Quick-curing sound insulation coating and preparation method thereof

By adding specific solutions and fillers to epoxy resin, and using thiourea and amine curing agents, the problem of slow curing speed of epoxy resin is solved, rapid curing and efficient sound insulation are achieved, and construction efficiency and coating performance are improved.

CN118725696AInactive Publication Date: 2024-10-01BEIJING HAOMING ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410931943.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure BDA0004939956470000021
    Figure BDA0004939956470000021
  • Figure BDA0004939956470000022
    Figure BDA0004939956470000022
  • Figure BDA0004939956470000051
    Figure BDA0004939956470000051
Patent Text Reader

Abstract

The invention relates to a quick-curing sound insulation coating and a preparation method thereof. The coating comprises the following components in parts by weight: 40-60 parts of epoxy acrylate emulsion, 15-25 parts of a dispersing agent, 10-30 parts of a curing agent and 0-2 parts of filler. Compared with the prior art, the curing speed is remarkably increased during application, and the sound insulation effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a fast-curing sound-insulating coating and a preparation method thereof. Background Art

[0002] Epoxy resin is a type of polymer with excellent mechanical properties, high stability and good adhesion, so it is widely used in the field of coatings. However, the curing speed of epoxy resin is greatly affected by the ambient temperature. When the temperature is below 10°C during winter construction, the curing time of epoxy resin coating will reach 48 hours or even longer, which seriously affects the construction progress. In addition, the curing speed is also very slow at room temperature.

[0003] CN117659352A discloses a water-based epoxy resin, a modified epoxy resin, a coating and a preparation method. The preparation method of the water-based epoxy resin comprises: mixing E-20 and E-51, and adding propylene glycol methyl ether; then adding 2,2-dihydroxymethyl propionic acid and p-hydroxyanisole; mixing acrylic acid and N,N-dimethylbenzylamine; mixing the above reactants to obtain a polymer; cooling and adding water to obtain a water-based epoxy resin. The preparation method of the modified epoxy resin comprises: adding an emulsifier to deionized water; adding a water-based epoxy resin and a modified monomer to the emulsifier solution to obtain a monomer; adding an initiator to the deionized water; adding a preset amount of deionized water to the second reactor, adding the monomer and the initiator solution to obtain a modified water-based epoxy resin. The coating preparation method comprises slurry preparation, main paint preparation, and mixing the main paint with a curing agent and diluting with water.

[0004] CN115386053B discloses a modified epoxy resin and its preparation method and application. The preparation method of the modified epoxy resin comprises the following steps: in a protective atmosphere, vegetable oil acid, epoxy resin and a catalyst are mixed and reacted to obtain a primary ester with an acid value less than or equal to 5 mgKOH / g; the primary ester is reacted with hydroxyphthalic anhydride to obtain a secondary ester with an acid value of 10 mgKOH / g-15 mgKOH / g; the secondary ester, acrylic acid, acrylic acid copolymer monomers, an initiator and a solvent are mixed and reacted to obtain a grafted product; and the grafted product is reacted with a neutralizer to obtain a modified epoxy resin.

[0005] However, the above application does not solve the problem that epoxy resin is difficult to cure quickly, and there is no further research on the functionalization of coatings in the prior art. Summary of the invention

[0006] The purpose of the present invention is to provide a fast-curing sound-insulating coating and a preparation method thereof in order to overcome the defects of the above-mentioned prior art. The coating significantly improves the curing speed when used and has a sound-insulating effect.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] The first aspect of the present invention provides a fast-curing sound-insulating coating, comprising the following components in parts by weight:

[0009]

[0010] Further, the coating comprises the following components by weight:

[0011]

[0012] Further, the preparation method of the epoxy acrylate emulsion is:

[0013] Slowly drop a mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide into epoxy resin E-51, and react at 60-100°C for 0.5-1.5h to obtain epoxy acrylate emulsion;

[0014] The molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid and p-hydroxyanisole is 1:(0.1-0.3):(0.8-1):(0.1-0.3).

[0015] Wherein, the coating dispersant comprises a polycarboxylic acid type dispersant;

[0016] Wherein, the filler is one or more of quartz sand, white carbon black, and mica powder.

[0017] Further, the curing agent includes the following components in parts by weight:

[0018] 30-50 parts of base curing agent

[0019] Thiourea 20-50 parts

[0020] Accelerator 70-100 parts.

[0021] Furthermore, the basic curing agent is one or more of diethylenetriamine, hexamethylenediamine, ethylenediamine, and triethylenetetramine.

[0022] Wherein, the accelerator is one or more of 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, triethylamine, triethanolamine, and o-hydroxybenzyldimethylamine.

[0023] A second aspect of the present invention provides a method for preparing a fast-curing sound-insulating coating, comprising the following steps:

[0024] The epoxy acrylate emulsion, the coating dispersant and the filler are mixed and stirred evenly, and then a curing agent is added and stirred evenly to obtain a coating.

[0025] Furthermore, the preparation method of the epoxy acrylate emulsion is:

[0026] Slowly drop a mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide into epoxy resin E-51, and react at 60-100°C for 0.5-1.5h to obtain epoxy acrylate emulsion;

[0027] The mass ratio of the epoxy acrylate emulsion, the coating dispersant, the curing agent and the filler is (40-60): (15-25): (10-30): (0-2);

[0028] The first stirring speed is 500-1000 r / min, the stirring time is 30-45 min, the second stirring speed is 500-600 r / min, the stirring time is 5-15 min;

[0029] Wherein, the coating dispersant comprises a polycarboxylic acid type dispersant;

[0030] Wherein, the filler is one or more of quartz sand, white carbon black, and mica powder.

[0031] Furthermore, the curing agent includes the following components in parts by weight:

[0032] 30-50 parts of base curing agent

[0033] Thiourea 20-50 parts

[0034] Accelerator 70-100 parts.

[0035] Furthermore, the basic curing agent is one or more of diethylenetriamine, hexamethylenediamine, ethylenediamine, and triethylenetetramine.

[0036] Wherein, the accelerator is one or more of 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, triethylamine, triethanolamine, and o-hydroxybenzyldimethylamine.

[0037] The third aspect of the present invention provides a fast-curing sound-insulating coating obtained by the preparation method of the fast-curing sound-insulating coating as described above.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] 1. The filler in the present invention has a significant sound insulation effect after being applied. This is mainly because with the addition of fillers, when the paint forms a film, the molecular materials in the paint can be sandwiched in the middle to form a dense network structure and play a bridge role. After the film is formed in the middle, it can effectively reduce the energy of the transmitted sound waves, so as to achieve the effect of sound absorption and sound insulation. In addition, since the paint film has a certain thickness, the filler is evenly distributed in the paint, and a porous structure is formed between two adjacent fillers. After the sound waves enter, they will penetrate along these pores and rub with other molecular materials of the paint, converting the sound energy into heat energy, so that the sound insulation effect is significantly increased.

[0040] 2. The curing agent used in the present invention has a good surface drying effect when the coating is cured. This is mainly due to the condensation reaction of thiourea and diethylenetriamine. Thiourea is very easy to be converted into its isomer ammonium thiocyanate. Ammonium thiocyanate is easily decomposed into thiocyanic acid and NH3. The decomposed ammonium thiocyanate reacts with 2,4,6-tris(dimethylaminomethyl)phenol. The source of the ingredients in the final curing agent can be divided into two categories: the condensation product of thiourea and diethylenetriamine; thiourea is converted into ammonium thiocyanate, and ammonium thiocyanate reacts with 2,4,6-tris(dimethylaminomethyl)phenol; there are a large number of active hydrogens in the thiourea molecule. The introduction of thiourea into the amine curing agent can not only improve the reaction activity and speed up the reaction rate, but also reduce the curing temperature of the amine curing agent. And the introduction of -SH group by modifying the polyamine with thiourea group significantly improves the curing speed of the amine curing agent, and the high electronegative N atom of the primary amine in the amine curing agent reacts with the C atom in thiourea for nucleophilic reaction. On the other hand, the thiocyanamide produced by the decomposition of some thioureas reacts with 2,4,6-tris(dimethylaminomethyl)phenol to generate a product containing a large amount of tertiary amines. This product not only has the possibility of curing epoxy with cyanamide, but also has the effect of extremely quickly promoting the curing reaction of modified polyamines containing -SH groups due to the presence of tertiary amine structures. Therefore, the two synergistically promote the curing effect of the curing agent. Moreover, the presence of the allyl functional group can improve the movement of molecules, increase the collision probability between the epoxy group and the curing agent, greatly improve the curing activity of the epoxy resin, accelerate the curing of the epoxy resin, and thus accelerate the curing of the coating. DETAILED DESCRIPTION

[0041] For ease of understanding of the present application, the present application will be described more fully below by way of embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0042] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art in the technical field of the present application. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. It should be noted that, unless otherwise specified, the term "and / or" used herein includes any and all combinations of one or more related listed items, and "above" and "below" include the number, and the meaning of "multiple" in "one or more" is more than two.

[0044] The curing speed of epoxy resin is greatly affected by the ambient temperature. During winter construction, when the temperature is below 10°C, the curing time of the epoxy resin coating will reach 48 hours or even longer, seriously affecting the construction progress. Moreover, the curing speed at room temperature is also very slow, and there is no further development in the functionalization of the coating.

[0045] Based on this, the first aspect of the embodiment of the present application provides a fast-curing sound insulation coating, including the following components in parts by weight:

[0046]

[0047] In some embodiments, the coating comprises the following components in parts by weight:

[0048]

[0049] In one embodiment, the coating comprises the following components in parts by weight:

[0050]

[0051] In some embodiments, the epoxy acrylate emulsion is prepared by:

[0052] A mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide is slowly added dropwise to the epoxy resin E-51, and the mixture is reacted at 60 to 100° C. for 0.5 to 1.5 h, preferably at 80° C. for 1 h, to obtain an epoxy acrylate emulsion.

[0053] The molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid and p-hydroxyanisole is 1:(0.1-0.3):(0.8-1):(0.1-0.3), preferably 1:0.2:0.95:0.2.

[0054] In some embodiments, the coating dispersant includes a polycarboxylic acid type dispersant. It should be noted that the embodiments of the present application do not specifically limit the coating dispersant, and synthetic polymers, coupling agents, silicates, etc. may be added. The dispersant is added to improve the coloring and hiding power of the coating in the embodiments of the present application and to prevent problems such as floating color and sedimentation.

[0055] In some embodiments, the curing agent includes the following components in parts by weight:

[0056] 30-50 parts of base curing agent

[0057] Thiourea 20-50 parts

[0058] Accelerator 70-100 parts.

[0059] In a preferred embodiment, the curing agent comprises at least the following components in parts by weight:

[0060] 40 parts of base curing agent

[0061] Thiourea 30 parts

[0062] 100 parts of accelerator.

[0063] It can be known that, based on the above embodiment, the basic curing agent is one or more of diethylenetriamine, hexamethylenediamine, ethylenediamine, and triethylenetetramine, preferably diethylenetriamine. The accelerator is one or more of 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, triethylamine, triethanolamine, and o-hydroxybenzyldimethylamine, preferably 2,4,6-tris(dimethylaminomethyl)phenol.

[0064] In some embodiments, the filler is quartz sand, white carbon black, or mica powder, preferably quartz sand, wherein the particle size of the quartz sand is 50 to 150 μm, preferably 50 μm.

[0065] A second aspect of the present application provides a method for preparing a fast-curing sound-insulating coating, comprising the following steps:

[0066] The epoxy acrylate emulsion, the coating dispersant and the filler are mixed and stirred evenly, and then a curing agent is added and stirred evenly to obtain a coating.

[0067] In some embodiments, the epoxy acrylate emulsion is prepared by:

[0068] A mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide is slowly added dropwise to the epoxy resin E-51, and the mixture is reacted at 60 to 100° C. for 0.5 to 1.5 h, preferably at 80° C. for 1 h, to obtain an epoxy acrylate emulsion.

[0069] The molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid and p-hydroxyanisole is 1:(0.1-0.3):(0.8-1):(0.1-0.3), preferably 1:0.2:0.95:0.2, wherein the ratio of the two addition amounts of tetrabutylammonium bromide is 1:1.

[0070] In some embodiments, the mass ratio of the epoxy acrylate emulsion, the coating dispersant, the curing agent, and the filler is (40-60): (15-25): (10-30): (0-2), preferably (50-60): (20-25): (15-30): (1-2), and preferably 60:20:18:2. The first stirring speed is 500-1000 r / min, and the stirring time is 30-45 min. Preferably, the first stirring speed is 800 r / min, and the stirring time is 35 min. The second stirring speed is 500-600 r / min, and the stirring time is 5-15 min. Preferably, the second stirring speed is 500 r / min, and the stirring time is 10 min.

[0071] In some embodiments, the coating dispersant includes a polycarboxylic acid-type dispersant;

[0072] The curing agent comprises the following components in parts by weight:

[0073] 30-50 parts of base curing agent

[0074] Thiourea 20-50 parts

[0075] Accelerator 70-100 parts.

[0076] In a preferred embodiment, the curing agent comprises at least the following components in parts by weight:

[0077] 40 parts of base curing agent

[0078] Thiourea 30 parts

[0079] 100 parts of accelerator.

[0080] Wherein, the basic curing agent is one or more of diethylenetriamine, hexamethylenediamine, ethylenediamine, triethylenetetramine, preferably diethylenetriamine. The accelerator is one or more of 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, triethylamine, triethanolamine, o-hydroxybenzyldimethylamine, preferably 2,4,6-tris(dimethylaminomethyl)phenol. The coating dispersant includes a polycarboxylic acid type dispersant, and the filler is quartz sand, white carbon black, mica powder, preferably quartz sand, wherein the particle size of the quartz sand is 50 to 150 μm, preferably 50 μm.

[0081] The third aspect of the embodiment of the present application provides a fast-curing sound-insulating coating obtained by the preparation method of the above-mentioned fast-curing sound-insulating coating.

[0082] The above implementation is described in more detail below in conjunction with specific examples.

[0083] Preparation Example

[0084] Unless otherwise specified, all reagents used in the following examples were purchased from Aladdin.

[0085] Example 1

[0086] This embodiment provides a fast-curing sound-insulating coating, the preparation method of which includes:

[0087] Mix epoxy acrylate emulsion and polycarboxylic acid type dispersant and stir, wherein the stirring speed is 800r / min, the stirring time is 35min, then add curing agent and stir evenly, wherein the stirring speed is 500r / min, the stirring time is 10min, and the coating is obtained, wherein the mass ratio of epoxy acrylate emulsion, coating dispersant and curing agent is 60:20:20. It should be noted that in this embodiment, the curing agent is composed of diethylenetriamine, thiourea and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 40:30:100, and the specific preparation method of epoxy acrylate emulsion is as follows: slowly drop a mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide in epoxy resin E-51, react at 80°C for 1h, and obtain epoxy acrylate emulsion, and the molar ratio of epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid and p-hydroxyanisole is 1:0.2:0.95:0.2.

[0088] Example 2

[0089] This embodiment provides a fast-curing sound-insulating coating, the preparation method of which includes:

[0090] Epoxy acrylate emulsion, polycarboxylic acid dispersant and quartz sand are mixed and stirred at a stirring speed of 800 r / min and a stirring time of 35 min, and then a curing agent is added and stirred evenly at a stirring speed of 500 r / min and a stirring time of 10 min to obtain a coating, wherein the mass ratio of epoxy acrylate emulsion, coating dispersant, curing agent and quartz sand is 60:20:18:2, and the particle size of the quartz sand is 50 μm. It should be noted that, in this embodiment, the curing agent is composed of diethylenetriamine, thiourea, and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 40:30:100. The specific preparation method of the epoxy acrylate emulsion is as follows: a mixed solution of methacrylic acid, p-hydroxyanisole, and tetrabutylammonium bromide is slowly added dropwise to the epoxy resin E-51, and the mixture is reacted at 80°C for 1 hour to obtain an epoxy acrylate emulsion. The molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid, and p-hydroxyanisole is 1:0.2:0.95:0.2.

[0091] Example 3

[0092] This embodiment provides a fast-curing sound-insulating coating, the preparation method of which includes:

[0093] Epoxy acrylate emulsion, polycarboxylic acid dispersant and quartz sand are mixed and stirred at a stirring speed of 800 r / min and a stirring time of 35 min, and then a curing agent is added and stirred evenly at a stirring speed of 500 r / min and a stirring time of 10 min to obtain a coating, wherein the mass ratio of epoxy acrylate emulsion, coating dispersant, curing agent and quartz sand is 60:20:18:2, and the particle size of the quartz sand is 100 μm. It should be noted that, in this embodiment, the curing agent is composed of diethylenetriamine, thiourea, and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 40:30:100. The specific preparation method of the epoxy acrylate emulsion is as follows: a mixed solution of methacrylic acid, p-hydroxyanisole, and tetrabutylammonium bromide is slowly added dropwise to the epoxy resin E-51, and the mixture is reacted at 80°C for 1 hour to obtain an epoxy acrylate emulsion. The molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid, and p-hydroxyanisole is 1:0.2:0.95:0.2.

[0094] Example 4

[0095] This embodiment provides a fast-curing sound-insulating coating, the preparation method of which includes:

[0096] Epoxy acrylate emulsion, polycarboxylic acid dispersant and quartz sand are mixed and stirred at a stirring speed of 800 r / min and a stirring time of 35 min, and then a curing agent is added and stirred evenly at a stirring speed of 500 r / min and a stirring time of 10 min to obtain a coating, wherein the mass ratio of epoxy acrylate emulsion, coating dispersant, curing agent and quartz sand is 60:20:18:2, and the particle size of the quartz sand is 150 μm. It should be noted that, in this embodiment, the curing agent is composed of diethylenetriamine, thiourea, and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 40:30:100. The specific preparation method of the epoxy acrylate emulsion is as follows: a mixed solution of methacrylic acid, p-hydroxyanisole, and tetrabutylammonium bromide is slowly added dropwise to the epoxy resin E-51, and the mixture is reacted at 80°C for 1 hour to obtain an epoxy acrylate emulsion. The molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid, and p-hydroxyanisole is 1:0.2:0.95:0.2.

[0097] Comparative Example 1

[0098] This embodiment provides a fast-curing sound-insulating coating, the preparation method of which includes:

[0099] Epoxy acrylate emulsion, polycarboxylic acid dispersant and quartz sand are mixed and stirred at a stirring speed of 800 r / min and a stirring time of 35 min, and then a curing agent is added and stirred evenly at a stirring speed of 500 r / min and a stirring time of 10 min to obtain a coating, wherein the mass ratio of epoxy acrylate emulsion, coating dispersant, curing agent and quartz sand is 60:20:18:2, and the particle size of the quartz sand is 300 μm. It should be noted that, in this comparative example, the curing agent is composed of diethylenetriamine, thiourea and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 40:30:100, and the specific preparation method of the epoxy acrylate emulsion is as follows: a mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide is slowly added dropwise to the epoxy resin E-51, and the mixture is reacted at 80°C for 1 hour to obtain an epoxy acrylate emulsion, and the molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid and p-hydroxyanisole is 1:0.2:0.95:0.2.

[0100] Comparative Example 2

[0101] This embodiment provides a fast-curing sound-insulating coating, the preparation method of which includes:

[0102] Mix epoxy acrylate emulsion, polycarboxylic acid type dispersant, quartz sand, and stir, wherein the stirring speed is 800r / min, the stirring time is 35min, then add curing agent and stir evenly, wherein the stirring speed is 500r / min, and the stirring time is 10min, to obtain coating, wherein the mass ratio of epoxy acrylate emulsion, coating dispersant, curing agent, and quartz sand is 60:20:18:2, wherein the particle size of quartz sand is 300μm. It should be noted that in this comparative example, the curing agent is diethylenetriamine, and the specific preparation method of epoxy acrylate emulsion is as follows: slowly drop a mixed solution of methacrylic acid, p-hydroxyanisole, and tetrabutylammonium bromide in epoxy resin E-51, react at 80°C for 1h, and obtain epoxy acrylate emulsion, wherein the molar ratio of epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid, and p-hydroxyanisole is 1:0.2:0.95:0.2.

[0103] Comparative Example 3

[0104] This embodiment provides a fast-curing sound-insulating coating, the preparation method of which includes:

[0105] Epoxy acrylate emulsion, polycarboxylic acid dispersant and quartz sand are mixed and stirred at a stirring speed of 800 r / min and a stirring time of 35 min, and then a curing agent is added and stirred evenly at a stirring speed of 500 r / min and a stirring time of 10 min to obtain a coating, wherein the mass ratio of epoxy acrylate emulsion, coating dispersant, curing agent and quartz sand is 60:20:18:2, and the particle size of the quartz sand is 50 μm. It should be noted that in this comparative example, the curing agent is 2,4,6-tris(dimethylaminomethyl)phenol, and the specific preparation method of the epoxy acrylate emulsion is as follows: a mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide is slowly added dropwise to the epoxy resin E-51, and the mixture is reacted at 80°C for 1 hour to obtain the epoxy acrylate emulsion, and the molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid and p-hydroxyanisole is 1:0.2:0.95:0.2.

[0106] Comparative Example 4

[0107] This embodiment provides a fast-curing sound-insulating coating, the preparation method of which includes:

[0108] Epoxy acrylate emulsion, polycarboxylic acid dispersant and quartz sand are mixed and stirred at a stirring speed of 800 r / min and a stirring time of 35 min, and then a curing agent is added and stirred evenly at a stirring speed of 500 r / min and a stirring time of 10 min to obtain a coating, wherein the mass ratio of epoxy acrylate emulsion, coating dispersant, curing agent and quartz sand is 60:20:18:2, and the particle size of the quartz sand is 50 μm. It should be noted that, in this comparative example, the curing agent is composed of diethylenetriamine and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 70:100, and the specific preparation method of the epoxy acrylate emulsion is as follows: a mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide is slowly added dropwise to the epoxy resin E-51, and the mixture is reacted at 80°C for 1 hour to obtain an epoxy acrylate emulsion, and the molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid and p-hydroxyanisole is 1:0.2:0.95:0.2.

[0109] Comparative Example 5

[0110] This embodiment provides a fast-curing sound-insulating coating, the preparation method of which includes:

[0111] Epoxy acrylate emulsion, polycarboxylic acid dispersant and quartz sand are mixed and stirred at a stirring speed of 800 r / min and a stirring time of 35 min, and then a curing agent is added and stirred evenly at a stirring speed of 500 r / min and a stirring time of 10 min to obtain a coating, wherein the mass ratio of epoxy acrylate emulsion, coating dispersant, curing agent and quartz sand is 60:20:18:2, and the particle size of the quartz sand is 50 μm. It should be noted that, in this comparative example, the curing agent is composed of diethylenetriamine and thiourea in a mass ratio of 70:100. The specific preparation method of the epoxy acrylate emulsion is as follows: a mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide is slowly added dropwise to the epoxy resin E-51, and the mixture is reacted at 80°C for 1 hour to obtain the epoxy acrylate emulsion. The molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid and p-hydroxyanisole is 1:0.2:0.95:0.2.

[0112] Comparative Example 6

[0113] This embodiment provides a fast-curing sound-insulating coating, the preparation method of which includes:

[0114] Epoxy resin E-51, polycarboxylic acid type dispersant, and quartz sand were mixed and stirred at a stirring speed of 800 r / min and a stirring time of 35 min, and then a curing agent was added and stirred evenly at a stirring speed of 500 r / min and a stirring time of 10 min to obtain a coating, wherein the mass ratio of epoxy acrylate emulsion, coating dispersant, curing agent, and quartz sand was 60:20:18:2, and the particle size of the quartz sand was 50 μm. It should be noted that in this comparative example, the curing agent was composed of diethylenetriamine, thiourea, and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 40:30:100.

[0115] Characterization example

[0116] 1. Sound insulation effect

[0117] Using a closed box, the coatings of Examples 1 to 4 and Comparative Example 1 were sprayed onto the inner surface of the closed box. The box was composed of a single-sided frosted acrylic plate with a thickness of 10 mm and a size of 20 mm × 900 mm × 1100 mm. The box was placed above the sound collecting chamber, and a microphone was placed inside the box, connected to the data acquisition instrument inside the sound collecting chamber. An iron ball with a diameter of 20 mm was freely dropped above the box until a collision sound was heard. The collection was completed and repeated at least 6 times. The results are shown in Table 1 below:

[0118] Table 1

[0119] Particle size (μm) Decibel (dB) Example 1 Not Join 102.78 Example 2 50 70.76 Example 3 100 84.87 Example 4 150 92.47 Comparative Example 1 300 100.77

[0120] As can be seen from the above table, adding filler, i.e. quartz sand, has a significant sound insulation effect. This is mainly because with the addition of quartz sand, when the coating forms a film, it can sandwich the molecular materials in the coating in the middle, forming a dense mesh structure and acting as a bridge. After the film is formed in the middle, it can effectively reduce the energy of the sound waves transmitted into it, achieving the effect of sound absorption and sound insulation. In addition, since the coating film has a certain thickness, the quartz sand is evenly distributed in the coating, and a porous structure is formed between two adjacent quartz sands. After the sound waves enter, they will penetrate along these pores and rub with other materials in the coating, converting the sound energy into heat energy, which significantly increases the sound insulation effect. And as the particle size of quartz sand becomes smaller, the sound insulation effect becomes better and better. This is mainly because when the equivalent is the same, the number of quartz sands increases, the porous gaps of the formed mesh structure become smaller, the number of holes increases, and the sound waves collide in multiple holes and convert into heat energy dissipation. However, when the particle size of quartz sand is too large, the distance between two adjacent quartz sands is too far, and when the sound waves enter, they cannot collide with them, and the effect naturally becomes worse.

[0121] 2. Curing speed

[0122] Example 2 and Comparative Examples 2 to 6 were tested, and the surface drying time of the cured product was measured according to the finger touch method of GB13477.5-2002. The results at room temperature are shown in the following table.

[0123] Table 2

[0124] Gel time (min) Paint surface drying time (min) Example 2 4.5 43 Comparative Example 2 22 The surface is always sticky Comparative Example 3 45 168 Comparative Example 4 59 212 Comparative Example 5 62 245 Comparative Example 6 8.7 70

[0125] As can be seen from the above table, the curing agent in Example 2 significantly improves the curing speed of the coating, and the surface drying effect at room temperature is good. This is mainly due to the condensation reaction of thiourea and diethylenetriamine, and thiourea is easily converted into its isomer ammonium thiocyanate. Ammonium thiocyanate is easily decomposed into thiocyanic acid and NH3, and the decomposed thiocyanate reacts with 2,4,6-tris (dimethylaminomethyl) phenol. The source of the ingredients in the final curing agent can be divided into two categories: the condensation product of thiourea and diethylenetriamine; thiourea is converted into ammonium thiocyanate, and ammonium thiocyanate reacts with 2,4,6-tris (dimethylaminomethyl) phenol; the number of active hydrogens in the thiourea molecule is large, and the introduction of thiourea in the amine curing agent can not only improve the reaction activity and speed up the reaction speed, but also reduce the curing temperature of the amine curing agent. And the introduction of -SH groups by modifying polyamines with thiourea groups significantly improves the curing speed of amine curing agents, and the high electronegativity N atoms of primary amines in amine curing agents react with C atoms in thiourea. On the other hand, the thiocyanamide produced by the decomposition of part of the thiourea reacts with 2,4,6-tris(dimethylaminomethyl)phenol to generate a product containing a large amount of tertiary amines, which not only has the possibility of cyanamide curing epoxy, but also has the effect of extremely fast promoting the curing reaction of the modified polyamine containing -SH groups due to the presence of the tertiary amine structure itself. Therefore, the two synergistically promote the curing effect of the curing agent. And compared with Comparative Example 6, Example 2 also has a significant improvement in the surface drying effect, which is mainly because the curing speed of epoxy resin at room temperature depends not only on the epoxy curing agent, but also on the activity of the epoxy resin. Improving the activity of the epoxy resin can also promote the curing speed of the epoxy resin. The presence of the allyl functional group can improve the motion of the molecule, increase the collision probability of the epoxy group and the curing agent, greatly improve the curing activity of the epoxy resin, and accelerate the curing of the epoxy resin.

[0126] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A fast-curing sound-insulating coating, characterized in that: It includes the following components by weight:

2. A fast-curing sound-insulating coating according to claim 1, characterized in that: The coating comprises the following components by weight:

3. A fast-curing sound-insulating coating according to claim 1 or 2, characterized in that: The epoxy acrylate emulsion preparation method is: Slowly drop a mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide into epoxy resin E-51, and react at 60-100° C. for 0.5-1.5 hours to obtain an epoxy acrylate emulsion, wherein the molar ratio of the epoxy resin E-51, tetrabutylammonium bromide, methacrylic acid and p-hydroxyanisole is 1:(0.1-0.3):(0.8-1):(0.1-0.3); and / or, the coating dispersant comprises a polycarboxylic acid type dispersant; And / or, the filler is one or more of quartz sand, white carbon black, and mica powder.

4. A fast-curing sound-insulating coating according to claim 1 or 2, characterized in that: The curing agent comprises the following components in parts by weight: 30-50 parts of base curing agent Thiourea 20-50 parts Accelerator 70-100 parts.

5. The fast-curing sound-proofing coating according to claim 4, characterized in that: The basic curing agent is one or more of diethylenetriamine, hexamethylenediamine, ethylenediamine, and triethylenetetramine; And / or, the promoter is one or more of 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, triethylamine, triethanolamine, and o-hydroxybenzyldimethylamine.

6. A method for preparing a fast-curing sound-insulating coating, characterized in that: The following steps are involved: The epoxy acrylate emulsion, the coating dispersant and the filler are mixed and stirred evenly, and then a curing agent is added and stirred evenly to obtain a coating.

7. The method for preparing a fast-curing sound-insulating coating according to claim 6, characterized in that: The epoxy acrylate emulsion preparation method is: Slowly drop a mixed solution of methacrylic acid, p-hydroxyanisole and tetrabutylammonium bromide into epoxy resin E-51, and react at 60-100°C for 0.5-1.5h to obtain epoxy acrylate emulsion; And / or, the mass ratio of the epoxy acrylate emulsion, the coating dispersant, the curing agent, and the filler is (40-60): (15-25): (10-30): (0-2); And / or, the first stirring speed is 500-1000 r / min, the stirring time is 30-45 min, and the second stirring speed is 500-600 r / min, the stirring time is 5-15 min; and / or, the coating dispersant comprises a polycarboxylic acid type dispersant; And / or, the filler is one or more of quartz sand, white carbon black, and mica powder.

8. The method for preparing a fast-curing sound-insulating coating according to claim 6, characterized in that: The curing agent comprises the following components in parts by weight: 30-50 parts of base curing agent Thiourea 20-50 parts Accelerator 70-100 parts.

9. The method for preparing a fast-curing sound-insulating coating according to claim 8, characterized in that: The basic curing agent is one or more of diethylenetriamine, hexamethylenediamine, ethylenediamine, and triethylenetetramine. And / or, the promoter is one or more of 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, triethylamine, triethanolamine, and o-hydroxybenzyldimethylamine.

10. A fast-curing sound-insulating coating obtained by the method for preparing the fast-curing sound-insulating coating according to any one of claims 6 to 9.

Citation Information

Patent Citations

  • Synthetic method of modified bisphenol A epoxy acrylate

    CN103360576A

  • Sound absorption epoxy resin composite coating and preparation method thereof

    CN108676469A

  • Polyacrylate emulsion and preparation method thereof

    CN111978486A

  • Low-temperature curing agent for epoxy resin and preparation method thereof

    CN112898535A

  • Water-borne epoxy resin, modified epoxy resin, coating and preparation method

    CN117659352A