Steel structure antifouling paint applied to marine environment and preparation method thereof
Through the combination of nano-silica coating modified zinc-based antibacterial agents and silane coupling agents, the problem of insufficient mechanical strength and binding force of silicone antifouling coatings in the marine environment is solved, and efficient antifouling and antibacterial properties are achieved. , extending the service life.
Patent Information
- Application Number
- CN202411011960.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing silicone low-surface-energy antifouling coatings have weak mechanical strength in the marine environment, and insufficient bonding force with epoxy intermediate paint, resulting in the antifouling coatings being prone to cracking and falling off and having a short service life.
Nano-silica-coated modified zinc-based antibacterial agents and 3-mercapto-1,2-propanediol are used to form modified antibacterial fillers through ultrasonic dispersion and hydrolysis, combined with silane coupling agents to enhance the mechanical properties and performance of antifouling coatings. The binding force with the epoxy intermediate paint forms a micron-nano binary rough structure, improving surface hydrophobicity and cross-linking ability.
It improves the mechanical properties and antibacterial ability of antifouling coatings, enhances the binding force with epoxy intermediate paint, extends the service life, prevents cracking and peeling of the coating, and significantly improves the impact resistance of antifouling coatings.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, relates to antifouling coatings, and specifically relates to an antifouling coating for steel structures in marine environments and a preparation method thereof. Background Art
[0002] In seawater, marine microorganisms are easily attached to the surface of steel structures, making the steel susceptible to microbial corrosion and destroying the coating on the metal surface, thereby accelerating metal corrosion and aging and shortening the service life of the steel structure. In order to reduce the damage caused by the attachment of marine organisms to marine steel structures, antifouling coatings are essential products.
[0003] As environmental protection concepts are gradually gaining popularity, the development and application of environmentally friendly and non-toxic marine antifouling coatings have received widespread attention. Low surface energy antifouling coatings are non-toxic and environmentally friendly, and are currently the main research direction. Silicone antifouling coatings have low surface energy and good fouling desorption capabilities.
[0004] Patent CN115093789A discloses a modified organic silicon marine antifouling coating and a preparation method thereof, wherein a modified silicon methoxy curing agent is synthesized to achieve a firm bond between the final cured organic silicon coating and various substrates. After the coating is cured, it still has a low surface free energy and a low elastic modulus. Although low surface energy and low elastic modulus are necessary conditions for good fouling desorption ability, the antifouling coating obtained by this scheme has weak mechanical strength and is easily broken and fallen off when hit or scratched in the ocean, resulting in antifouling failure.
[0005] Patent CN117511371A discloses a low surface energy marine antifouling coating, which solves the technical problem of how to make the coating formed by the coating have both low surface energy and excellent antifouling performance, and at the same time, the coating formed by the coating also has good mechanical properties; however, this solution does not take into account the connection performance between the antifouling coating and the epoxy intermediate paint, and there is still the problem of low bonding strength of the antifouling coating layer and easy falling off. Summary of the invention
[0006] The purpose of the present invention is to provide an antifouling coating for steel structures in marine environments and a preparation method thereof, so as to solve the problems of weak mechanical strength and weak bonding with epoxy intermediate paint of organic silicon low surface energy antifouling coating.
[0007] The purpose of the present invention can be achieved through the following technical solutions: An antifouling coating for steel structures in marine environments, comprising the following raw materials in parts by mass: 60-80 parts of polydimethylsiloxane, 20-30 parts of isophorone diisocyanate, 20-30 parts of modified antibacterial filler, 177.8-266.7 parts of tetrahydrofuran, 75.8-94.8 parts of N,N-dimethylformamide, 0.2-0.3 parts of chain extender, and 0.2-0.3 parts of catalyst.
[0008] The modified antibacterial filler is prepared by the following steps: The zinc-based antibacterial agent is added to anhydrous ethanol in a reactor, and ultrasonic dispersion is performed for 30-40 minutes. Then, the pH value is adjusted to 7.8-8.2 with an ammonia solution. Then, ethyl orthosilicate and 3-mercapto-1,2-propylene glycol are stirred and hydrolyzed in deionized water and added to the reactor. The temperature is raised to 75-85°C, and the reaction is stirred for 4-5 hours. After the reaction is completed, the precipitate is filtered, washed with acetone, and vacuum dried at 40-50°C to obtain a modified antibacterial filler.
[0009] The zinc-based antibacterial agent is a micron-sized zirconium phosphate-loaded silver-zinc antibacterial agent.
[0010] Furthermore, the chain extender is 1,4-butanediol; and the catalyst is dibutyltin dilaurate.
[0011] Furthermore, the dosage ratio of zinc-based antibacterial agent, anhydrous ethanol, ethyl orthosilicate, 3-mercapto-1,2-propylene glycol and deionized water is 4-5 g: 30-50 mL: 8-10 g: 3-4 g: 100-120 mL.
[0012] A method for preparing an antifouling coating for steel structures in a marine environment comprises the following steps: In a reaction kettle, add isophorone diisocyanate and polydimethylsiloxane to a mixed solvent of tetrahydrofuran and N,N-dimethylformamide, heat to 65-75°C and stir for 50-70 minutes under nitrogen protection, then add modified antibacterial filler, heat to 80-85°C and stir for 50-70 minutes, then add 1,4-butanediol and dibutyltin dilaurate, continue stirring and reacting for 2-3 hours, after rotary evaporation of most of the solvent, add deionized water, filter the precipitate after obtaining it, and vacuum dry the precipitate at 50-60°C for 24-26 hours to obtain an antifouling coating.
[0013] A method for using an antifouling coating for steel structures in a marine environment comprises the following steps: The antifouling coating, silane coupling agent and tetrahydrofuran are mixed and stirred to dissolve the antifouling coating. The antifouling coating is coated on the surface of the epoxy intermediate paint by a solution-casting film-forming method. The antifouling coating layer for the steel structure is obtained after the solvent is completely evaporated.
[0014] Furthermore, the antifouling coating, the silane coupling agent and tetrahydrofuran are used in a ratio of 30-55 g: 0.5-1.5 g: 100-120 mL.
[0015] Furthermore, the silane coupling agent is any one of KH550, KH560 and KH570.
[0016] Beneficial effects of the present invention: (1) The antifouling coating for steel structures in marine environments prepared by the present invention has low surface energy and low elastic modulus, and has good antifouling ability. The antifouling coating contains a modified zinc-based antibacterial agent coated with nano-silicon dioxide, and has good antibacterial ability. The nano-silicon dioxide improves the mechanical properties of the antifouling coating, making the antifouling coating less likely to crack or fall off, and having a long service life.
[0017] (2) The antifouling coating for steel structures in marine environments prepared by the present invention has a strong bonding force with the epoxy intermediate paint. Under the coupling effect of the silane coupling agent, the silica on the surface of the modified zinc-based antibacterial agent in the antifouling coating has a strong coupling effect with the epoxy intermediate paint. The mercapto group and epoxy group contained on the surface of the modified zinc-based antibacterial agent can also be covalently bonded, which further enhances the bonding ability between the antifouling coating and the epoxy intermediate paint, making the antifouling coating less likely to fall off.
[0018] (3) The present invention grafts 3-mercapto-1,2-propanediol containing a mercapto group onto the surface of the zinc-based antimicrobial agent, so that the zinc-based antimicrobial agent and nano-silicon dioxide that are easy to agglomerate are evenly dispersed, and a micron-nano binary rough structure is formed on the surface of the antifouling coating, thereby reducing the surface energy of the antifouling coating and increasing the surface area of the antifouling coating, providing more surface area for the cross-linking of the antifouling coating and the epoxy intermediate paint, and improving the bonding force between the antifouling coating and the epoxy intermediate paint. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Embodiment 1: A method for preparing an antifouling coating for steel structures in a marine environment, comprising the following steps: Step 1: Add 40 g of zinc-based antibacterial agent to 300 mL of anhydrous ethanol in a reactor, and perform ultrasonic dispersion for 30 min. Then adjust the pH value to 7.8 with an ammonia solution, and then add 80 g of ethyl orthosilicate and 30 g of 3-mercapto-1,2-propylene glycol to the reactor after stirring and hydrolyzing in 1000 mL of deionized water. Heat to 75 ° C, stir and react for 4 h. After the reaction is completed, filter, wash the precipitate with acetone, and dry in vacuo at 40 ° C to obtain a modified antibacterial filler.
[0021] Step 2: Add 20g of isophorone diisocyanate and 60g of polydimethylsiloxane to a mixed solvent of 200mL of tetrahydrofuran and 80mL of N,N-dimethylformamide in a reactor. Heat to 65°C and stir for 50min under nitrogen protection. Add 20g of modified antibacterial filler, heat to 80°C and stir for 50min. Then add 0.2g of 1,4-butanediol and 0.2g of dibutyltin dilaurate, continue stirring and reacting for 2h, and after rotary evaporation of most of the solvent, add deionized water, filter the precipitate after obtaining it, and vacuum dry the precipitate at 50°C for 24h to obtain an antifouling coating.
[0022] A method for using an antifouling coating for steel structures in a marine environment comprises the following steps: 30 g of antifouling paint, 0.5 g of KH550 and 100 mL of tetrahydrofuran were mixed and stirred to dissolve the antifouling paint. The antifouling paint was coated on the surface of the epoxy intermediate paint by a solution-casting film-forming method. After the solvent was completely evaporated, an antifouling paint layer for the steel structure was obtained.
[0023] Embodiment 2: A method for preparing an antifouling coating for steel structures in a marine environment, comprising the following steps: Step 1. Add 45 g of zinc-based antibacterial agent to 400 mL of anhydrous ethanol in a reactor, ultrasonically disperse for 35 minutes, then adjust the pH value to 8 with an ammonia solution, then stir and hydrolyze 90 g of ethyl orthosilicate and 35 g of 3-mercapto-1,2-propylene glycol in 1100 mL of deionized water and add them to the reactor, heat to 80°C, stir and react for 4.5 hours, filter after the reaction, wash the precipitate with acetone, and vacuum dry at 45°C to obtain a modified antibacterial filler.
[0024] Step 2: Add 25g of isophorone diisocyanate and 70g of polydimethylsiloxane to a mixed solvent of 250mL of tetrahydrofuran and 90mL of N,N-dimethylformamide in a reactor. Heat to 70°C and stir for 60min under nitrogen protection. Add 25g of modified antibacterial filler, heat to 82°C and stir for 60min. Then add 0.25g of 1,4-butanediol and 0.25g of dibutyltin dilaurate, continue stirring and reacting for 2.5h, and after rotary evaporation of most of the solvent, add deionized water, filter the precipitate after obtaining it, and vacuum dry the precipitate at 55°C for 25h to obtain an antifouling coating.
[0025] A method for using an antifouling coating for steel structures in a marine environment comprises the following steps: 45g of antifouling coating, 1g of KH560 and 110mL of tetrahydrofuran were mixed and stirred to dissolve the antifouling coating. The antifouling coating was coated on the surface of the epoxy intermediate paint by a solution-casting film-forming method. After the solvent was completely evaporated, an antifouling coating layer for the steel structure was obtained.
[0026] Embodiment 3: A method for preparing an antifouling coating for steel structures in a marine environment, comprising the following steps: Step 1. Add 50 g of zinc-based antibacterial agent to 500 mL of anhydrous ethanol in a reactor, ultrasonically disperse for 40 minutes, then adjust the pH value to 8.2 with an ammonia solution, then stir and hydrolyze 100 g of ethyl orthosilicate and 40 g of 3-mercapto-1,2-propylene glycol in 1200 mL of deionized water and add them to the reactor, heat to 85°C, stir and react for 5 hours, filter after the reaction, wash the precipitate with acetone, and vacuum dry at 50°C to obtain a modified antibacterial filler.
[0027] The nano-silicon dioxide-coated zinc-based antibacterial agent is obtained by hydrolyzing and polycondensing on the surface of a zinc-based antibacterial agent containing nano-silver. The zinc-based antibacterial agent is in the micron scale, and the polycondensed silicon dioxide is in the nanoscale. The two form a micron-nano binary rough structure. When the nano-silicon dioxide is polycondensed, the silanol groups on the surface are covalently bonded to the thiol groups on 3-mercapto-1,2-propylene glycol, and the 3-mercapto-1,2-propylene glycol is bonded to the surface of the zinc-based antibacterial agent, thereby modifying the surface of the zinc-based antibacterial agent.
[0028] Step 2: Add 30g of isophorone diisocyanate and 80g of polydimethylsiloxane to a mixed solvent of 300mL of tetrahydrofuran and 100mL of N,N-dimethylformamide in a reactor. Heat to 75°C and stir for 70min under nitrogen protection. Add 30g of modified antibacterial filler, heat to 85°C and stir for 70min. Then add 0.3g of 1,4-butanediol and 0.3g of dibutyltin dilaurate, continue stirring and reacting for 3h, after rotary evaporation of most of the solvent, add deionized water, filter the precipitate after obtaining it, and vacuum dry the precipitate at 60°C for 26h to obtain an antifouling coating.
[0029] Through the good compatibility and dispersibility of 3-mercapto-1,2-propanediol in the solvent, the zinc-based antibacterial agent is evenly dispersed in the solvent, so that the modified antibacterial coating can form a composite low surface energy coating on the surface of the antifouling coating, that is, the surface energy of the antifouling coating is reduced and the hydrophobicity of the surface of the antifouling coating is improved. The nanosilver in the modified antibacterial coating also has antibacterial ability, which improves the antibacterial property of the antifouling coating.
[0030] A method for using an antifouling coating for steel structures in a marine environment comprises the following steps: 55 g of antifouling paint, 1.5 g of KH570 and 120 mL of tetrahydrofuran were mixed and stirred to dissolve the antifouling paint. The antifouling paint was coated on the surface of the epoxy intermediate paint by a solution-casting film-forming method. After the solvent was completely evaporated, an antifouling paint layer for the steel structure was obtained.
[0031] Under the action of silane coupling agent, the nano-silica on the surface of the modified antibacterial filler in the antifouling coating can be well combined with the epoxy intermediate paint, and the micron-nano binary rough structure on the surface of the modified antibacterial coating provides more specific surface area, which improves the bonding strength between the antifouling coating and the epoxy intermediate paint, and solves the problem of low bonding strength between the antifouling coating and the epoxy intermediate paint. The thiol and epoxy groups on the surface of the modified antibacterial filler can produce a cross-linking reaction to form a covalent bond with strong bonding strength, which further improves the bonding strength between the antifouling coating and the epoxy intermediate paint.
[0032] Comparative Example 1: The difference from Example 1 is that the modified antibacterial filler is replaced by a zinc-based antibacterial agent.
[0033] Comparative Example 2: The difference from Example 1 is that hexadecyl dimethyl ethyl ammonium bromide is used to replace the modified antibacterial filler.
[0034] Comparative Example 3: The difference from Example 1 is that the modified antibacterial filler is replaced by nanosilver / silicon dioxide core-shell particles.
[0035] Nanosilicon dioxide-coated nanosilver is prepared from nanosilver and ethyl orthosilicate. The specific steps can be referred to CN102671588A, a method for synthesizing nanosilver / silicon dioxide core-shell particles in an aqueous system.
[0036] The sources of some reagents in the comparative examples and embodiments are as follows: Polydimethylsiloxane, isophorone diisocyanate, 3-mercapto-1,2-propanediol, tetrahydrofuran, N,N-dimethylformamide, 1,4-butanediol, and dibutyltin dilaurate were purchased from Macklin Reagent.
[0037] Hexadecyl dimethyl ethyl ammonium bromide was purchased from Wuhan Jixinyibang Biotechnology Co., Ltd.
[0038] The zinc-based antibacterial agent is a micron-sized zirconium phosphate-loaded silver-zinc antibacterial agent purchased from Guangdong Kepuin Biotechnology Co., Ltd., model KP-J151.
[0039] The antifouling coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were coated on steel plates coated with epoxy intermediate paint to form films with a film thickness of 150 μm to obtain antifouling coating layers, and the performance of the antifouling coating layers was tested.
[0040] The contact angles of deionized water and diiodomethane on the surface of the antifouling coating layer were measured using a DSA25S contact angle meter from Kruss, Germany. The test droplet volume was 2 μL, and the liquids used in the test were deionized water and diiodomethane. Five different areas of the antifouling coating layer were tested, and the contact angle results were averaged. The surface energy of the coating was calculated using the Owens-Wendt-Rabel-Kaelble method.
[0041] According to ASTM D4541, the antifouling coating was dissolved in tetrahydrofuran and coated between an aluminum ingot with a diameter of 20 mm and an epoxy resin plate, and cured at room temperature for 7 days. The bonding strength between the coating and the substrate was measured using a digital pull-off adhesion tester (BGD500), and 5 different areas of the antifouling coating layer were tested, and the test results were averaged.
[0042] According to GB / T1732-2020, the impact resistance of the coating to be tested is tested. The tinplate coated with the antifouling coating layer is placed on the paint film impactor (BGD304) and tested by drop hammer impact. After each test, if there is no obvious crack, peeling or other damage, the test height is raised and repeated until the coating is damaged. The height is raised by 5 cm each time. If the coating is damaged, the test height is lowered and repeated until the coating is not damaged. The final test result is expressed as the maximum height (cm) at which the coating does not show cracks, peeling or other damage in three parallel tests.
[0043] The antibacterial ability test was carried out in accordance with the national standards GB / T21866-2008 and GB / T4789.2-2016. The test bacteria were Escherichia coli (Gram-negative bacteria) and Staphylococcus aureus (Gram-positive bacteria); 200μL of the test bacteria were transferred with a pipette and dropped on the surface of the antifouling coating layer after UV sterilization, and evenly covered with a sterilized PE cover film, and the test coating was placed in an incubator for 1 hour. After the incubation, the coating was removed, and the coating and cover film were repeatedly rinsed with 20mL of sterile saline. 20μL of the elution solution was dropped on the culture dish and evenly coated, and cultured in the incubator for 48h, which was recorded as the sample group. The number of colonies on the sample group culture dish was counted with a plate colony counter. Each test coating was tested in 2 groups in parallel, and the test results were averaged. Another group of blank control group tests were conducted, and the number of colonies on the control group culture dish was counted. The sterilization rate was calculated according to the following formula: Sterilization rate (%) = (number of colonies in the control group – number of colonies in the sample) / number of colonies in the control group × 100% The results are shown in Table 1:
[0044] It can be seen from Table 1 that the surface energy of the antifouling coating layers prepared in Examples 1 to 3 is lower than 30 mJ / m 2 , having good antifouling ability. In comparative example 1, the zinc-based antibacterial agent is not well dispersed, so the surface energy of the antifouling coating layer is relatively high; in comparative example 2, a large amount of polydimethylsiloxane migrates to the surface of the antifouling coating layer, reducing the surface energy of the antifouling coating layer, but it is still lower than that of Examples 1 to 3; in comparative example 3, the nanosilver / silicon dioxide core-shell particles have a good dispersion and are evenly distributed on the surface of the antifouling coating layer, so they also have a lower surface energy.
[0045] The antifouling coating layers prepared in Examples 1 to 3 have good bonding strength on the epoxy resin board, and the bonding strength is greater than 1.70 MPa; in Comparative Example 1, only a zinc-based antibacterial agent is added, but due to poor dispersibility, the bonding performance of the antifouling coating and the epoxy intermediate paint is slightly improved; the inorganic antibacterial agent added in Comparative Example 2 has almost no improvement in the bonding performance of the antifouling coating and the epoxy intermediate paint, so the bonding strength is the smallest; although nanosilver / silicon dioxide core-shell particles are added in Comparative Example 3, since both nanosilver and silicon dioxide are nanoscale, a micron-nano binary rough structure cannot be formed, so the bonding strength is lower than that of Examples 1 to 3.
[0046] The antifouling coating layers prepared in Examples 1 to 3 have excellent antibacterial properties, all of which can reach 99.9%; Comparative Example 1 has poor dispersibility of the zinc-based antibacterial agent, resulting in reduced antibacterial properties; Comparative Example 2 uses a quaternary ammonium salt antibacterial agent, which has good antibacterial properties, but since polydimethylsiloxane is easily enriched on the surface during film formation, the antibacterial groups are covered and cannot fully exert their antibacterial effects, so the bactericidal rate is slightly lower than that of Examples 1 to 3; Comparative Example 3 contains silicon dioxide, so its dispersibility in the antifouling coating is improved, but due to the spherical pore structure coated with nano-silicon dioxide, the effective surface area of nano-silver is smaller than the effective surface area of nano-silver in the layered structure of the zinc-based antibacterial agent, so the bactericidal rate is slightly lower than that of Examples 1 to 3.
[0047] The antifouling coating layers prepared in Examples 1 to 3 have good impact resistance, and the maximum impact resistance height reaches 65 cm; Comparative Example 1 has low impact resistance due to poor dispersion of the zinc-based antibacterial agent in the antifouling coating layer; Comparative Example 2 has low impact resistance due to the absence of filler; Comparative Example 3 has high impact resistance due to good dispersibility of the nanosilver / silicon dioxide core-shell particles, but is still lower than that of Examples 1 to 3.
[0048] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An antifouling coating for steel structures in marine environments, characterized in that: The following raw materials are included by mass: 60-80 parts of polydimethylsiloxane, 20-30 parts of isophorone diisocyanate, 20-30 parts of modified antibacterial filler, 177.8-266.7 parts of tetrahydrofuran, 75.8-94.8 parts of N,N-dimethylformamide, 0.2-0.3 parts of chain extender, 0.2-0.3 parts of catalyst; The modified antibacterial filler is prepared by the following steps: In a reaction kettle, the zinc-based antibacterial agent is added to anhydrous ethanol, ultrasonically dispersed for 30-40 minutes, and then the pH value is adjusted to 7.8-8.2 with an ammonia solution, and then ethyl orthosilicate and 3-mercapto-1,2-propylene glycol are stirred and hydrolyzed in deionized water and added to the reaction kettle, the temperature is raised to 75-85° C., and the reaction is stirred for 4-5 hours. After the reaction is completed, the precipitate is filtered, washed with acetone, and vacuum dried at 40-50° C. to obtain a modified antibacterial filler; The zinc-based antibacterial agent is a micron-sized zirconium phosphate-loaded silver-zinc antibacterial agent.
2. The antifouling coating for steel structures in marine environments according to claim 1 is characterized in that: The chain extender is 1,4-butanediol; and the catalyst is dibutyltin dilaurate.
3. The antifouling coating for steel structures in marine environments according to claim 1 is characterized in that: The dosage ratio of the zinc-based antibacterial agent, anhydrous ethanol, ethyl orthosilicate, 3-mercapto-1,2-propylene glycol and deionized water is 4-5 g: 30-50 mL: 8-10 g: 3-4 g: 100-120 mL.
4. The method for preparing an antifouling coating for steel structures in marine environments according to claim 1, characterized in that: The preparation method comprises the following steps: In a reaction kettle, add isophorone diisocyanate and polydimethylsiloxane to a mixed solvent of tetrahydrofuran and N,N-dimethylformamide, heat to 65-75°C and stir for 50-70 minutes under nitrogen protection, then add modified antibacterial filler, heat to 80-85°C and stir for 50-70 minutes, then add 1,4-butanediol and dibutyltin dilaurate, continue stirring and reacting for 2-3 hours, after rotary evaporation of most of the solvent, add deionized water, filter the precipitate after obtaining it, and vacuum dry the precipitate at 50-60°C for 24-26 hours to obtain an antifouling coating.
5. The method for preparing an antifouling coating for steel structures in marine environments according to claim 4, characterized in that: The method for using the antifouling coating comprises the following steps: The antifouling coating, silane coupling agent and tetrahydrofuran are mixed and stirred to dissolve the antifouling coating. The antifouling coating is coated on the surface of the epoxy intermediate paint by a solution-casting film-forming method. The antifouling coating layer for the steel structure is obtained after the solvent is completely evaporated.
6. The method for preparing an antifouling coating for steel structures in marine environments according to claim 5, characterized in that: The antifouling coating, the silane coupling agent and tetrahydrofuran are used in a dosage ratio of 30-55 g: 0.5-1.5 g: 100-120 mL.
7. The method for preparing an antifouling coating for steel structures in marine environments according to claim 5, characterized in that: The silane coupling agent is any one of KH550, KH560 and KH570.
Citation Information
Cited By
Silver ion antibacterial non-woven fabric for mask and preparation method of silver ion antibacterial non-woven fabric
CN119392500A
Silver ion antibacterial non-woven fabric for masks and preparation method thereof
CN119392500B