By introducing sulfonic acid groups and rigid benzene rings into the ink, changing the composition of the free radical curing prepolymer, and reacting with acrylic esters and glyceryl ethers, an atmospheric ink with high hardness and heat resistance is formed, solving the problems of existing inks. Heat resistance and adhesion issues, achieving rapid curing and good mechanical properties of the ink.

CN118725636AActive Publication Date: 2024-10-01DONGGUAN HUAHONG SCREEN PRINTING MATERIALS CO LTD

Patent Information

Application Number
CN202410964188.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

Existing water-based free radical-cation hybrid photo-curable inks have problems such as poor heat resistance, low hardness, low tensile strength and flexibility, poor abrasion resistance, long curing time, and weak bonding with printing materials.

Method used

By introducing sulfonic acid groups and rigid benzene rings into epoxy acrylate, the composition of the free radical curing prepolymer is changed, and the alicyclic epoxy compound is reacted with acrylate and glyceryl ether to form a cationic curing prepolymer, and the Under UV irradiation, it reacts with mixed monomers, photoinitiators and other substances to form inks with high hardness, heat resistance and good mechanical properties.

Benefits of technology

The obtained ink has a hardness of 3H-5H, Td10 of 394-448℃, Td90 of 530-589℃, tensile strength of 29.16-43.27MPa, flexibility of 2-3mm, curing time of 0.9-3.1s, and wear loss. The percentage is 8.9%-22.7%, and it has strong adhesion to packaging materials, making it suitable for screen printing of packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725636A_ABST
    Figure CN118725636A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ink, in particular to water-based free radical-cation hybrid photocuring ink and application thereof. The preparation method comprises the following steps: preparing a cationic cured prepolymer from an alicyclic epoxy compound, acrylate and glyceryl ether, and curing the cationic cured prepolymer with a prepared free radical cured prepolymer, a mixed monomer, a water-based pigment, an auxiliary agent and other substances through ultraviolet radiation to obtain the ink. By introducing a sulfonic acid group and a rigid benzene ring group, the cured ink has good hardness and heat resistance; the ink obtained by adding the cationic curing prepolymer has high tensile strength and flexibility; the mixed monomer is formed by mixing the monomer and the acrylate and used for diluting and curing the printing ink, the curing time of the printing ink is short, and the wear resistance is high; the ratio of the free radical photoinitiator to the cationic photoinitiator is changed, and sesamin is introduced, so that the hardness of the cured ink is 4H and 5H; the prepared light-cured ink is suitable for screen printing of various types of packaging materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inks, in particular to a water-based free radical-cation hybrid photocurable ink and application thereof. Background Art

[0002] UV ink is also called ultraviolet ink. This light-curing ink can polymerize the prepolymer and monomer in the ink through an instant photochemical reaction under the irradiation of ultraviolet rays and solidify into a film. In response to the call for environmental protection, the ink has been transformed from solvent-based to water-based. Water-based light-curing ink has the advantages of safety, reliability, high printing quality and high curing efficiency. It has been widely used in the printing of various materials such as mirror paper, posters, containers, plastics and cigarette packs.

[0003] The UV curing process of water-based ink can be divided into three systems according to different polymerization mechanisms, namely free radical polymerization system, cationic polymerization system and free radical-cationic mixed system. The curing process dominated by free radical polymerization includes chain initiation, chain growth and chain termination. The monomer reaction activity is high, the polymerization reaction rate is high and the cost is low, but there is an oxygen inhibition effect, incomplete curing, and a large volume shrinkage rate after curing. The cationic polymerization system can achieve deep curing of the ink, and there is no oxygen inhibition effect, and the shrinkage rate of the system after curing is small. However, the monomers used for cationic polymerization, such as epoxy monomers, have the disadvantages of high brittleness and poor fatigue resistance.

[0004] The free radical-cationic hybrid system combines the advantages of the above two curing systems. For example, patent CN201811332330.5 discloses "a water-based free radical-cationic hybrid photocurable ink and its application". The ink obtained by curing the oxygen-containing heterocyclic water-based silicone-modified polyester oligomer has good water resistance and fast curing speed, but the hardness is 2H and 3H, the hardness is low, and the heat resistance is poor. In addition, after the water-based ink is cured, there are problems of poor adhesion and low bonding strength between the water-based ink and the printed material. Patent CN202110316534.5 provides a "LED-UV curable offset ink". The ink components contain cation-curable compounds and free radical-curable compounds. The ink is used for printing and has strong adhesion to securities.

[0005] Raw materials used for ink: The oligomers used for free radical photocuring are resins with unsaturated double bonds, and the oligomers used for cationic photocuring are generally resins with epoxy or vinyl ether groups. Patent CN202111185113.X discloses "a fully bio-based thermosetting resin and its preparation method and application", which uses acrylates, unsaturated double-bond dibasic acids and epoxy compounds to prepare resins that can be used for inks. The resin has good mechanical properties, heat resistance and acid and alkali resistance, which solves the problem of poor flexibility of the resin. Patent CN202210689110.8 discloses "a printing process and printing ink for environmentally friendly printing inks". The printing ink contains raw materials such as water-based acrylates, polyurethane acrylates and wear-resistant color-retaining fillers. The obtained environmentally friendly ink overcomes the disadvantage of poor wear resistance of the ink.

[0006] The prior art aqueous free radical-cation hybrid photocurable inks also have the problems of poor heat resistance, low hardness, low tensile strength and flexibility, poor abrasion resistance, long curing time and weak bonding with the printed material.

[0007] Therefore, an aqueous free radical-cation hybrid photocurable ink and its application are proposed. Summary of the invention

[0008] The purpose of the present invention is to provide a water-based free radical-cation hybrid photocurable ink and its application, wherein a cationic curable prepolymer is obtained by reacting alicyclic epoxy compounds with acrylates and glycerol ethers, and then the modified free radical curable prepolymer, mixed monomers, water-based pigments, additives and other substances are cured by ultraviolet radiation to obtain ink. By modifying epoxy acrylate, introducing sulfonic acid groups and rigid benzene rings, and changing the composition and content of the free radical curable prepolymer in the system, the photocurable ink obtained has a hardness of 3H-5H and a T d10 394-448℃, T d90 530-589℃; by using alicyclic epoxy compounds as raw materials, further reacting with acrylate and glycerol ether to obtain cationic curing prepolymers, the tensile strength of the ink obtained by curing is 29.16-43.27MPa, and the flexibility is 2-3mm; by synthesizing monomers, adding mixed monomers into the system, the curing time of the ink is 0.9-3.1s, and the wear loss percentage of the cured ink is 8.9%-22.7%; by introducing a free radical photoinitiator and a cationic photoinitiator containing sesame, the curing time of the obtained ink is 1.0-4.5s, and the hardness of the cured ink is 4H and 5H; the adhesion of the water-based free radical-cationic hybrid photocurable ink to five kinds of packaging materials is 0 and 1. The ink prepared by the present invention has the advantages of high hardness, good heat resistance, strong tensile strength and flexibility, short curing time, wear resistance, and is suitable for screen printing of packaging materials.

[0009] To achieve the above object, the present invention provides the following technical solutions:

[0010] In one aspect, the present invention provides an aqueous free radical-cation hybrid photocurable ink, comprising the following preparation steps:

[0011] Adding concentrated sulfuric acid and ferric chloride to epoxy acrylate to obtain a reaction solution; adding 127.6-182.6 parts of sulfocarboxylic acid and triethylamine to the reaction solution for reflux reaction to obtain a product; layering, centrifuging and drying the product to obtain a free radical curing prepolymer;

[0012] Oxabicycloheptane, 2,5-divinyl, azobisisobutyronitrile and toluene are uniformly mixed to obtain a reaction solution; 40.1-68.5 parts of acrylate are added to the reaction solution, and nitrogen is introduced to react to obtain an intermediate; methacrylate glycidyl ether is added to the intermediate, reacted, and rotary evaporated to obtain a cationic curing prepolymer;

[0013] Triethylenetetramine, 21.6-41.3 parts of glycidyl methacrylate, THF and phenol are mixed to obtain a pre-reaction monomer; the pre-reaction monomer is reacted to obtain a monomer; the monomer and tri(propylene glycol) diacrylate are mixed to form a mixed monomer in a mass ratio of 0-8:1-9;

[0014] 40-90 parts of the free radical curing prepolymer, 0-60 parts of the cationic curing prepolymer, silane-PEG-carboxyl, terminal hydroxy silane, triethylamine and hydrochloride are reacted for 12 hours to obtain a precured ink precursor; the precured ink precursor, 32-46 parts of the mixed monomer, 1.9-4.5 parts of a free radical photoinitiator, 1.3-3.4 parts of a cationic photoinitiator, a red water-based pigment, sodium carboxymethyl cellulose, a defoamer, water and ethanol are uniformly mixed to obtain a precured ink; in terms of mass percentage, the free radical photoinitiator is composed of 0-45% of sesamin and 55-100% of benzophenone; the precured ink is irradiated with an intensity of 50-80mW / cm 2 The aqueous free radical-cation hybrid photocurable ink is obtained by irradiation and curing.

[0015] Preferably, the sulfocarboxylic acid is one of sulfo CY7 carboxyl, sulfo CY3 carboxylic acid, Alexa Fluor 647 carboxylic acid, sulfo anthocyanidin CY5 carboxylic acid, 3-cyanobiscaproic acid potassium salt, sulfobis-(N,N'-carboxylic acid)-CY5, CY7 diacid and CY3 diacid.

[0016] Preferably, the acrylate is one of ethylene glycol dimethacrylate, 2-hydroxy-1,3-propylene glycol acrylate, 1,5-pentanediol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,12-dodecanediol dimethacrylate, triethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate.

[0017] Preferably, the cationic curing prepolymer is 35-60 parts; and the cationic photoinitiator is a triarylsulfonium salt.

[0018] Preferably, the free radical curing prepolymer is 40-80 parts.

[0019] Preferably, the monomer and the tri(propylene glycol) diacrylate form the mixed monomer in a mass ratio of 2-8:1-5.

[0020] Preferably, the sesamin is 40%-45%.

[0021] Preferably, the benzophenone is 55-60%.

[0022] On the other hand, the present invention provides an application of an aqueous free radical-cation hybrid photocurable ink, wherein the aqueous free radical-cation hybrid photocurable ink is applied in screen printing of packaging materials; the packaging material comprises one of high-density polyethylene, low-density polyethylene, polyethylene terephthalate, polyvinyl chloride and polypropylene.

[0023] The use of an aqueous free radical-cation hybrid photocurable ink as described above, wherein the aqueous free radical-cation hybrid photocurable ink contains a free radical curable prepolymer, a cationic curable prepolymer, silane-PEG-carboxyl, triethylamine, hydrochloride, a mixed monomer, a free radical photoinitiator, a cationic photoinitiator, a red aqueous pigment, sodium carboxymethyl cellulose, a defoamer, water and ethanol; by changing the type of sulfocarboxylic acid and the amount of the free radical curable prepolymer added, the aqueous free radical-cation hybrid photocurable ink has a hardness of 3H-5H, T d10 394-448℃, T d90The aqueous free radical-cation hybrid photocurable ink obtained by adding the cationic curing prepolymer has a tensile strength of 29.16-43.27 MPa and a flexibility of 2-3 mm; by adding the mixed monomer, the curing time of the aqueous free radical-cation hybrid photocurable ink is 0.9-3.1 s, and the wear loss percentage is 8.9%-22.7%; by adding the cationic photoinitiator and the free radical photoinitiator, the curing time of the aqueous free radical-cation hybrid photocurable ink is 1.0-4.5 s, and the hardness is 4H and 5H; the adhesion of the aqueous free radical-cation hybrid photocurable ink to the packaging material is level 0 and level 1.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention obtains modified epoxy acrylate by modifying epoxy acrylate, and then reacts with cationic curing prepolymer, mixed monomer and initiator to form ink by UV curing. By introducing functional groups containing sulfonic acid group and rigid benzene ring and changing the content of modified epoxy acrylate free radical curing prepolymer in the system, the hardness of the obtained light-curing ink is 3H-5H; T d10 394-448℃, T d90 The temperature is 530-589°C. The water-based free radical-cation hybrid light-curing ink has good hardness and heat resistance.

[0026] 2. The alicyclic epoxyheptane containing two unsaturated double bonds reacts with acrylate to undergo condensation reaction. The double bonds of the reaction product continue to react with methacrylate glycidyl ether to obtain a cationic curing prepolymer containing epoxy groups at both ends. The cationic curing prepolymer and other substances form a curing ink under the conditions of initiator and ultraviolet radiation. By changing the type and amount of acrylate, introducing a flexible ether bond, and adjusting the content ratio of the cationic curing prepolymer in the precuring ink, the alicyclic epoxy compound will produce not only secondary oxygen salt intermediates but also tertiary oxygen salt intermediates during the ultraviolet polymerization process, and the photopolymerization activity is high. The obtained ink has a tensile strength of 29.16-43.27MPa and a flexibility of 2-3mm. The ink has good curing effect and mechanical properties.

[0027] 3. A stable monomer is formed by triethylenetetramine and glycidyl methacrylate, and the monomer is then mixed with tri(propylene glycol) diacrylate in a ratio of 2-8:1-5 to form a mixed monomer, and the content of the mixed monomer in the pre-cured ink is adjusted between 32-46 parts. The mixed monomer plays a role in diluting the reaction system and reducing the viscosity of the system. In addition, it is cured under the action of the photoinitiator to form a dense cross-linked structure. The obtained ink has a curing time of 0.9-3.1s, and a wear loss percentage of 8.9%-22.7%. The ink has a short curing time and good wear resistance.

[0028] 4. By changing the ratio of free radical photoinitiator and cationic photoinitiator, using sesamin to replace part of benzophenone in the free radical photoinitiator, the pre-cured ink was cured under different UV radiation intensities. The exciplex formed by sesamin generates free radicals by taking hydrogen, which promotes the polymerization and curing of modified epoxy acrylate and tri(propylene glycol) diacrylate. The curing time of the ink is 1.0-4.5s, and the hardness is 4H and 5H. The ink has a short curing time and high hardness.

[0029] 5. The aqueous free radical-cation hybrid photocurable ink prepared by the present invention is used for screen printing of packaging materials, and the adhesion between the ink and the material is strong. The adhesion between the ink and high-density polyethylene, low-density polyethylene, polyethylene terephthalate, polyvinyl chloride and polypropylene type packaging materials is between 0 and 1 levels, and the prepared ink is suitable for printing the above types of packaging materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a graph showing the curing time and abrasion resistance test results of the aqueous free radical-cation hybrid photocurable ink of Example 32 of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] See also Figure 1 The present invention provides a water-based free radical-cation hybrid photocurable ink and its application, and the technical scheme is as follows:

[0033] The substance information involved in the present invention is as follows:

[0034] Epoxy acrylate CAS: 71281-65-7; Sulfonic acid CY7 carboxyl CAS: 1251915-04-4; Sulfonic acid CY3 carboxylic acid CAS: 146368-13-0; Alexa Fluor 647 carboxylic acid CAS: 2090339-69-6; Sulfonic anthocyanidin CY5 carboxylic acid CAS: 2183440-68-6; 3-cyanobiscaproic acid potassium salt CAS: 762260-71-9; Sulfonic bis-(N, N'-carboxylic acid)-CY5 CAS: 2353410-10-1; CY7 diacid CAS: 146368-12-9; CY3 diacid CAS: 1034871-56-1; Oxabicycloheptane, 2,5-divinyl CAS: 165727-60-6; ​​Azobisisobutyronitrile CAS: 78-67-1; Methacrylate glycidyl ether CAS: 106-91-2; Ethylene glycol dimethacrylate CAS: 97-90-5; 2-Propylene glycol ester CAS: 1709-71- 3; 1,5-pentanediol dimethacrylate CAS: 13675-34-8; 1,6-hexanediol dimethacrylate CAS: 6606-59-3; 1,12-dodecanediol dimethacrylate CAS: 121150-60-5; triethylene glycol dimethacrylate CAS: 109-16-0; tetraethylene glycol dimethacrylate CAS: 109-17-1; triarylsulfonium salt CAS: 8945-2-37-9; benzophenone CAS: 119-61-9; sesamin CAS: 607-80-7; tri(propylene glycol) diacrylate CAS: 42978-66-5; triethylenetetramine CAS: 112-24-3; 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride CAS: 7084-11-9;

[0035] Silane-PEG-carboxyl product number PM01844 was purchased from Shanghai Chuangsai Technology Co., Ltd.; terminal hydroxyl silane was purchased from Shenzhen Jipeng Silicon Fluoride Materials Co., Ltd.; red water-based pigment product number Pigmosol Red 3855 was purchased from BASF (China) Co., Ltd.; SN-DISPERSANT 5027 is a defoaming agent purchased from Guangzhou Yachuang Innovation Materials Co., Ltd.

[0036] It should be noted that, if no specific conditions are specified in the examples, the experiments were carried out under conventional conditions. If no specific information is specified for the reagents or instruments used, they are all conventional products that can be purchased from the market, and the reagents used are of analytical grade.

[0037] Examples 1-7

[0038] 49 parts of epoxy acrylate are placed in a three-necked flask, the temperature is set to 70°C, and 3.2 parts of concentrated sulfuric acid and 3 parts of ferric chloride are added thereto under stirring to obtain a reaction liquid; 127.6-182.6 parts of sulfocarboxylic acid and triethylamine are added to the reaction liquid for reflux reaction for 24 hours to obtain a product; and the product is subjected to layering, centrifugation and drying to obtain a modified epoxy acrylate, i.e., a free radical curing prepolymer;

[0039] 15.2 parts of oxabicycloheptane, 2,5-divinyl, 16.5 parts of azobisisobutyronitrile and 50 parts of toluene were added to a reaction bottle and mixed evenly to obtain a reaction liquid; 68.5 parts of 1,12-dodecanediol dimethacrylate were added to the reaction liquid, nitrogen was introduced for 30 minutes, and the reaction was carried out at 65° C. for 5 hours to obtain an intermediate; 28.8 parts of methacrylate glycidyl ether were added to the intermediate, the reaction was carried out for 3 hours, and acrylate, i.e., a cationic curing prepolymer, was obtained by rotary evaporation;

[0040] 15.0 parts of triethylenetetramine, 21.6 parts of glycidyl methacrylate, 50 mL of THF and 1 mL of phenol are uniformly mixed to obtain a pre-reaction monomer; the pre-reaction monomer is reacted at 45° C. for 5 hours, and is separated, concentrated and dried to obtain a monomer; the monomer and tri(propylene glycol) diacrylate are mixed in a mass ratio of 2:1 to form a mixed monomer;

[0041] 40-80 parts of the free radical curing prepolymer, 40 parts of the cationic curing prepolymer, 6.5 parts of silane-PEG-carboxyl, 3.2 parts of terminal hydroxyl silane, 1.0 part of triethylamine, 2.0 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 10 mL of THF are reacted at 70° C. for 12 hours to obtain a precured ink precursor; 60 parts of the precured ink precursor, 38 parts of the mixed monomer, 3.9 parts of a free radical photoinitiator, 2.6 parts of a cationic photoinitiator, 28 parts of a red water-based pigment, 1.5 parts of sodium carboxymethyl cellulose, 3.0 parts of SN-DISPERSANT 5027, 26 parts of water and 12 parts of ethanol are uniformly mixed to obtain a precured ink; the cationic photoinitiator is a triarylsulfonium salt; in terms of mass percentage, the free radical photoinitiator consists of 43% of sesamin and 57% of benzophenone; the precured ink is irradiated at an intensity of 80 mW / cm 2 After irradiation and curing for 5 seconds, a water-based free radical-cation hybrid photocurable ink was obtained.

[0042] The specific information of the embodiment is shown in Table 1.

[0043] Table 1 Conditions of the preparation process of modified epoxy acrylate and light-curing ink

[0044]

[0045] Example 10

[0046] The water-based free radical-cation hybrid photocurable ink prepared in Examples 1-9 and Comparative Example 1 was placed for 24 hours before a hardness test was conducted; the prepared water-based free radical-cation hybrid photocurable ink was subjected to a heat resistance test. The hardness test was conducted in accordance with GB / T 6739-2006 "Determination of film hardness by pencil method for paints and varnishes". The heat resistance test method is as follows: the solidified graphite was scraped off the material and collected in a bowl, ground into powder, and 8 mg of the ink powder was weighed and tested in a TGA4000 thermogravimetric analyzer. During the test, nitrogen protection was introduced with a flow rate of 30 mL / min, a heating rate of 10 K / min, and a heating range of 30-600 ° C. T d10 and T d90 The temperatures are respectively when the ink weight loss rate reaches 10% and 90%. The test results are shown in Table 2.

[0047] Table 2 Performance test results of water-based free radical-cation hybrid photocurable ink

[0048]

[0049]

[0050] As shown in Table 2, the hardness of the photocurable ink prepared by the present invention is between 3H and 5H; d10 394-448℃, T d90 530-589°C. The present invention introduces sulfonic acid groups into the system by covalently linking the hydroxyl group of epoxy acrylate and the carboxyl group of sulfonic acid, thereby improving the affinity of water-based ink with water, and the ink has good properties after curing. In Examples 1-3, as the number of unsaturated double bonds in the sulfonic acid increases, the hardness of the cured ink decreases, and more double bonds give the system elasticity and flexibility. As shown in Example 1, its hardness is lower than that of Examples 2 and 3; however, the thermal stability of Example 1 is improved compared with Examples 2 and 3, and the ink T of Example 1 is d10 422℃, T d90is 559°C. Compared with other embodiments, Example 4 has more unsaturated six-membered rings in addition to the benzene ring, so it has high hardness and good thermal stability. The hardness of the cured ink obtained in Examples 5-7 is good. The hardness of the cured ink in Comparative Example 1 is reduced, only 3H. The reason is that compared with Example 5, its structure does not contain sulfonic acid groups, so the modified epoxy acrylate obtained as a binder for the ink has reduced compatibility with water, which leads to worse curing effect of the ink than the examples, and ultimately leads to reduced hardness. Comparison between Example 5 and Example 2 shows that due to the exposed unreacted carboxyl group, it can continue to react with the terminal hydroxy silane in the subsequent reaction process to introduce silicon elements, so the thermal stability is improved. At the same time, the terminal hydroxy silane can also play a role in leveling and lubrication of the system; similarly, the thermal stability of the ink in Example 6 is higher than that in Example 3, and the thermal stability of the ink in Example 7 is higher than that in Example 1, but the hardness is reduced. In Examples 5-7, the photocurable ink T of Example 7 d10 429℃, T d90 The temperature of the ink prepared under the conditions of Example 7 is the best. In general, the water-based free radical-cation hybrid light-curable ink prepared by the present invention has good hardness and thermal stability.

[0051] Examples 11-19

[0052] 49 parts of epoxy acrylate are placed in a three-necked flask, the temperature is set to 70°C, and 3.2 parts of concentrated sulfuric acid and 3 parts of ferric chloride are added thereto under stirring to obtain a reaction liquid; 156.1 parts of CY7 diacid and triethylamine are added to the reaction liquid and refluxed for 24 hours to obtain a product; the product is layered, centrifuged and dried to obtain a modified epoxy acrylate, i.e., a free radical curing prepolymer;

[0053] 15.2 parts of oxabicycloheptane, 2,5-divinyl, 16.5 parts of azobisisobutyronitrile and 50 parts of toluene are added to a reaction bottle and mixed evenly to obtain a reaction solution; 40.1-68.5 parts of acrylate are added to the reaction solution, nitrogen is introduced for 30 minutes, and the reaction is carried out at 65° C. for 5 hours to obtain an intermediate; 28.8 parts of glycidyl methacrylate are added to the intermediate, the reaction is carried out for 3 hours, and acrylate is obtained by rotary evaporation, i.e., a cationic curing prepolymer;

[0054] 15.0 parts of triethylenetetramine, 21.6 parts of glycidyl methacrylate, 50 mL of THF and 1 mL of phenol are uniformly mixed to obtain a pre-reaction monomer; the pre-reaction monomer is reacted at 45° C. for 5 hours, and is separated, concentrated and dried to obtain a monomer; the monomer and tri(propylene glycol) diacrylate are mixed in a mass ratio of 2:1 to form a mixed monomer;

[0055] 60 parts of the free radical curing prepolymer, 35-60 parts of the cationic curing prepolymer, 6.5 parts of silane-PEG-carboxyl, 3.2 parts of terminal hydroxyl silane, 1.0 part of triethylamine, 2.0 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 10 mL of THF are reacted at 70° C. for 12 hours to obtain a precured ink precursor; 60 parts of the precured ink precursor, 38 parts of the mixed monomer, 4.1 parts of a free radical photoinitiator, 2.8 parts of a cationic photoinitiator, 28 parts of a red water-based pigment, 1.5 parts of sodium carboxymethyl cellulose, 3.0 parts of SN-DISPERSANT 5027, 26 parts of water and 12 parts of ethanol are uniformly mixed to obtain a precured ink; the cationic photoinitiator is a triarylsulfonium salt; in terms of mass percentage, the free radical photoinitiator consists of 43% of sesamin and 57% of benzophenone; the precured ink is irradiated at an intensity of 80 mW / cm 2 After irradiation and curing for 6 seconds, a water-based free radical-cation hybrid photocurable ink was obtained.

[0056] The detailed information of the preparation is shown in Table 3.

[0057] Table 3 Cationic curing prepolymer preparation information and total addition amount

[0058]

[0059] Comparative Example 2

[0060] The difference from Example 19 is that the amount of the cationic curing prepolymer added is 0 parts, and the amount of the free radical curing prepolymer added is 90 parts.

[0061] Embodiment 20

[0062] The water-based free radical-cation hybrid photocurable ink prepared in Examples 11-19 and Comparative Example 2 was tested for tensile properties and flexibility. The specific test methods are as follows: flexibility was tested according to the method of GB / 1731-2020 "Determination of Flexibility of Paint Film and Putty Film"; for tensile properties test, the obtained pre-cured ink was placed in a tetrafluoroethylene mold, and the tensile properties were measured after UV curing. The cured ink was tested using a universal material testing machine, and the two ends of the ink were fixed with the chuck of the instrument, and stretched at a speed of 8mm / min, and the data at the time of fracture were recorded. The final results are shown in Table 4.

[0063] Table 4 Test results of mechanical properties of cured ink

[0064] Group Tensile strength(MPa) Flexibility(mm) Embodiment 11 31.85 2 Example 12 34.24 1 Example 13 32.50 1 Embodiment 14 33.39 1 Embodiment 15 35.71 1 Example 16 38.02 1 Embodiment 17 40.65 1 Embodiment 18 29.16 1 Embodiment 19 43.27 1 Comparative Example 2 10.08 3

[0065] The aqueous free radical-cation hybrid photocurable ink prepared in the embodiment of the present invention has a tensile strength of 29.16-43.27 MPa and a flexibility of 1, 2, and 3 mm. Comparison of the results of Examples 11 and 12 shows that the tensile strength of Example 2 is higher than that of Example 1. This is because the hydroxyl group of the acrylate in Example 2 reacts with the carboxyl group of the silane-PEG-carboxyl group, and the introduction of silane improves the flexibility of the system; Comparison of the results of Examples 11, 13-15 shows that as the molecular chain is extended, the tensile strength of the cured ink increases, among which Example 15 has the highest tensile strength of 35.71 MPa; Comparison of the results of Examples 16 and 17 shows that Example 17 has a high tensile strength of 40.65 MPa, which is due to the ether bond in the system increasing the tensile property of the ink; Comparison of the results of Examples 17-19 shows that the increase in the proportion of cationic curing prepolymers in the system further improves the tensile property of the system. Compared with other examples, Example 18 has the lowest tensile strength and the worst flexibility. The proportion of flexible groups in the system decreases, and the proportion of rigid groups contained in the free radical curing prepolymer increases, so the performance decreases. At the same time, the ink has good flexibility. In Comparative Example 2, since no cationic curing prepolymer is contained, the tensile strength is only 10.08Mpa and the flexibility is 1mm. On the one hand, the content of flexible groups in the system is small, and on the other hand, there is an oxygen inhibition effect during the curing process of the ink that is only cured by free radicals, and the curing is incomplete, so the tensile strength and flexibility are reduced at the same time. In summary, the water-based free radical-cationic hybrid light-curable ink prepared in the embodiment of the present invention has good tensile strength and flexibility.

[0066] Examples 21-31 and Comparative Example 3

[0067] 49 parts of epoxy acrylate are placed in a three-necked flask, the temperature is set to 70°C, and 3.2 parts of concentrated sulfuric acid and 3 parts of ferric chloride are added thereto under stirring to obtain a reaction liquid; 156 parts of CY7 diacid and triethylamine are added to the reaction liquid and refluxed for 24 hours to obtain a product; the product is layered, centrifuged and dried to obtain a modified epoxy acrylate, i.e., a free radical curing prepolymer;

[0068] 15.2 parts of oxabicycloheptane, 2,5-divinyl, 16.5 parts of azobisisobutyronitrile and 50 parts of toluene were added to a reaction bottle and mixed evenly to obtain a reaction solution; 43.5 parts of 2-acrylic acid-2-hydroxy-1,3-propanediol were added to the reaction solution, nitrogen was introduced for 30 minutes, and the reaction was carried out at 65° C. for 5 hours to obtain an intermediate; 28.8 parts of methyl methacrylate glycidyl ether were added to the intermediate, the reaction was carried out for 3 hours, and acrylate, i.e., a cationic curing prepolymer, was obtained by rotary evaporation;

[0069] 15.0 parts of triethylenetetramine, 21.6-44.6 parts of glycidyl methacrylate, 50 mL of THF and 1 mL of phenol are uniformly mixed to obtain a pre-reaction monomer; the pre-reaction monomer is reacted at 45° C. for 5 hours, and is separated, concentrated and dried to obtain a monomer; the monomer and tri(propylene glycol) diacrylate are mixed in a mass ratio of 0-8:1-9 to form a mixed monomer;

[0070] 55 parts of the free radical curing prepolymer, 35 parts of the cationic curing prepolymer, 6.5 parts of silane-PEG-carboxyl, 3.2 parts of terminal hydroxyl silane, 1.0 part of triethylamine, 2.0 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 10 mL of THF were reacted at 70° C. for 12 hours to obtain a precured ink precursor; 60 parts of the precured ink precursor, 32-46 parts of the mixed monomer, 3.9 parts of free radical photoinitiator, 2.6 parts of cationic photoinitiator, 28 parts of red water-based pigment, 1.5 parts of sodium carboxymethyl cellulose, 3.0 parts of SN-DISPERSANT 5027, 26 parts of water and 12 parts of ethanol were uniformly mixed to obtain a precured ink; the cationic photoinitiator was a triarylsulfonium salt; in terms of mass percentage, the free radical photoinitiator consisted of 44% of sesamin and 56% of benzophenone; the precured ink was irradiated with an intensity of 80 mW / cm 2 After irradiation and curing, a water-based free radical-cation hybrid light-curable ink is obtained.

[0071] The specific preparation information of the embodiments and comparative examples is shown in Table 5.

[0072] Table 5 Preparation of mixed monomers and information on the amount of mixed monomers added

[0073]

[0074]

[0075] Embodiment 32

[0076] The curing time and abrasion resistance of the aqueous free radical-cation hybrid photocurable ink prepared in Examples 21-31 and Comparative Example 3 were tested. The abrasion resistance tester NMC-Ⅱ was used to test the abrasion resistance of the ink. The test results are shown in the figure. Figure 1 shown.

[0077] Figure 1The results show that the time required for the ink of the embodiment of the present invention to be completely cured is in the range of 0.9-3.1s, and the percentage of wear loss is between 8.9% and 22.7%. In Examples 21-25, as the amount of glycidyl methacrylate added increases, the curing time shows a trend of first decreasing and then stabilizing, and the wear resistance gradually increases; after the epoxy groups of four molecules of glycidyl methacrylate are ring-opened, the hydroxyl group formed reacts with the amino group of one molecule of triethylenetetramine to form a stable monomer, which is cross-linked with the system under the action of the subsequent initiator. As the raw material content increases, the density of the formed ink increases and the curing time is shortened; the wear resistance first increases and then decreases, because the amount of initiator in the system is constant, and the free radicals formed by the initiator are not enough to cause the excess functional groups to undergo cross-linking and curing. Comparison of the results of Examples 24, 26-29 shows that as the mass ratio of the monomer to tri(propylene glycol) diacrylate increases, the curing time gradually decreases, and the wear resistance first increases and then stabilizes. As shown in the figure, the results of Examples 24, 30 and 31 show that as the amount of mixed monomer increases, the curing time increases, and the mass loss shows a trend of first decreasing and then increasing. The mixed monomer plays two roles in the system. One is to dilute the reaction system and reduce the viscosity of the system, so increasing its addition amount will increase the curing time; the other is that it is cured under the action of the photoinitiator, and excessive addition will cause incomplete curing and reduced wear resistance. Since no monomer was added to Comparative Example 3, the curing time increased and the wear resistance was the worst.

[0078] Examples 33-42

[0079] 60 parts of the free radical curing prepolymer prepared in Example 4, 40 parts of the cationic curing prepolymer prepared in Example 17, 6.5 parts of silane-PEG-carboxyl, 3.2 parts of terminal hydroxyl silane, 1.0 part of triethylamine, 2.0 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 10 mL of THF were reacted at 70° C. for 12 h to obtain a precured ink precursor; 60 parts of the precured ink precursor, 41.5 parts of the mixed monomer, 1.9-4.5 Parts of free radical photoinitiator, 1.3-3.4 parts of cationic photoinitiator, 28 parts of red water-based pigment, 1.5 parts of sodium carboxymethyl cellulose, 3.0 parts of SN-DISPERSANT5027, 26 parts of water and 12 parts of ethanol are uniformly mixed to obtain a pre-cured ink; the cationic photoinitiator is a triarylsulfonium salt; the free radical photoinitiator is composed of 40% of sesamin and 60% of benzophenone in terms of mass percentage; the pre-cured ink is irradiated with an intensity of 50-75mW / cm 2 After irradiation and curing for 5 seconds, a water-based free radical-cation hybrid light-curable ink is obtained. The specific preparation information of the embodiment is shown in Table 6.

[0080] Table 6 Composition and dosage of photoinitiator and preparation of ink

[0081]

[0082]

[0083] Embodiment 43

[0084] The free radical photoinitiator consists of 45% of sesamin and 55% of benzophenone.

[0085] Comparative Example 4

[0086] The free radical photoinitiator consists only of benzophenone.

[0087] Embodiment 44

[0088] The inks prepared in Examples 33-43 and Comparative Example 4 were tested for curing time and hardness. The time required for the aqueous free radical-cation hybrid photocurable ink to be completely cured and the hardness after storage for one day after curing are recorded in Table 7.

[0089] The curing time of the ink is 1.0-4.5s, and the hardness is 4H and 5H. In Examples 33-37, the ratio of the amount of free radical photoinitiator and cationic photoinitiator added is fixed at 3:2. As the total amount of the two added increases, the curing time shows a trend of first decreasing and then increasing. The amount of photoinitiator added increases, the more active groups are generated, and the shorter the curing time of the ink. Among them, the curing time of Example 36 is the shortest, which is 1.0s. In Example 37, the curing time increases with the increase in the amount of photoinitiator added. It may be due to the combination of the excess free radicals generated, resulting in a decrease in curing efficiency and a decrease in the hardness of the ink. The results of Examples 38-40 are compared with those of Example 36. The total amount of photoinitiator added remains unchanged. The curing time changes when the ratio between the free radical photoinitiator and the cationic photoinitiator is changed. The curing process initiated by the free radical and cationic photoinitiators is inconsistent. Controlling the ratio of the two at 3:2 is conducive to the curing process. When the ratio of the two free radical initiators in Example 38 is 7:3, the hardness decreases. Comparing the results of Example 36 with those of Examples 41 and 42, it is concluded that as the irradiation intensity increases, the curing time gradually shortens. The test results of the examples show that it is feasible to use part of sesamin instead of benzophenone as an initiator, and the results of the examples are better than the test results of Comparative Example 4. The possible reason is that sesamin combines with substances in the system to form an exciplex, which generates free radicals by extracting hydrogen, thereby promoting the polymerization of modified epoxy acrylate and tri(propylene glycol) diacrylate.

[0090] Table 7 Ink curing time and hardness

[0091] Group Curing time(s) hardness Embodiment 33 2.5 5H Embodiment 34 2.1 5H Embodiment 35 1.2 5H Embodiment 36 1.0 5H Embodiment 37 1.3 4H Embodiment 38 2.9 4H Embodiment 39 1.5 5H Embodiment 40 1.8 5H Embodiment 41 2.1 5H Embodiment 42 2.4 5H Embodiment 43 1.1 5H Comparative Example 4 4.5 4H

[0092] Examples 45-49

[0093] The precured ink prepared in Example 36 and ethanol are poured into one end of the screen printing plate to obtain pre-screen printing ink; the pre-scraper moves from the one end to the other end of the screen printing plate, so that the pre-screen printing ink is squeezed from the mesh of the graphic part to the packaging material by the scraper during the movement; then, the pre-screen printing ink is irradiated with an ultraviolet intensity of 75 mW / cm 2 The ink screen printing material was obtained by irradiating for 15 seconds. The specific types of packaging materials are shown in Table 8.

[0094] Comparative Example 5

[0095] Different from Example 45, the precured ink prepared in Comparative Example 1 was printed on high-density polyethylene by UV screen printing.

[0096] Embodiment 50

[0097] The ink screen printing materials obtained in Examples 45-49 and Comparative Example 5 were subjected to ink adhesion test, and the adhesion test was conducted according to the method of GB / T 9286-1998 "Scratching test for paints, varnishes and paint films". The specific test results are shown in Table 8.

[0098] As shown in Table 8, after the aqueous free radical-cation hybrid photocurable ink prepared by the present invention is cured on the packaging material, its adhesion is between 0 and 1, where 0 indicates that the ink has the best curing effect, the cutting edge is completely smooth, and no grid falls off, and 1 indicates the worst effect. The free radical curing prepolymer, the cationic curing prepolymer and the monomer in the ink prepared by the present invention contain groups such as unsaturated double bonds, rigid benzene rings and ether bonds, and have good adhesion to these packaging materials. Comparing the results of comparative example 5 with those of example 45, it can be seen that the adhesion of the ink cured in the comparative example is lower than that of the example, mainly because high-density polyethylene has a certain hygroscopicity, and the compatibility of the ink in the comparative example with water is lower than that of example 45, so a layer of water is formed between the ink and the high-density polyethylene material, which reduces the adhesion between the ink and the material. In general, the aqueous free radical-cation hybrid photocurable ink prepared by the present invention has good adhesion to the packaging material, and the prepared ink is suitable for printing packaging materials.

[0099] Table 8 Material types and adhesion test results

[0100] Group Types of packaging materials Adhesion(grade) Embodiment 45 High Density Polyethylene 0 Embodiment 46 Low density polyethylene 0 Embodiment 47 Polyethylene terephthalate 0 Embodiment 48 Polyvinyl chloride 0 Embodiment 49 Polypropylene 0 Comparative Example 5 High Density Polyethylene 1

[0101] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A water-based free radical-cation hybrid photocurable ink, characterized in that: The method comprises the following preparation steps: Adding concentrated sulfuric acid and ferric chloride to epoxy acrylate to obtain a reaction solution; adding 127.6-182.6 parts of sulfocarboxylic acid and triethylamine to the reaction solution for reflux reaction to obtain a product; layering, centrifuging and drying the product to obtain a free radical curing prepolymer; Oxabicycloheptane, 2,5-divinyl, azobisisobutyronitrile and toluene are uniformly mixed to obtain a reaction solution; 40.1-68.5 parts of acrylate are added to the reaction solution, and nitrogen is introduced to react to obtain an intermediate; methacrylate glycidyl ether is added to the intermediate, reacted, and rotary evaporated to obtain a cationic curing prepolymer; Triethylenetetramine, 21.6-41.3 parts of glycidyl methacrylate, THF and phenol are mixed to obtain a pre-reaction monomer; the pre-reaction monomer is reacted to obtain a monomer; the monomer and tri(propylene glycol) diacrylate are mixed to form a mixed monomer in a mass ratio of 0-8:1-9; 40-90 parts of the free radical curing prepolymer, 0-60 parts of the cationic curing prepolymer, silane-PEG-carboxyl, terminal hydroxy silane, triethylamine and hydrochloride are reacted for 12 hours to obtain a precured ink precursor; the precured ink precursor, 32-46 parts of the mixed monomer, 1.9-4.5 parts of a free radical photoinitiator, 1.3-3.4 parts of a cationic photoinitiator, a red water-based pigment, sodium carboxymethyl cellulose, a defoamer, water and ethanol are uniformly mixed to obtain a precured ink; in terms of mass percentage, the free radical photoinitiator is composed of 0-45% of sesamin and 55-100% of benzophenone; the precured ink is irradiated with an intensity of 50-80mW / cm 2 The aqueous free radical-cation hybrid photocurable ink is obtained by irradiation and curing.

2. The aqueous free radical-cation hybrid photocurable ink according to claim 1, characterized in that: The sulfocarboxylic acid is one of sulfo CY7 carboxyl, sulfo CY3 carboxylic acid, Alexa Fluor 647 carboxylic acid, sulfo anthocyanidin CY5 carboxylic acid, 3-cyanobiscaproic acid potassium salt, sulfobis-(N,N'-carboxylic acid)-CY5, CY7 diacid and CY3 diacid.

3. The aqueous free radical-cation hybrid photocurable ink according to claim 1, characterized in that: The acrylic acid ester is one of ethylene glycol dimethacrylate, 2-acrylic acid-2-hydroxy-1,3-propylene glycol ester, 1,5-pentanediol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,12-dodecanediol dimethacrylate, triethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate.

4. The aqueous free radical-cation hybrid photocurable ink according to claim 1, characterized in that: The cationic curing prepolymer is 35-60 parts; the cationic photoinitiator is triarylsulfonium salt.

5. The aqueous free radical-cation hybrid photocurable ink according to claim 1, characterized in that: The free radical curing prepolymer is 40-80 parts.

6. The aqueous free radical-cation hybrid photocurable ink according to claim 1, characterized in that: The monomer and the tri(propylene glycol) diacrylate form the mixed monomer in a mass ratio of 2-8:1-5.

7. The aqueous free radical-cation hybrid photocurable ink according to claim 1, characterized in that: The sesamin content is 40%-45%.

8. The aqueous free radical-cation hybrid photocurable ink according to claim 1, characterized in that: The benzophenone is 55-60%.

9. An application of a water-based free radical-cation hybrid photocurable ink, characterized in that: The water-based free radical-cation hybrid photocurable ink is used in screen printing of packaging materials; the packaging material comprises one of high-density polyethylene, low-density polyethylene, polyethylene terephthalate, polyvinyl chloride and polypropylene.

10. The use of a water-based free radical-cation hybrid photocurable ink according to claim 9, characterized in that: The aqueous free radical-cation hybrid photocurable ink contains free radical curable prepolymer, cationic curable prepolymer, silane-PEG-carboxyl, triethylamine, hydrochloride, mixed monomer, free radical photoinitiator, cationic photoinitiator, red aqueous pigment, sodium carboxymethyl cellulose, defoamer, water and ethanol; by changing the type of sulfocarboxylic acid and the addition amount of the free radical curable prepolymer, the hardness of the aqueous free radical-cation hybrid photocurable ink is 3H-5H, T d10 394-448℃, T d90 The aqueous free radical-cation hybrid photocurable ink obtained by adding the cationic curing prepolymer has a tensile strength of 29.16-43.27 MPa and a flexibility of 2-3 mm; by adding the mixed monomer, the curing time of the aqueous free radical-cation hybrid photocurable ink is 0.9-3.1 s, and the wear loss percentage is 8.9%-22.7%; by adding the cationic photoinitiator and the free radical photoinitiator, the curing time of the aqueous free radical-cation hybrid photocurable ink is 1.0-4.5 s, and the hardness is 4H and 5H; the adhesion of the aqueous free radical-cation hybrid photocurable ink to the packaging material is level 0 and level 1.

Citation Information

Patent Citations

  • Water-based free radical-cation hybrid photo-cured printing ink and application thereof

    CN109575681A

  • Silica gel for wine bottle cap, preparation method of silica gel and wine bottle cap

    CN112940202A

Cited By

  • High-strength PP material and application thereof in decorative film

    CN119144034A