluminum oxide, showing high chemical activity. This chemical composition and structural characteristics make fly ash an ideal matrix for inorganic substances, providing basic support for the realization of high added value comprehensive utilization of fly ash. Summary of the invention

[0004] The present invention aims to provide a fly ash-based antistatic powder, an epoxy coating prepared therefrom and a preparation method thereof. Firstly, the prepared antistatic powder has the characteristics of excellent antistatic performance and low cost. The powder is used in epoxy emulsion to prepare a feasible antistatic epoxy coating. The prepared water-based antistatic coating can be cured at room temperature and is green and environmentally friendly.

[0005] In the present invention, fly ash is used as the matrix of tin dioxide to reduce the aggregation of tin dioxide, reduce costs, and realize the secondary utilization of solid waste. The mechanism of antistatic powder is that the electrostatic property of the powder comes from the tin gap and oxygen vacancies formed by the non-stoichiometric characteristics of SnO2 itself. When the tin matrix is ​​formed, a slight lattice distortion is generated during the entry process, and only low energy is required to generate it. When the defect of oxygen vacancy is formed, the doubly ionized oxygen vacancy will release the released electrons. When the oxygen vacancy and the tin matrix work together, the tin matrix will generate a donor energy level in the conduction band, and the free electrons formed on the oxygen vacancy are easily excited to the conduction band to form conductive carriers, and the resistivity is reduced.

[0006] The invention provides a fly ash-based antistatic powder, which adopts a hydrothermal method to load nano-sized tin dioxide onto the surface of micron-sized fly ash to prepare an antistatic composite powder that can be used as a filler. The mass ratio of tin dioxide to fly ash is 26-28:100.

[0007] In the present invention, the above powder is used in epoxy emulsion to prepare a feasible antistatic coating. First, nano-sized tin dioxide is loaded on the surface of micron-sized fly ash by a hydrothermal method to prepare an antistatic composite powder that can be used as a filler, and then the composite powder is organically modified by silane to obtain a modified composite powder, and the modified composite powder is mixed with epoxy emulsion and an auxiliary agent in a certain proportion, and then cured by a curing agent to obtain a fly ash-based antistatic epoxy coating.

[0008] Specifically, a fly ash-based antistatic coating is prepared by a hydrothermal method using fly ash as raw material, ammonia water and tin tetrachloride as coating agents to prepare a fly ash composite powder coated with tin dioxide, and the composite powder is modified with dodecyltriethoxysilane (DTES) and then filled with epoxy emulsion to obtain a fly ash-based antistatic composite coating. In the coating, the mass percentage of each component is: modified composite powder accounts for 1.9%-8.8%, epoxy emulsion accounts for 43.8%-47.6%, various additives account for 2.9%-3.7%, and water accounts for 43.8%-47.6%.

[0009] A method for preparing a fly ash-based antistatic coating comprises the following steps: In the first step, fly ash is calcined at 700℃ for 2h to obtain calcined fly ash, and the calcined fly ash is mixed with water at a mass ratio of 1:1 at room temperature to obtain a fly ash solution, and tin tetrachloride and ammonia solution are dripped into the fly ash solution at the same rate. After the dripping is completed, it is placed in a vacuum reactor and transferred to an oven for high-temperature reaction, and then washed, filtered, and dried to obtain a light yellow composite powder of fly ash coated with nano-tin dioxide. The concentration of the tin tetrachloride solution is 1mol / L; the mass concentration of the ammonia solution is 25%-28%.

[0010] In the second step, the fly ash composite powder coated with nano-tin dioxide is placed in a beaker and placed on a magnetic stirrer. It is heated in a water bath during stirring. When the temperature rises to 70°C, a certain amount of hydrolyzed dodecyltriethoxysilane (DTES) is slowly added and stirring is continued for 15 minutes to obtain the modified composite powder.

[0011] In the third step, the modified composite powder is added with deionized water and defoamer and dispersed at a high speed of 1000 r / min, and then epoxy emulsion and other additives (part of the defoamer, wetting agent, dispersant) are added and mixed on a stirrer at 500 r / min for 45 minutes, and then other additives such as leveling agent are added and stirred for 15 minutes to obtain a uniform water-soluble antistatic emulsion. After adding curing agent to the antistatic emulsion and mixing evenly on a magnetic stirrer for five minutes, an antistatic slurry that can be cured at room temperature is formed, and then the slurry is brushed and cured in a 100 mm×30 mm mold, and finally a sheet with a thickness of 2 mm±0.1 mm is obtained after natural air drying.

[0012] Taking the mass of epoxy emulsion as 100%, the additive content is the mass percentage of the additive in the epoxy emulsion, and the contents of wetting agent, defoamer, leveling agent and dispersant in the additive are in the range of 1.8% - 2.4%, 1.5% - 2%, 0.9% - 1.3% and 2% - 2.8% respectively. The curing agent is a polyamine, and its dosage is best at 30% of the mass of epoxy emulsion.

[0013] In the first step, the mass ratio of nano-tin dioxide on the surface of the composite material to fly ash is 24-28:100. The nano-tin dioxide is a theoretically generated mass.

[0014] The hydrothermal temperature in the first step is 140°C-180°C.

[0015] In the second step, the mass ratio of dodecyltriethoxysilane to the composite powder is 1.5~2.5:100.

[0016] In the third step, the mass ratio of silane-modified composite powder: epoxy emulsion: additive is 4-20:100:6-8.5.

[0017] Beneficial effects of the present invention: The fly ash-based composite powder prepared by the invention has the advantages of good antistatic performance, low cost and the like, and is of great significance for the preparation technology of novel composite antistatic filler and its application in epoxy coatings. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The SEM images of fly ash (a) and nano-tin dioxide / fly ash composite powder (b) of Example 2 of the present invention; Figure 2 This is a schematic diagram showing the activation index of the modified composite powder and the original composite powder in Example 6; Figure 3 FTIR graphs of fly ash, the coated composite powder in Example 2, and the modified composite powder in Example 6. DETAILED DESCRIPTION

[0019] The present invention is further illustrated by the following examples, but is not limited to the following examples. Example 1

[0020] A method for preparing fly ash-based antistatic powder comprises the following steps: 10.7g of fly ash and 11.6mL of water were mixed, 7.0125g of crystalline tin tetrachloride was weighed and dissolved in 20mL of water to prepare a 1mol / L tin tetrachloride solution; ammonia water was a 25%-28% concentration solution, and ammonia solution and crystalline tin tetrachloride solution were added to the fly ash aqueous solution at a drop rate of 1mL / min through a constant flow pump; after the addition was completed, the pH value was adjusted to 11, and the mixture was placed in a hydrothermal reactor and reacted in an oven at 160°C for 6h to obtain a fly ash-based antistatic powder. Example 2

[0021] A method for preparing fly ash-based antistatic powder comprises the following steps: 11.6g of fly ash and 11.6mL of water were mixed, 7.0125g of crystalline tin tetrachloride was weighed and dissolved in 20mL of water to prepare a 1mol / L tin tetrachloride solution; ammonia water was fixed as a 25%-28% solution, and ammonia solution and crystalline tin tetrachloride solution were added dropwise to the fly ash aqueous solution at a dropping speed of 1mL / min through a constant flow pump; after the addition was completed, the pH value was adjusted to 11, and the mixture was placed in a hydrothermal reactor and reacted in an oven at 160°C for 6h to obtain a fly ash-based antistatic powder. Example 3

[0022] A method for preparing fly ash-based antistatic powder comprises the following steps: 12.5g of fly ash and 11.6mL of water were mixed, 7.0125g of crystalline tin tetrachloride was weighed and dissolved in 20mL of water to prepare a 1mol / L tin tetrachloride solution; ammonia water was fixed as a 25%-28% solution, and ammonia solution and crystalline tin tetrachloride solution were added dropwise to the fly ash aqueous solution at a dropping speed of 1mL / min through a constant flow pump; after the addition was completed, the pH value was adjusted to 11, and the mixture was placed in a hydrothermal reactor and reacted in an oven at 160°C for 6h to obtain a fly ash-based antistatic powder. Example 4

[0023] A method for preparing fly ash-based antistatic powder comprises the following steps: 11.6g of fly ash and 11.6mL of water were mixed, 7.0125g of crystalline tin tetrachloride was weighed and dissolved in 20mL of water to prepare a 1mol / L tin tetrachloride solution; ammonia water was fixed as a 25%-28% solution, and ammonia solution and crystalline tin tetrachloride solution were added dropwise to the fly ash aqueous solution at a dropping speed of 1mL / min through a constant flow pump; after the addition was completed, the pH value was adjusted to 11, and the mixture was placed in a hydrothermal reactor and reacted in an oven at 140°C for 6h to obtain a fly ash-based antistatic powder. Example 5

[0024] A method for preparing fly ash-based antistatic powder comprises the following steps: 11.6g of fly ash and 11.6mL of water were mixed, 7.0125g of crystalline tin tetrachloride was weighed and dissolved in 20mL of water to prepare a 1mol / L tin tetrachloride solution; ammonia water was fixed as a 25%-28% solution, and ammonia solution and crystalline tin tetrachloride solution were added dropwise to the fly ash aqueous solution at a dropping speed of 1mL / min through a constant flow pump; after the addition was completed, the pH value was adjusted to 11, and the mixture was placed in a hydrothermal reactor and reacted in an oven at 180°C for 6h to obtain a fly ash-based antistatic powder. Example 6

[0025] A method for preparing fly ash-based modified composite powder comprises the following steps: Mix 11.6g fly ash and 11.6mL water, weigh 7.0125g crystallized tin tetrachloride and dissolve it in 20mL water to prepare a 1mol / L tin tetrachloride solution; ammonia water is a fixed 25%-28% solution, and ammonia water solution and crystallized tin tetrachloride solution are added to the fly ash aqueous solution at a drop rate of 1mL / min through a constant flow pump; after the dropwise addition is completed, adjust the pH value to 11, put it into a hydrothermal reactor, and react it in an oven at 160℃ for 6h. Take 10g of composite powder, add 2.5g of hydrolyzed DTES, stir and react at 70℃ for 15min to obtain dry modified composite powder. Example 7

[0026] An epoxy coating made of fly ash-based antistatic powder, the additives used in the embodiment of the present invention are as follows: Dispersant 5040, industrial grade, Guangzhou Runhong Chemical Co., Ltd.; Defoaming agent, industrial grade, Guangzhou Runhong Chemical Co., Ltd.; Wetting agent X-405, industrial grade, Guangzhou Runhong Chemical Co., Ltd.; Leveling agent, industrial grade, Guangzhou Runhong Chemical Co., Ltd.

[0027] The coating preparation method of this embodiment comprises the following steps: Mix 11.6g fly ash and 11.6mL water, weigh 7.0125g crystallized tin tetrachloride and dissolve it in 20mL water to prepare a 1mol / L tin tetrachloride solution; ammonia water is a fixed 25%-28% solution, and ammonia water solution and crystallized tin tetrachloride solution are added to the fly ash aqueous solution at a drop rate of 1mL / min through a constant flow pump; after the dropwise addition is completed, adjust the pH value to 11, put it into a hydrothermal reactor, and react it in an oven at 160℃ for 6h. Take 10g of composite powder, add 2.5g of hydrolyzed DTES, stir and react at 70℃ for 15min to obtain dry modified composite powder. Take 10g of composite powder, add 0.25g of hydrolyzed DTES, stir and react at 70℃ for 15min to obtain dry-modified composite powder, take 0.4g of modified composite powder, add 0.06 defoamer, disperse at 1000r / min, then add 10g epoxy emulsion and 0.12g defoamer, 0.2g wetting agent, 0.2g dispersant, 0.1g leveling agent and mix at 500 r / min for 1h to obtain antistatic emulsion, then add 3g curing agent, stir evenly and pour into a mold to wait for curing. After four days, an antistatic coating with a relatively stable volume resistivity is obtained. Example 8

[0028] An epoxy coating made of fly ash-based antistatic powder, the preparation method comprising the following steps: Mix 11.6g fly ash and 11.6mL water, weigh 7.0125g crystallized tin tetrachloride and dissolve it in 20mL water to prepare a 1mol / L tin tetrachloride solution; ammonia water is a fixed 25%-28% solution, and ammonia water solution and crystallized tin tetrachloride solution are added to the fly ash aqueous solution at a drop rate of 1mL / min through a constant flow pump; after the dropwise addition is completed, adjust the pH value to 11, put it into a hydrothermal reactor, and react it in an oven at 160℃ for 6h. Take 10g of composite powder, add 2.5g of hydrolyzed DTES, stir and react at 70℃ for 15min to obtain dry modified composite powder. Take 10g of composite powder, add 0.25g of hydrolyzed DTES, stir and react at 70℃ for 15min to obtain dry-modified composite powder, take 0.5g of modified composite powder, add auxiliary defoaming agent, disperse at 1000r / min, then add 10g epoxy emulsion and 0.12g defoaming agent, 0.2g wetting agent, 0.2g dispersant, 0.1g leveling agent and mix at 500 r / min for 1h to obtain antistatic emulsion, then add 3g curing agent, stir evenly and pour into a mold to wait for curing. After four days, an antistatic coating with a relatively stable volume resistivity is obtained. Example 9

[0029] An epoxy coating made of fly ash-based antistatic powder, the preparation method comprising the following steps: Mix 11.6g fly ash and 11.6mL water, weigh 7.0125g crystallized tin tetrachloride and dissolve it in 20mL water to prepare a 1mol / L tin tetrachloride solution; ammonia water is a fixed 25%-28% solution, and ammonia water solution and crystallized tin tetrachloride solution are added to the fly ash aqueous solution at a drop rate of 1mL / min through a constant flow pump; after the dropwise addition is completed, adjust the pH value to 11, put it into a hydrothermal reactor, and react it in an oven at 160℃ for 6h. Take 10g of composite powder, add 2.5g of hydrolyzed DTES, stir and react at 70℃ for 15min to obtain dry modified composite powder. Take 10g of composite powder, add 0.25g of hydrolyzed DTES, stir and react at 70℃ for 15min to obtain dry-modified composite powder, take 1g of modified composite powder, add additives, disperse at 1000r / min, then add 10g of epoxy emulsion and 0.12g of defoamer, 0.2g of wetting agent, 0.2g of dispersant, 0.1g of leveling agent, mix at 500r / min for 1h to obtain antistatic emulsion, then add 3g of curing agent, stir evenly, pour into a mold and wait for curing, and after four days, an antistatic coating with a relatively stable volume resistivity is obtained.

[0030] Embodiment 10: An epoxy coating made of fly ash-based antistatic powder, the preparation method comprising the following steps: Mix 11.6g fly ash and 11.6mL water, weigh 7.0125g crystalline tin tetrachloride and dissolve it in 20mL water to prepare a 1mol / L tin tetrachloride solution; ammonia water is a fixed 25%-28% solution, and ammonia water and crystalline tin tetrachloride solution are added to the fly ash aqueous solution at a drop rate of 1mL / min through a constant flow pump; after the drop addition is completed, adjust the pH value to 11, put it into a hydrothermal reactor, and react at 160℃ in an oven for 6h. Take 10g of composite powder, add 0.25g of hydrolyzed DTES, stir and react at 70℃ for 15min to obtain dry-modified composite powder. Take 10g of composite powder, add 2.5g of hydrolyzed DTES, stir and react at 70℃ for 15min to obtain dry-modified composite powder, take 1.5g of modified composite powder, add additives, disperse at 1000r / min, then add 10g of epoxy emulsion and 0.12g of defoamer, 0.2g of wetting agent, 0.2g of dispersant, and 0.1g of leveling agent, mix at 500 r / min for 1h to obtain antistatic emulsion, then add 3g of curing agent and wait for curing in the mold. After four days, an antistatic coating with a relatively stable volume resistivity is obtained.

[0031] Figure 1The scanning electron microscope images of fly ash and fly ash loaded with nano-tin dioxide prepared in Example 2 show that the composite powder fly ash surface is successfully loaded with tin dioxide particles. Table 1 shows the antistatic properties of fly ash and tin dioxide\fly ash composite powders prepared in Examples 1, 2, 3, 4, and 5. As can be seen from Table 1, the volume resistivity of fly ash is relatively high, while the volume resistivity of the powder prepared in Examples 1-5 is between 10 7 Ω·cm or less, and Example 2 reaches 5×10 3 Ω·cm, has good antistatic properties.

[0032] Table 1 Antistatic performance test results of pure fly ash and sample powders

[0033] Figure 2 This is a comparison chart of the activation index of the modified composite powder and the original composite powder in Example 6: it can be seen that the unmodified composite powder does not need to be stirred when placed in water, and the powder automatically falls to the bottom, while the modified powder basically all floats on the surface of the aqueous solution, indicating that the composite powder changes from hydrophilic to hydrophobic.

[0034] Figure 3 FTIR graphs of fly ash, the coated composite powder in Example 2, and the modified composite powder in Example 6. Compared with the fly ash in curve (a), the powder in Example 2 in curve (b) has a higher FTIR value at 727 cm -1 The new peak at 2923.95 cm-1 is the interaction between the active substances of tin dioxide and fly ash, indicating that tin dioxide is loaded on fly ash. -1 and 2852.58 cm -1 The existence of is caused by the stretching vibration of -CH3 and -CH2 groups in DTOFA, indicating that the coupling agent successfully acts on the composite powder.

[0035] Table 2 shows the antistatic properties of pure epoxy resin coatings and coatings prepared in Examples 7, 8, 9, and 10. As can be seen from Table 2, the volume resistivity of pure epoxy coatings is 10 13 Ω·cm, the volume resistivity of the epoxy coating prepared in Examples 7-10 after filling with composite powder is 10 7 Ω·cm, which is within the national standard for the volume resistivity of antistatic coatings 10 4 -10 9 Ω·cm standard range, among which Example 8 reached 4.5×10 5 Ω·cm, has good antistatic properties.

[0036] Table 2 Antistatic performance test results of pure epoxy coating and example coating .

Claims

1. A fly ash-based antistatic powder, characterized in that: Using fly ash as raw material, ammonia water and tin tetrachloride as coating agents, nano-sized tin dioxide is loaded onto the surface of micron-sized fly ash by hydrothermal method to prepare tin dioxide-coated fly ash composite powder, in which tin dioxide occupies 26%-28% of the fly ash mass.

2. A fly ash-based antistatic coating prepared from the fly ash-based antistatic powder according to claim 1, characterized in that: The fly ash-based antistatic powder is used in epoxy emulsion to prepare antistatic coating; specifically, firstly, fly ash is used as raw material, ammonia water and tin tetrachloride are used as coating agents, and nano-scale tin dioxide is loaded on the surface of micron-scale fly ash by a hydrothermal method to prepare an antistatic composite powder that can be used as a filler, and then, the composite powder is organically modified by silane to obtain a modified composite powder, the modified composite powder is mixed with epoxy emulsion and an auxiliary agent, and then cured by a curing agent to obtain a fly ash-based antistatic epoxy coating.

3. The fly ash-based antistatic coating according to claim 2, characterized in that: The mass percentages of the components in the coating are as follows: modified composite powder accounts for 1.9%-8.8%, epoxy emulsion accounts for 44%-47.3%, various additives account for 3.2%-3.5%, and water accounts for 44%-47.3%.

4. A method for preparing the fly ash-based antistatic coating according to claim 2 or 3, characterized in that The following steps are involved: In the first step, fly ash is calcined at 700°C for 2h to obtain calcined fly ash, and the calcined fly ash is mixed with water at a mass ratio of 1:1 at room temperature to obtain a fly ash solution, and a tin tetrachloride solution and an ammonia solution are dripped into the fly ash solution at the same rate. After the dripping is completed, the solution is placed in a vacuum reactor and transferred to an oven for high-temperature reaction, and then washed, filtered, and dried to obtain a light yellow composite powder of fly ash coated with nano-tin dioxide; The second step is to put the fly ash composite powder coated with nano-tin dioxide into a beaker and place it on a magnetic stirrer, and heat it in a water bath while stirring. When the temperature rises to 70°C, slowly add the hydrolyzed dodecyltriethoxysilane and continue stirring for 15 minutes to obtain the modified composite powder. In the third step, the modified composite powder is added with deionized water and defoamer and dispersed at a high speed of 1000 r / min, and then the epoxy emulsion and defoamer, wetting agent and dispersant are added and mixed on a stirrer at 500 r / min for 45 min, and then the leveling agent is added and stirred for 15 min to obtain a uniform water-soluble antistatic emulsion; the antistatic emulsion is added with a curing agent and evenly mixed on a magnetic stirrer for five minutes to form an antistatic slurry that can be cured at room temperature, and then the slurry is brushed and cured in a 100 mm×30 mm mold, and finally a thin sheet with a thickness of 2 mm±0.1 mm is obtained after natural air drying.

5. The method for preparing the fly ash-based antistatic coating according to claim 4, characterized in that: In the first step, the mass ratio of nano-tin dioxide on the surface of the composite material to fly ash is 24-28:100; the concentration of the tin tetrachloride solution is 1 mol / L; and the concentration of the ammonia water is 25%-28%.

6. The method for preparing the fly ash-based antistatic coating according to claim 4, characterized in that: The hydrothermal temperature in the first step is 140°C-180°C.

7. The method for preparing the fly ash-based antistatic coating according to claim 4, characterized in that: In the second step, the mass ratio of dodecyltriethoxysilane to the composite powder is 1.5-2.5:

100.

8. The method for preparing the fly ash-based antistatic coating according to claim 4, characterized in that: In the third step, the mass ratio of silane-modified composite powder: epoxy emulsion: additive is 4-20:100:6-8.

5.

9. The method for preparing the fly ash-based antistatic coating according to claim 4, characterized in that: In the third step, the mass percentage of each additive content in the epoxy emulsion is: wetting agent: 1.8% - 2.4%, defoaming agent: 1.5%-2%, leveling agent: 0.9%-1.3%, dispersant: 2%-2.8%.

10. The method for preparing the fly ash-based antistatic coating according to claim 4, characterized in that: In the third step, the curing agent is a polyamine, and its dosage is 30% of the mass of the epoxy emulsion.

Citation Information

Patent Citations

  • Aqueous expansion-type steel structure fireproof paint and preparation method thereof

    CN102850905A

  • Anticorrosive wear-resistant water-based filler and preparation method and application thereof in coating

    CN111892853A

  • Preparation method of antistatic waterborne epoxy resin floor coating

    CN112266704A

Cited By

  • Preparation method of fly ash-based flame-retardant antistatic composite powder and application of fly ash-based flame-retardant antistatic composite powder in waterborne epoxy coating

    CN122810630A