Optical laminate and wound body

By designing an optical laminate structure and utilizing stretched polyester film and polymerizable liquid crystal compound, the peeling force and distance were controlled, solving the problem of cracking and breakage during the peeling of the separator on the vertically oriented liquid crystal cured film, and achieving good peeling and bonding of the separator.

CN118725759APending Publication Date: 2024-10-01SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410366253.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-02-15
Filing Date
2024-03-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When an adhesive layer with spacers and a surface protective film are laminated on a vertically oriented liquid crystal curing film, peeling off the spacers can easily cause the laminate to float, crack, or the adhesive layer to break, making it difficult to peel off and adhere well to the substrate.

Method used

An optical laminate structure is adopted, including a surface protective film, a first protective layer, a light absorption anisotropic layer, a second protective layer, and an adhesive layer. By controlling the peel force and distance, good peeling and adhesion of the separator are ensured. Stretched polyester film and polymeric liquid crystal compound are used to meet specific light absorption and peel force relationships.

Benefits of technology

It achieves good peeling and bonding of the separator, avoids cracks and fractures in the laminate, and improves the reliability and stability of the bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725759A_ABST
    Figure CN118725759A_ABST
Patent Text Reader

Abstract

The invention relates to an optical laminate and a wound body. The present invention addresses the problem of providing an optical laminate which is capable of satisfactorily peeling off a separator and which can be easily bonded to any adherend. [Solution] An optical laminate in which a surface protective film, a first protective layer, a light-absorbing anisotropic layer, a second protective layer, a first adhesive layer, and a separator are laminated in this order. The surface protective film and the separator each comprise a stretched polyester film. The peeling force F1 [N / 25 mm] between the surface protective film and the first protective layer and the peeling force F2 [N / 25 mm] between the separator and the first adhesive layer satisfy the relationships of formulae (4)-(6). The distance from the surface of the first protective layer on the surface protective film side to the surface of the second protective layer on the first adhesive layer side is 30 [mu] m or less. 0.05 < = F1 < = 0.30 (4); 0.02 < = F2 < = 0.15 (5); and 0.02 < = F1-F2 (6).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical layered body and a rolled body obtained by rolling the optical layered body. Background Art

[0002] In an organic EL (electroluminescent) display device, in order to reduce the hue difference between the front hue when viewed from the front and the oblique hue when viewed from an oblique direction when displaying white, it is known to use a stack having a vertically oriented liquid crystal cured film containing a dichroic pigment and a horizontally oriented phase difference film (for example, Patent Document 1).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-076920 Summary of the invention

[0006] Problems to be solved by the invention

[0007] The vertically oriented liquid crystal curing film is used by being attached to an adherend such as an organic EL display device or a circular polarizing plate, and therefore, an adhesive layer with a separator is sometimes laminated on one surface. For the other surface of the vertically oriented liquid crystal curing film, in order to suppress the attachment of dirt or damage associated with manufacturing and transportation, a surface protective film is sometimes laminated in a peelable manner. For a laminate obtained by laminating an adhesive layer with a separator and a surface protective film on the vertically oriented liquid crystal curing film, the adhesive layer exposed by peeling off the separator is attached to the adherend, and then the surface protective film is peeled off.

[0008] In particular, when the vertically oriented liquid crystal curing film is a thin film, if the isolation member is to be peeled off from the laminate, the following situations may occur: the isolation member alone cannot be peeled off, the laminate floats from the suction workbench that sucks and fixes the laminate, a crack-like stripe pattern is generated in the vertically oriented liquid crystal curing film, or the adhesive layer is broken.

[0009] An object of the present invention is to provide an optical layered body including a light absorption anisotropic layer, which can be easily bonded to any adherend while allowing a separator to be peeled off satisfactorily.

[0010] Means for solving problems

[0011] The present invention provides the following optical layered body and rolled body.

[0012] [1] An optical laminate comprising a surface protective film, a first protective layer, a light absorption anisotropic layer, a second protective layer, a first adhesive layer, and a separator laminated in this order,

[0013] The surface protection film and the separator both comprise a stretched polyester film.

[0014] The light absorption anisotropic layer comprises a polymer of a polymerizable liquid crystal compound and a dichroic pigment, and satisfies the following relationships (1) to (3):

[0015] The peeling force F1 [N / 25 mm] between the surface protection film and the first protection layer, and the peeling force F2 [N / 25 mm] between the separator and the first adhesive layer satisfy the relationship of the following formulas (4) to (6):

[0016] A distance from a surface of the first protective layer on the surface protection film side to a surface of the second protective layer on the first adhesive layer side is 30 μm or less.

[0017] Az>(Ax+Ay) / 2 (1)

[0018] 0.001≤Ax≤0.1 (2)

[0019] Ax(z=60°) / Ax≥5 (3)

[0020] 0.05≤F1≤0.30 (4)

[0021] 0.02≤F2≤0.15 (5)

[0022] 0.02≤F1-F2 (6)

[0023] [In formulas (1) to (3),

[0024] Ax, Ay, and Az are absorbances of the absorption maximum wavelength of the light absorption anisotropic layer within the wavelength range of 380 nm to 780 nm, and respectively represent absorbances of linearly polarized light vibrating in the x-axis direction, y-axis direction, and z-axis direction.

[0025] Ax(z=60°) is the absorbance at the absorption maximum wavelength, and indicates the absorbance of linearly polarized light vibrating in the x-axis direction when the light absorption anisotropic layer is rotated 60° about the y-axis.

[0026] The x-axis is any direction in the plane of the light absorption anisotropic layer.

[0027] The y-axis is a direction orthogonal to the x-axis in the plane of the light absorption anisotropic layer.

[0028] The aforementioned z-axis is a direction orthogonal to the aforementioned x-axis and the aforementioned y-axis.]

[0029] [2] The optical layered body according to [1], wherein the stretched polyester film included in the surface protection film has a thickness of 30 μm or more.

[0030] [3] The optical layered body according to [1] or [2], wherein the stretched polyester film included in the separator has a thickness of 30 μm or more.

[0031] [4] The optical layered body according to any one of [1] to [3], wherein the surface protection film is a layered body of a stretched polyester film and a second pressure-sensitive adhesive layer.

[0032] [5] The optical layered body according to any one of [1] to [4], wherein the stretched polyester film contained in the surface protection film and the separator is a biaxially stretched polyester film.

[0033] [6] The optical layered body according to any one of [1] to [5], wherein the surface protection film is in direct contact with the first protective layer.

[0034] [7] The optical layered body according to any one of [1] to [6], wherein the first protective layer is directly in contact with the light absorption anisotropic layer, or has only an orientation layer between the first protective layer and the light absorption anisotropic layer.

[0035] [8] The optical layered body according to any one of [1] to [7], wherein the light absorption anisotropic layer is in direct contact with the second protective layer.

[0036] [9] The optical layered body according to any one of [1] to [8], wherein the polymerizable liquid crystal compound is a liquid crystal compound that forms a smectic phase.

[0037]

[10] The optical layered body according to any one of [1] to [9], wherein the thickness of the first protective layer is 28 μm or less.

[0038]

[11] The optical layered body according to any one of [1] to

[10] , wherein the thickness of the second protective layer is 15 μm or less.

[0039]

[12] A wound body obtained by winding the optical layered body according to any one of [1] to

[11] .

[0040] Effects of the Invention

[0041] According to the present invention, the separator can be peeled off favorably from the optical layered body including the light absorption anisotropic layer, and the optical layered body can be easily bonded to any adherend. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] [ Figure 1] is a cross-sectional view schematically showing an optical layered body according to one embodiment of the present invention.

[0043] Description of Reference Numerals

[0044] 10 optical laminate, 11 surface protection film, 12 first protective layer, 13 light absorption anisotropic layer, 14 second protective layer, 15 first adhesive layer, 16 separator. DETAILED DESCRIPTION

[0045] Hereinafter, preferred embodiments of the optical layered body and the rolled body will be described with reference to the drawings.

[0046] <Optical laminate>

[0047] Figure 1 The optical layered body 10 schematically shows a cross-sectional view of an optical layered body according to one embodiment of the present invention. The optical layered body 10 includes a surface protection film 11, a first protective layer 12, a light absorption anisotropic layer 13, a second protective layer 14, a first pressure-sensitive adhesive layer 15, and a separator 16 laminated in this order.

[0048] The surface protection film 11 and the first protection layer 12 may be in direct contact. The surface protection film 11 is usually laminated on the first protection layer 12 in a peelable manner. The first protection layer 12 and the light absorption anisotropic layer 13 may be in direct contact, or only an orientation layer may be provided between the first protection layer 12 and the light absorption anisotropic layer 13. The light absorption anisotropic layer 13 and the second protection layer 14 may be in direct contact. The second protection layer 14 and the first adhesive layer 15 may be in direct contact. The first adhesive layer 15 and the spacer 16 are usually in direct contact. The spacer 16 is usually laminated on the first adhesive layer 15 in a peelable manner.

[0049] The surface protection film 11 and the separator 16 both include a stretched polyester film. Preferably, the surface protection film 11 and the separator 16 both include a biaxially stretched polyester film. The stretched polyester films included in the surface protection film 11 and the separator 16 may be the same or different.

[0050] The surface protection film 11 may be a laminate of a stretched polyester film and a second adhesive layer, and the stretched polyester film and the second adhesive layer may be directly in contact. When the surface protection film 11 has a second adhesive layer, the second adhesive layer side is arranged on the first protective layer 12 side in the optical laminate 10. By providing the surface protection film 11 with a second adhesive layer, when the optical laminate 10 is bent, the stress relaxation of the second adhesive layer can be utilized to suppress the generation of cracks in the light absorption anisotropic layer 13.

[0051] The surface protection film 11 may be a film obtained by subjecting the surface of a stretched polyester film to a release treatment.

[0052] The surface protection film 11 may also be a laminate of a stretched polyester film and a release force adjustment layer, and the stretched polyester film and the release force adjustment layer may be directly in contact. In the case where the release force adjustment layer side is arranged on the first protective layer 12 side in the optical laminate 10, it is preferred that the release force adjustment layer is directly in contact with the first protective layer. Thus, the step of laminating the second adhesive layer on the stretched polyester film can be omitted, and the overall thickness of the optical laminate 10 can be reduced, thereby helping to improve the bendability of the optical laminate 10. The release force adjustment layer can be formed, for example, using a silane coupling agent or the like.

[0053] The separator 16 may also be a film obtained by subjecting the surface of a stretched polyester film to a demolding treatment. The separator 16 may also be a laminate of a stretched polyester film and a release force adjusting layer, and the stretched polyester film and the release force adjusting layer may be directly in contact with each other. When the separator 16 has a release force adjusting layer, it is preferred that the release force adjusting layer is directly in contact with the first adhesive layer. The release force adjusting layer may be formed, for example, using a silane coupling agent or the like.

[0054] The light absorption anisotropic layer 13 contains a polymer of a polymerizable liquid crystal compound and a dichroic dye, and satisfies the relationships of the following formulae (1) to (3).

[0055] Az>(Ax+Ay) / 2 (1)

[0056] 0.001≤Ax≤0.1 (2)

[0057] Ax(z=60°) / Ax≥5 (3)

[0058] [In formulas (1) to (3),

[0059] Ax, Ay, and Az are absorbances of the absorption maximum wavelength of the light absorption anisotropic layer 13 within the wavelength range of 380 nm to 780 nm, and respectively represent absorbances of linearly polarized light vibrating in the x-axis direction, the y-axis direction, and the z-axis direction.

[0060] Ax (z=60°) is the absorbance at the absorption maximum wavelength, and indicates the absorbance of linearly polarized light vibrating in the x-axis direction when the light absorption anisotropic layer 13 is rotated 60° about the y-axis.

[0061] The x-axis is any direction in the plane of the light absorption anisotropic layer 13.

[0062] The y-axis is a direction orthogonal to the x-axis in the plane of the light absorption anisotropic layer 13.

[0063] The z-axis is a direction perpendicular to the x-axis and the y-axis.]

[0064] It is considered that by making the light absorption anisotropic layer 13 satisfy the relationships of the above formulas (1) to (3), the absorption axis of the dichroic pigment is oriented in a direction perpendicular to the plane of the light absorption anisotropic layer 13. Therefore, the light absorption anisotropic layer 13 can effectively transmit light from the front direction and effectively absorb light from the oblique direction.

[0065] The absorbance Az in the z direction in the above formula (1) is measured by making light incident on the side surface of the light absorption anisotropic layer 13, so it is difficult to measure. Therefore, when the angle formed by the vibration plane of the linearly polarized light as the measurement light and the x-y plane of the light absorption anisotropic layer 13 is 90°, with respect to this vibration plane, the x-y plane of the light absorption anisotropic layer 13 is tilted by 30° and 60° along the incident direction of the linearly polarized light for measurement, whereby the absorbance Az in the z direction can be calculated.

[0066] Specifically, the calculation can be performed using the following methods or the like.

[0067] In a state where the light absorption anisotropic layer 13 is rotated by 30° and 60° about the y-axis, the same linearly polarized light as the linearly polarized light for which Ax was measured is made incident, whereby the absorbances Ax(z = 30°) and Ax(z = 60°) are measured respectively. Similarly, in a state where the light absorption anisotropic layer 13 is rotated by 30° and 60° about the x-axis, the same linearly polarized light as the linearly polarized light for which Ay was measured is made incident, whereby the absorbances Ay(z = 30°) and Ay(z = 60°) are measured respectively.

[0068] At this time, if Ax(z = 30°) < Ax(z = 60°) and Ay(z = 30°) = Ay(z = 60°), then Ax(z = 30°) < Ax(z = 60°) < Ax(z = 90°) = Az, and if Ay(z = 30°) < Ay(z = 60°) and Ax(z = 30°) = Ax(z = 60°), then Ay(z = 30°) < Ay(z = 60°) < Ay(z = 90°) = Az. Therefore, it can be said that the relationship of formula (1) is necessarily satisfied.

[0069] Here, Ax(z = 90°) is the absorbance measured by making the same linearly polarized light as the linearly polarized light for which Ax was measured incident in a state where the light absorption anisotropic layer 13 is rotated by 90° about the y-axis. Ay(z = 90°) is the absorbance measured by making the same linearly polarized light as the linearly polarized light for which Ax was measured incident in a state where the light absorption anisotropic layer 13 is rotated by 90° about the x-axis.

[0070] Particularly, in the case where there is no absorption anisotropy in the x-y plane of the light absorption anisotropic layer 13, that is, when Ax and Ay are equal, Ax(z = 30°) = Ay(z = 30°) and Ax(z = 60°) = Ay(z = 60°). Here, let Ax(z = 30°) = Ay(z = 30°) = A(z = 30°), let Ax(z = 60°) = Ay(z = 60°) = A(z = 60°), and let Ax(z = 90°) = Ay(z = 90°) = A(z = 90°). Thus, if A(z = 30°) < A(z = 60°), then the relationship A(z = 30°) < A(z = 60°) < A(z = 90°) = Az is satisfied. In addition, if A(z = 30°) > (Ax + Ay) / 2, it can be said that Az necessarily satisfies formula (1).

[0071] The above-mentioned Ax and Ay refer to the absorbance in the front direction of the light absorption anisotropic layer 13. The smaller the values of Ax and Ay, the more precisely the dichroic pigment in the light absorption anisotropic layer 13 is oriented in the direction perpendicular to the plane. The values of Ax and Ay are preferably 0.3 or less. When the values of Ax and Ay are greater than 0.3, the coloring in the front direction of the light absorption anisotropic layer 13 becomes stronger, so there is a tendency for the front transmittance color difference when the light absorption anisotropic layer 13 is applied to a display device. Therefore, the values of Ax and Ay are each independently preferably 0.1 or less, more preferably 0.05 or less, and further preferably 0.02 or less. In addition, the lower limit values of the values of Ax and Ay are each independently usually 0.001 or more, can also be 0.003 or more, and can also be 0.005 or more. For the light absorption anisotropic layer 13 that satisfies the relationship of the above formula (2), it can be said that the absorption axis of the dichroic pigment is precisely oriented in the direction perpendicular to the plane of the light absorption anisotropic layer 13. When the absorbance Ax is greater than 0.10, the coloring in the front direction of the light absorption anisotropic layer 13 becomes stronger, so there is a tendency for the front color difference when combined and applied to an organic EL display device with, for example, a circular polarizing plate, etc.

[0072] In the light absorption anisotropic layer 13, Ax and Ay are preferably the same value. When Ax and Ay are different, there is absorption anisotropy in the plane of the light absorption anisotropic layer 13, and when the light absorption anisotropic layer 13 is applied to a display device, there is a tendency for the coloring of the front hue to increase.

[0073] For Ax(z = 60°) / Ax in the above formula (3), the larger its value, the more excellent the light absorption anisotropy is shown. It is preferably greater than 5, more preferably 7 or more, further preferably 10 or more, and in addition, preferably 50 or less.

[0074] In the light absorption anisotropic layer 13 satisfying the relationship of the above formula (3), it is considered that the absorption axis of the dichroic dye is oriented in a direction perpendicular to its plane, and therefore the light absorption anisotropic layer 13 can effectively absorb light from an oblique direction.

[0075] The above-mentioned Ax (z = 60°) refers to the oblique absorbance of the light absorption anisotropic layer 13, and can be appropriately selected according to the light leaking obliquely along the display device. Ax (z = 60°) is preferably 1.0 or less, more preferably 0.5 or less, and further preferably 0.3 or less. In addition, the lower limit is usually 0.001 or more, and can also be 0.003 or more. Considering its necessity, it is 0.01 or more.

[0076] The light absorption anisotropic layer 13 satisfying the relationship of the above-mentioned formulas (1) to (3) can be adjusted by, for example, the thickness of the light absorption anisotropic layer 13, the conditions of the manufacturing process of the light absorption anisotropic layer 13, the type or content of the dichroic dye and the polymerizable liquid crystal compound contained in the light absorption anisotropic layer forming composition used to obtain the light absorption anisotropic layer 13, etc.

[0077] The peel force F1 [N / 25 mm] between the surface protection film 11 and the first protection layer 12 and the peel force F2 [N / 25 mm] between the separator 16 and the first adhesive layer 15 satisfy the relationship of the following formulas (4) to (6).

[0078] 0.05≤F1≤0.30 (4)

[0079] 0.02≤F2≤0.15 (5)

[0080] 0.02≤F1-F2 (6)

[0081] The peeling force F1 is preferably 0.08N / 25mm to 0.28N / 25mm, more preferably 0.1N / 25mm to 0.25N / 25mm, and may be 0.12N / 25mm to 0.23N / 25mm. The peeling force F2 is preferably 0.03N / 25mm to 0.13N / 25mm, more preferably 0.05N / 25mm to 0.10N / 25mm, and may be 0.06N / 25mm to 0.08N / 25mm. The difference (F1-F2) between the peeling force F1 and the peeling force F2 is preferably 0.03 or more, more preferably 0.04 or more, and may be 0.05 or more, and may be 0.07 or more, and is usually 0.2 or less.

[0082] The peel force F1 can be adjusted by the surface state of the stretched polyester film included in the surface protection film 11 due to the release treatment, etc., the composition of the adhesive composition used to form the second adhesive layer when the surface protection film 11 includes the second adhesive layer, the type of the silane coupling agent used to form the release force adjustment layer when the surface protection film 11 includes the release force adjustment layer, the surface treatment of the bonding surface of the surface protection film 11 and the first protective layer 12, etc. The peel force F2 can be adjusted by the surface state of the separator 16 due to the release treatment, etc., the composition of the adhesive composition used to form the first adhesive layer 15, the surface treatment of the bonding surface of the separator 16 and the first adhesive layer 15, etc. The peel forces F1 and F2 can be measured by the method described in the examples described later.

[0083] The distance D from the surface of the first protective layer 12 on the surface protective film 11 side to the surface of the second protective layer 14 on the first adhesive layer 15 side is 30 μm or less. The distance D is preferably 28 μm or less, and may be 25 μm or less, or 20 μm or less, and is usually 2 μm or more, or 5 μm or more. If the distance D is reduced, it is easy to suppress the reduction in the visual recognition of the bent portion when the optical laminate is bent in a manner where the surface protective film becomes the inner side.

[0084] The laminate obtained by removing the surface protection film 11 and the separator 16 from the optical laminate 10 can be laminated on an adherend such as an organic EL display device or a circular polarizing plate as an antireflection film and used. This can suppress the change in color tone depending on the angle at which the image of the display device is viewed.

[0085] When the laminate obtained by removing the surface protection film 11 and the spacer 16 from the optical laminate 10 is laminated on the adherend, it can be carried out, for example, as described below. First, on a suction workbench with suction holes, the optical laminate 10 is fixed by suction in such a way that the surface protection film 11 side becomes the suction workbench side. In this state, the spacer 16 of the optical laminate 10 is peeled off. Next, the first adhesive layer 15 exposed by peeling off the spacer 16 is attached to the adherend. Then, the surface protection film 11 can be peeled off at an appropriate time. When the distance D is small as in the optical laminate 10, the following situation exists: the optical laminate as a whole easily follows the action of peeling off the spacer and it is difficult to peel off only the spacer, the optical laminate floats from the suction workbench where the optical laminate is fixed by suction, and a crack-like stripe pattern is generated in any one of the first protective layer, the light absorption anisotropic layer, the second protective layer and the first adhesive layer as the spacer is peeled off, or these layers are broken. However, since the optical layered body 10 satisfies the relationships of the above-mentioned formulae (4) to (6), only the separator 16 can be peeled off satisfactorily and can be easily bonded to an adherend.

[0086] <Wound body>

[0087] The roll is obtained by rolling up the optical layered body 10. The optical layered body described above can be used as the optical layered body 10. The optical layered body 10 constituting the roll is preferably a long-length optical layered body.

[0088] The roll diameter (diameter) of the roll can be, for example, from 50 mm to 1000 mm. The long strip of optical laminated body wound into a roll to form a roll can, for example, have a length of from 5 m to 10000 m in the length direction of the winding direction of the roll, or from 5 m to 5000 m, or from 100 m to 5000 m, or from 500 m to 3000 m, or from 1000 m to 3000 m. The length can be from 300 mm to 5000 mm in the width direction of the winding axis direction of the roll, or from 500 mm to 3000 mm, or from 500 mm to 2500 mm, or from 500 mm to 2000 mm.

[0089] Hereinafter, the layers included in the optical layered body, the components contained in the layers, and the like will be described in detail.

[0090] (Surface protection film)

[0091] The surface protection film includes a stretched polyester film. The surface protection film can be a laminate of a stretched polyester film and a second adhesive layer, can be a film obtained by subjecting the surface of the stretched polyester film to a demolding treatment, or can be a laminate of a stretched polyester film and a release force regulating layer. As a demolding treatment, a method of forming a release layer by coating a release agent or the like can be cited. As a release agent, a silicone release agent and a fluorine release agent can be cited. The stretched polyester film is preferably a biaxially stretched polyester film. The release force regulating layer can be formed by, for example, coating a silane coupling agent or the like.

[0092] The thickness of the stretched polyester film is preferably 30 μm or more, more preferably 35 μm or more, and may be 40 μm or more, and is usually 100 μm or less. The thickness of the second adhesive layer is 5 μm or more, and may be 10 μm or more, or 15 μm or more, and is usually 30 μm or less.

[0093] The stretched polyester film is a film obtained by uniaxially stretching or biaxially stretching a polyethylene terephthalate (PET) film, and is preferably a film obtained by biaxially stretching a polyethylene terephthalate (PET) film.

[0094] The tensile modulus of the stretched polyester film at a temperature of 23°C and a relative humidity of 55% is preferably 4000 MPa or more, and may be 5000 MPa or more, or 6000 MPa or more, and is usually 20000 MPa or less. The tensile modulus can be calculated from the slope of the initial straight line in the obtained stress-strain curve by clamping the two ends of a test piece of 100 mm in length and 25 mm in width in the long side direction with the upper and lower clamps of a tensile testing machine in a manner that the interval between the clamps is 5 cm, and stretching the test piece at a tensile speed of 1 mm / min under an environment of a temperature of 23°C and a relative humidity of 55%.

[0095] (1st protective layer)

[0096] The first protective layer can support the light absorption anisotropic layer. The first protective layer can be a layer to which a composition for forming a light absorption anisotropic layer is to be coated. The first protective layer can be a single-layer structure or a multi-layer structure. When an orientation layer is used when forming the light absorption anisotropic layer, the orientation layer can be formed on the side of the surface of the first protective layer where the light absorption anisotropic layer is to be formed.

[0097] The first protective layer may include one or more of a film substrate, a coating layer, and a glass substrate. The first protective layer preferably includes a film substrate or a coating layer, and may be a laminate of a film substrate and other layers such as a coating layer.

[0098] Examples of the resin constituting the film substrate include olefin resins such as polyethylene and polypropylene; cyclic olefin resins having a ring system or norbornene structure; polyvinyl alcohol; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; (meth) acrylic resins; cellulose ester resins such as cellulose triacetate, cellulose diacetate, and cellulose acetate propionate; polyimide resins; polycarbonate; polysulfone; polyethersulfone; polyetherketone; polyphenylene sulfide; polyphenylene ether, etc. The so-called "(meth) acrylic-" refers to at least one of "acrylic-" and "methacrylic-". The same applies to expressions such as (meth)acryloyl.

[0099] As the film substrate, a commercially available cellulose ester resin film can be used. Examples of such cellulose ester resin films include "Fujitac Film" (manufactured by Fuji Photo Film Co., Ltd.); "KC8UX2M", "KC8UY" and "KC4UY" (all manufactured by Konica Minolta Opto Co., Ltd.).

[0100] As the cyclic olefin resin constituting the film substrate, commercially available cyclic olefin resins can also be used. As such cyclic olefin resins, "Topas" (registered trademark) (manufactured by Ticona (Germany)), "ARTON" (registered trademark) (manufactured by JSR Corporation), "ZEONOR" (registered trademark), "ZEONEX" (registered trademark) (manufactured by Zeon Corporation of Japan) and "Apel" (registered trademark) (manufactured by Mitsui Chemicals, Inc.) can be cited. These cyclic olefin resins can be made into film substrates by known means such as solvent casting method and melt extrusion method.

[0101] As the film substrate, a commercially available cyclic olefin resin substrate may also be used. Examples of such cyclic olefin resin substrates include "Escena" (registered trademark), "SC A40" (registered trademark) (all manufactured by Sekisui Chemical Co., Ltd.), "ZEON ORFILM" (registered trademark) (manufactured by OPTES Co., Ltd.), and "ARTONFILM" (registered trademark) (manufactured by JSR Co., Ltd.).

[0102] When the first protective layer is a coating, for example, the coating may be formed on a film substrate, and after the light absorption anisotropic layer is formed on the coating, the film substrate may be peeled off, thereby using the coating as the first protective layer. In this case, the film substrate is easily peeled off by subjecting the surface of the film substrate on the side where the coating is to be formed to a release treatment (a release layer is formed by applying a release agent or the like). The film substrate to be peeled off may also be used as the surface protective film described above.

[0103] Examples of the coating layer include: a layer formed by applying a hard coating agent, an easy-adhesion composition, a coupling agent, etc. on the surface of a film substrate; a layer formed by applying a reactive monomer or a reactive polymer, etc., and then irradiating them with active energy rays to graft polymerize them; and the like. As the film substrate having a coating layer, a hard coating film having a hard coating layer as a coating layer is preferred. When the first protective layer is a hard coating film, it is preferred to laminate a light absorbing anisotropic layer on the hard coating side. As the coating layer, a hard coating layer is preferred.

[0104] The hard coat layer is preferably a cured layer of a curable composition containing an active energy ray-curable resin, and more preferably a cured layer of a composition containing an ultraviolet-curable resin. The curable composition containing an ultraviolet-curable resin preferably contains a (meth)acrylic compound as a curable component, and the hard coat layer is preferably formed of a (meth)acrylic resin. The (meth)acrylic compound is a compound having at least one (meth)acryloyl group, and may be a monomer, an oligomer, or a polymer.

[0105] As (meth) acrylic compounds, for example, (meth) acrylic compounds such as monofunctional (meth) acrylic ester compounds and multifunctional (meth) acrylic ester compounds; carbamate (meth) acrylic ester compounds such as multifunctional carbamate (meth) acrylic ester compounds; epoxy (meth) acrylic ester compounds such as multifunctional epoxy (meth) acrylic ester compounds; carboxyl modified epoxy (meth) acrylic ester compounds; polyester (meth) acrylic ester compounds, etc. They can be used alone or in combination. Among them, preferably a multifunctional (meth) acrylic ester compound or a carbamate (meth) acrylic ester compound, more preferably a combination of a multifunctional (meth) acrylic ester compound and a carbamate (meth) acrylic ester.

[0106] The content of the multifunctional (meth)acrylate compound is preferably 50 to 100 parts by mass, more preferably 60 to 95 parts by mass, and further preferably 70 to 90 parts by mass, relative to 100 parts by mass of the solid content of the curable composition. In this specification, the solid content of the curable composition refers to the total amount of the components after removing the solvent from the curable composition when the curable composition contains a solvent.

[0107] The curable composition may contain a polymerization initiator in addition to the curable component. Examples of the polymerization initiator include photopolymerization initiators and radical polymerization initiators, and known polymerization initiators may be used.

[0108] The curable composition can be cured by being coated on a film substrate and then irradiated with active energy rays to polymerize curable components such as a (meth)acrylic compound.

[0109] The hard coating layer preferably shows a value of 8B or harder in the pencil hardness test (measured by placing the film substrate on a glass plate) specified in JIS K 5600-5-4:1999 "General Test Methods for Coatings - Part 5: Mechanical Properties of Coatings - Section 4: Scratch Hardness (Pencil Method)", and may also be 5B or harder.

[0110] The surface of the first protective layer on the side where the light absorption anisotropic layer is to be formed may be subjected to a surface treatment. Examples of the surface treatment method include a method of subjecting the surface of the first protective layer to a corona treatment or a plasma treatment in an atmosphere ranging from vacuum to atmospheric pressure, a method of subjecting the surface of the first protective layer to a laser treatment, a method of subjecting the surface of the first protective layer to an ozone treatment, a method of subjecting the surface of the first protective layer to a saponification treatment, and the like.

[0111] The thickness of the first protective layer is preferably 28 μm or less, and may be 0.5 μm or more and 25 μm or less, 1 μm or more and 20 μm or less, 1 μm or more and 15 μm or less, 1 μm or more and 10 μm or less, or 1 μm or more and 5 μm or less. If the thickness of the first protective layer is reduced, it is easy to suppress the reduction in the visual recognition of the bent portion when the optical laminate is bent in a manner where the surface protective film is on the inside.

[0112] The thickness of the film substrate that can be included in the first protective layer is preferably thin from the viewpoint of quality to the extent that it can be handled in a practical manner, but if it is too thin, the strength decreases and there is a tendency for poor processability. From this viewpoint, the thickness of the film substrate is preferably 5 μm to 28 μm, more preferably 10 μm to 25 μm, and further preferably 10 μm to 23 μm.

[0113] If the thickness of the coating layer that the first protective layer may include is too thin, the strength is reduced, and if it is too thick, there is a tendency to generate cracks, etc. From this viewpoint, the thickness of the coating layer is preferably 0.5 μm to 20 μm, more preferably 1 μm to 15 μm, further preferably 1 μm to 10 μm, and further preferably 1 μm to 5 μm.

[0114] The tensile modulus of the first protective layer at a temperature of 23° C. and a relative humidity of 55% is preferably 100 MPa to 10,000 MPa, may be 200 MPa to 8,000 MPa, or may be 300 MPa to 6,000 MPa. The tensile modulus can be measured by the above method.

[0115] (Light Absorption Anisotropic Layer)

[0116] The light absorption anisotropic layer contains a polymer of a polymerizable liquid crystal compound and a dichroic pigment. The light absorption anisotropic layer may contain one polymer of a polymerizable liquid crystal compound or two or more polymerizable liquid crystal compound polymers. The light absorption anisotropic layer may contain one dichroic pigment or two or more dichroic pigments.

[0117] The light absorption anisotropic layer can be formed using a composition for forming a light absorption anisotropic layer containing a polymerizable liquid crystal compound and a dichroic pigment. In the composition for forming a light absorption anisotropic layer, as a solid component, in addition to the polymerizable liquid crystal compound and the dichroic pigment, a non-liquid crystal compound having a polymerizable group, and additives such as a polymerization initiator, a leveling agent, an orientation promoter, an antioxidant, and a photosensitizer may be included as described later. Therefore, the light absorption anisotropic layer may also contain a polymer of a non-liquid crystal compound having a polymerizable group and additives.

[0118] The polymerizable liquid crystal compound is preferably a liquid crystal compound that forms a smectic phase. The polymer of the polymerizable liquid crystal compound may or may not show liquid crystal properties. The light absorption anisotropic layer may be formed by a composition for forming a light absorption anisotropic layer comprising a polymerizable liquid crystal compound and a dichroic pigment, and may be a liquid crystal cured film (a cured material layer of a polymerizable liquid crystal compound) formed by polymerizing and curing the polymerizable liquid crystal compound in the composition for forming a light absorption anisotropic layer. The polymer of the polymerizable liquid crystal compound is a polymer obtained by polymerizing the polymerizable liquid crystal compounds with each other, and the polymerizable liquid crystal compound may be polymerized with a non-liquid crystal compound having a polymerizable group, or the polymerizable liquid crystal compound may be polymerized with a dichroic pigment.

[0119] Relative to 100 parts by mass of the light absorption anisotropic layer, the content of the polymer of the polymerizable liquid crystal compound in the light absorption anisotropic layer is preferably 40 parts by mass or more and 99.9 parts by mass or less, and may be 60 parts by mass or more and 99 parts by mass or less, or 70 parts by mass or more and 99 parts by mass or less. If the content of the polymer of the polymerizable liquid crystal compound is within the above range, there is a tendency that the orientation of the polymer of the polymerizable liquid crystal compound when forming the light absorption anisotropic layer becomes higher. The proportion of the polymer of the polymerizable liquid crystal compound in the light absorption anisotropic layer can be calculated in the form of the proportion of the polymerizable liquid crystal compound (in the case of containing more than 2 kinds) relative to 100 parts by mass of the solid content of the light absorption anisotropic layer forming composition for forming the light absorption anisotropic layer. The so-called solid content of the light absorption anisotropic layer forming composition refers to all the components after removing volatile components such as organic solvents from the light absorption anisotropic layer forming composition.

[0120] The content of the dichroic pigment in the light absorption anisotropic layer is preferably 0.1 to 30 parts by mass, or 0.5 to 20 parts by mass, or 1 to 10 parts by mass, or 1 to 5 parts by mass. The content ratio of the dichroic pigment in the light absorption anisotropic layer can be calculated as the ratio of the dichroic pigment to 100 parts by mass of the solid content of the light absorption anisotropic layer-forming composition. The content of the dichroic pigment when the light absorption anisotropic layer includes two or more dichroic pigments refers to the total amount thereof.

[0121] The thickness of the light absorption anisotropic layer is preferably 0.2 μm to 5.0 μm, more preferably 0.5 μm to 4.0 μm, and further preferably 0.5 μm to 3.0 μm. If the thickness of the light absorption anisotropic layer is reduced, the light absorption from the oblique direction tends to be weakened, and if the thickness is increased, the orientation of the dichroic dye tends to be disordered, thereby tending to reduce the transmission characteristics in the front direction.

[0122] The surface of the light-absorbing anisotropic layer on the side where the second protective layer is to be formed may be subjected to a surface treatment. Examples of the surface treatment method include a method of subjecting the surface of the light-absorbing anisotropic layer to a corona treatment or a plasma treatment in an atmosphere ranging from vacuum to atmospheric pressure, a method of subjecting the surface to a laser treatment, a method of subjecting the surface to an ozone treatment, a method of subjecting the surface to a flame treatment, and the like.

[0123] (Polymerizable Liquid Crystal Compound)

[0124] The polymerizable liquid crystal compound contained in the light absorption anisotropic layer-forming composition is used to align the dichroic dye by guest-host interaction. The polymerizable liquid crystal compound is a compound having one or more polymerizable groups in the molecule and having liquid crystallinity.

[0125] A polymerizable group refers to a group that participates in the polymerization reaction, preferably a photopolymerizable group. Here, the so-called photopolymerizable group refers to a group that can participate in the polymerization reaction using active free radicals, acids, etc. generated by the photopolymerization initiator described later. As a polymerizable group, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, (meth)acryloyl, (meth)acryloyloxy, oxacyclopropyl, oxetane, etc. can be cited. Among them, preferably (meth)acryloyl, (meth)acryloyloxy, vinyloxy, oxacyclopropyl, and oxetane, more preferably (meth)acryloyl and (meth)acryloyloxy. Liquid crystal can be thermotropic liquid crystal or lyotropic liquid crystal, and when mixed with the above-mentioned dichroic pigment, it is preferably thermotropic liquid crystal. In this specification, the so-called (meth)acryloyl refers to at least one of acryloyl and methacryloyl. The same is true for the expressions such as "(meth)acryloyl-".

[0126] When a polymer of a polymerizable liquid crystal compound is formed by polymerization reaction and exhibits light absorption anisotropy in the form of a film containing the polymer and a dichroic pigment, the liquid crystal state displayed by the polymerizable liquid crystal compound is a smectic phase, and from the viewpoint of high performance, it is preferably a high-order smectic phase. Among them, it is more preferably a high-order smectic polymerizable liquid crystal compound that forms a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, or a smectic L phase, and it is further preferably a high-order smectic polymerizable liquid crystal compound that forms a smectic B phase, a smectic F phase, or a smectic I phase. If the liquid crystal phase formed by the polymerizable liquid crystal compound is these high-order smectic phases, it is possible to manufacture a light absorption anisotropic layer with higher light absorption anisotropy. In this way, a light absorption anisotropic layer with high light absorption anisotropy can obtain a Bragg peak from a high-order structure such as a hexagonal phase and a crystalline phase in an X-ray diffraction measurement. The Bragg peak is a peak derived from a periodic structure of molecular orientation. For a light-absorbing anisotropic layer, its periodic interval can be From the viewpoint of obtaining higher light absorption anisotropic characteristics, the light absorption anisotropic layer preferably contains a polymer of a polymerizable liquid crystal compound oriented in a smectic phase.

[0127] The polymerizable liquid crystal compound may be a monomer, an oligomer obtained by polymerizing a polymerizable group, or a polymer. As such a polymerizable liquid crystal compound, a known polymerizable liquid crystal compound may be used, for example, a polymerizable liquid crystal compound described in Japanese Patent Publication No. 2020-76920 and Japanese Patent No. 6728581 may be cited.

[0128] (Dichroic Pigments)

[0129] The so-called dichroic pigment refers to a pigment having a property that the absorbance in the long axis direction of the molecule is different from the absorbance in the short axis direction of the molecule. As a dichroic pigment, it is preferred to have the characteristic of absorbing visible light, and more preferably to have an absorption maximum wavelength (λmax) within the range of 380 to 680 nm.

[0130] As such dichroic pigment, for example, acridine pigment, oxazine pigment, cyanine pigment, naphthalene pigment, azo pigment and anthraquinone pigment etc. can be enumerated, wherein, preferably azo pigment.As azo pigment, monoazo pigment, disazo pigment, triazo pigment, tetraazo pigment and stilbene azo pigment etc. can be enumerated, preferably disazo pigment and triazo pigment.Dichroic pigment can be separately also can combine more than 2 kinds, but preferably according to the wavelength range of light absorption anisotropy requirement in light absorption anisotropy layer and use in combination more than 2 kinds.

[0131] Examples of the azo dye include compounds represented by formula (I) (hereinafter referred to as "compound (I)" as the case may be).

[0132] K 1 (-N=NK 2 ) p -N=NK 3 (I)

[0133] [In formula (I),

[0134] K 1 and K 3 Each independently represents a phenyl group which may have a substituent, a naphthyl group which may have a substituent, or a monovalent heterocyclic group which may have a substituent.

[0135] K 2 It represents a p-phenylene group which may have a substituent, a naphthalene-1,4-diyl group which may have a substituent, or a divalent heterocyclic group which may have a substituent.

[0136] p represents an integer of 1-4.

[0137] When p is an integer greater than or equal to 2, multiple K 2 They can be the same or different from each other.

[0138] In the range that shows absorption in the visible light region, the -N=N- bond can be replaced by a -C=C-, -COO-, -NHCO-, or -N=CH- bond.]

[0139] Examples of the monovalent heterocyclic group include groups obtained by removing one hydrogen atom from heterocyclic compounds such as quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, and benzoxazole. Examples of the divalent heterocyclic group include groups obtained by removing two hydrogen atoms from the above heterocyclic compounds.

[0140] As K 1 and K 3 The phenyl, naphthyl and monovalent heterocyclic groups in 2 The substituents optionally possessed by the p-phenylene, naphthalene-1,4-diyl and divalent heterocyclic groups include alkyl groups having 1 to 4 carbon atoms; alkoxy groups having 1 to 4 carbon atoms such as methoxy, ethoxy and butoxy; fluoroalkyl groups having 1 to 4 carbon atoms such as trifluoromethyl; cyano; nitro; halogen atoms; substituted or unsubstituted amino groups such as amino, diethylamino and pyrrolidinyl (the so-called substituted amino group refers to an amino group having 1 or 2 alkyl groups having 1 to 6 carbon atoms, or an amino group obtained by two substituted alkyl groups bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. The unsubstituted amino group is -NH2.).

[0141] Among the compounds (I), the compounds represented by any one of formula (I-1) to (I-8) are preferred, the compounds represented by any one of formula (I-1) to (I-3) are more preferred, and the compounds represented by any one of formula (I-1) and (I-3) are further preferred.

[0142] [Chemical formula 1]

[0143]

[0144] [In formulas (I-1) to (I-8),

[0145] B 1 ~B 30 Each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the definitions of the substituted amino group and the unsubstituted amino group are as described above), a chlorine atom or a trifluoromethyl group.

[0146] n1 to n4 independently represent integers of 0 to 3.

[0147] When n1 is 2 or more, multiple B 2 They can be the same or different from each other.

[0148] When n2 is 2 or more, multiple B 6 They can be the same or different from each other.

[0149] When n3 is 2 or more, multiple B 9 They can be the same or different from each other.

[0150] When n4 is 2 or more, multiple B 14 They may be the same or different from each other.]

[0151] As the anthraquinone dye, a compound represented by formula (I-9) is preferred.

[0152] [Chemical formula 2]

[0153]

[0154] [In formula (I-9),

[0155] R 1 ~R 8 Each independently represents a hydrogen atom, -R x 、-NH2、-NHR x 、-NR x 2. -SR x or halogen atoms.

[0156] R xrepresents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]

[0157] As the above-mentioned oxazinone coloring matter, a compound represented by formula (I-10) is preferred.

[0158] [Chemical formula 3]

[0159]

[0160] [In formula (I-10),

[0161] R 9 ~R 15 Each independently represents a hydrogen atom, -R x 、-NH2、-NHR x 、-NR x 2. -SR x or halogen atoms.

[0162] Rx represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]

[0163] The acridine dye is preferably a compound represented by formula (I-11).

[0164] [Chemical formula 4]

[0165]

[0166] [In formula (I-11),

[0167] R 16 ~R 23 Each independently represents a hydrogen atom, -R x 、-NH2、-NHR x 、-NR x 2. -SR x or halogen atoms.

[0168] R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]

[0169] In formula (I-9), formula (I-10) and formula (I-11), R x Examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, propyl, butyl, pentyl and hexyl, and examples of the aryl group having 6 to 12 carbon atoms include phenyl, toluoyl, xylyl and naphthyl.

[0170] As the cyanine dye, a compound represented by formula (I-12) and a compound represented by formula (I-13) are preferred.

[0171] [Chemical formula 5]

[0172]

[0173] [In formula (I-12),

[0174] D 1 and D 2 Each independently represents a group represented by any one of formula (I-12a) to formula (I-12d).

[0175] [Chemical formula 6]

[0176]

[0177] n5 represents an integer from 1 to 3.]

[0178] [Chemical formula 7]

[0179]

[0180] [In formula (I-13),

[0181] D 3 and D 4 Each independently represents a group represented by any one of formula (I-13a) to formula (I-13h).

[0182] [Chemical formula 8]

[0183]

[0184] n6 represents an integer from 1 to 3.]

[0185] Among these dichroic dyes, azo dyes are preferred from the viewpoint of orientation.

[0186] Regarding the content of the dichroic pigment in the light absorption anisotropic layer forming composition (the total amount when two or more are included), from the viewpoint of obtaining good light absorption characteristics, it is generally 1 mass part or more and 60 mass parts or less, preferably 1 mass part or more and 40 mass parts or less, and more preferably 1 mass part or more and 20 mass parts or less, relative to 100 mass parts of polymerizable liquid crystal compounds. When the content of the dichroic pigment is less than this range, light absorption becomes insufficient and sufficient light absorption anisotropic characteristics cannot be obtained. When it is more than this range, there is a situation where the orientation of the liquid crystal molecules of the polymerizable liquid crystal compound is hindered.

[0187] (Method for forming light absorption anisotropic layer)

[0188] The light absorption anisotropic layer can be formed, for example, by coating a light absorption anisotropic layer-forming composition on the first protective layer. The light absorption anisotropic layer-forming composition contains a polymerizable liquid crystal compound and a dichroic dye, and may also contain a non-liquid crystal compound having a polymerizable group, a solvent, and additives described below.

[0189] The coating layer formed by applying the composition for forming anisotropic light-absorbing layer is subjected to a drying treatment for removing the solvent, etc. The coating layer after the drying treatment is irradiated with active energy rays, etc. to polymerize the polymerizable liquid crystal compound, thereby forming a light-absorbing anisotropic layer as a cured layer (liquid crystal cured film) of the composition for forming anisotropic light-absorbing layer on the first protective layer. The composition for forming anisotropic light-absorbing layer can be applied to the surface of the first protective layer, or to the surface of the alignment layer formed on the surface of the first protective layer.

[0190] Examples of a method for applying the light absorption anisotropic layer-forming composition include known methods such as coating methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator, and printing methods such as flexographic methods.

[0191] The coating layer of the light-absorbing anisotropic layer-forming composition formed on the first protective layer is preferably dried. When the light-absorbing anisotropic layer-forming composition contains a solvent, the solvent in the coating layer can be removed by drying the coating layer. As the drying method, known methods can be mentioned, and one or more methods of natural drying method, heating drying method, ventilation drying method, reduced pressure drying method, etc. can be mentioned.

[0192] The drying conditions in the drying process can be appropriately determined according to the components contained in the composition for forming anisotropic light-absorbing layer. For example, the drying temperature in the drying process is 50° C. to 150° C., or 60° C. to 120° C. The drying time in the drying process is 15 seconds to 10 minutes, or 0.5 minutes to 5 minutes.

[0193] In the case of performing a heat treatment during the drying treatment, the polymerizable liquid crystal compound contained in the composition for forming the light absorbing anisotropic layer may be heated to a temperature above the liquid crystal phase transition temperature at which the phase transition occurs in the polymerizable liquid crystal compound contained in the composition for forming the light absorbing anisotropic layer, thereby orienting the polymerizable liquid crystal compound while removing the solvent in the coating layer. In particular, in the case of orienting the polymerizable liquid crystal compound forming the smectic phase in a direction perpendicular to the surface of the light absorbing anisotropic layer, it is preferred to heat in a temperature region that is converted to the smectic phase. Thus, the polymerizable liquid crystal compound can be oriented in a direction perpendicular to the surface of the light absorbing anisotropic layer, and along with the orientation of the polymerizable liquid crystal compound, the dichroic pigment can also be oriented.

[0194] After drying the coating layer formed on the first protective layer, the polymerizable liquid crystal compound and the dichroic dye are irradiated with active energy rays in an aligned state to polymerize and cure the polymerizable liquid crystal compound, thereby forming a light absorption anisotropic layer.

[0195] As a method for polymerizing a polymerizable liquid crystal compound, photopolymerization is preferred. Photopolymerization can be implemented by irradiating a laminated structure comprising a coating layer obtained by coating a light-absorbing anisotropic layer-forming composition on a first protective layer with active energy rays. As the active energy rays irradiated, it can be appropriately selected according to the type of polymerizable liquid crystal compound contained in the coating layer (especially the type of photopolymerizable functional group possessed by the polymerizable liquid crystal compound), the type of photopolymerization initiator when a photopolymerization initiator is included, and their amount. Specifically, one or more lights selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α rays, β rays, and γ rays can be cited. Among them, from the aspect of easy control of the progress of the polymerization reaction, and the aspect that a device widely used in the art can be used as a photopolymerization device, ultraviolet light is preferred, and the type of polymerizable liquid crystal compound is preferably selected in a manner that can be photopolymerized using ultraviolet light.

[0196] As the light source of active energy rays, for example, there can be mentioned a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in a wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, a metal halide lamp, and the like.

[0197] The UV radiation intensity is usually 10mW / cm 2 ~3,000mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a cationic polymerization initiator or a free radical polymerization initiator. The irradiation time is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and further preferably 10 seconds to 1 minute. When irradiation is performed once or multiple times with such an ultraviolet irradiation intensity, the cumulative light amount is 10 mJ / cm 2 ~3,000mJ / cm 2 , preferably 50 mJ / cm 2 ~2,000mJ / cm 2 , more preferably 100 mJ / cm 2 ~1,000mJ / cm 2When the accumulated light amount is below this range, the curing of the polymerizable liquid crystal compound may be insufficient, and good transferability may not be obtained when the light absorption anisotropic layer on the first protective layer is transferred to the adherend. On the contrary, when the accumulated light amount is above this range, the light absorption anisotropic layer may be colored.

[0198] (Non-liquid crystal compound having a polymerizable group)

[0199] A non-liquid crystal compound having a polymerizable group (hereinafter, sometimes referred to as a "non-liquid crystal compound"). It is a compound having a polymerizable group but not having liquid crystal. As the polymerizable group possessed by the non-liquid crystal compound, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, (methyl) acryloyl, (methyl) acryloyloxy, oxirane, oxetane, etc. can be cited. Among them, preferred polymerizable groups are (methyl) acryloyl, (methyl) acryloyloxy, vinyloxy, oxirane, and oxetane, and more preferred polymerizable groups are (methyl) acryloyl and (methyl) acryloyloxy, and further preferred polymerizable groups are (methyl) acryloyloxy. The polymerizable group in the non-liquid crystal compound can be one kind or a combination of two or more kinds, but is preferably a polymerizable group identical to the polymerizable group possessed by the polymerizable liquid crystal compound.

[0200] The number of polymerizable groups possessed by the non-liquid crystal compound is not particularly limited, and may be, for example, 1 to 20. From the viewpoint of further improving the film strength of the light absorption anisotropic layer, the number is preferably 2 to 10, and more preferably 3 to 6. When the non-liquid crystal compound has two or more polymerizable groups, the polymerizable groups may be the same or different from each other.

[0201] As non-liquid crystal compounds, monofunctional (meth) acrylates and multifunctional (meth) acrylates can be cited. Monofunctional acrylates and multifunctional acrylates as non-liquid crystal compounds having polymerizable groups are non-liquid crystals, and therefore, are preferably compounds without a mesogenic structure. Monofunctional acrylates and multifunctional acrylates may contain a carbamate structure, an amino structure, an epoxy structure, an ethylene glycol structure, and / or a polyester structure in the molecule.

[0202] (Solvent)

[0203] The solvent that may be contained in the light absorption anisotropic layer-forming composition is preferably a solvent that can completely dissolve the polymerizable liquid crystal compound, and is preferably a solvent that is inactive with respect to the polymerization reaction of the polymerizable liquid crystal compound. As the solvent, for example, alcohol solvents such as methanol, ethanol, ethylene glycol, isopropanol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether can be cited; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorinated solvents such as chloroform and chlorobenzene; amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone, etc. These solvents can be used alone or in combination of two or more.

[0204] The content of the solvent in the composition for forming an anisotropic light-absorbing layer is preferably 50 to 98% by mass relative to the total amount of the composition for forming an anisotropic light-absorbing layer. In other words, the content of the solid component in the composition for forming an anisotropic light-absorbing layer is preferably 2 to 50% by mass, and more preferably 5 to 30% by mass. If the content of the solid component is 50% by mass or less, the viscosity of the composition for forming an anisotropic light-absorbing layer becomes low, so it is easy to form an anisotropic light-absorbing layer with a substantially uniform thickness, and there is a tendency that it is not easy to produce unevenness in the anisotropic light-absorbing layer. The content of the solid component can be determined in consideration of the thickness of the anisotropic light-absorbing layer to be manufactured.

[0205] (additive)

[0206] The composition for forming a light-absorbing anisotropic layer may contain additives such as a polymerization initiator such as a photopolymerization initiator or a thermal polymerization initiator, a leveling agent, an alignment promoter, an antioxidant, and a photosensitizer.

[0207] The composition for forming anisotropic light-absorbing layer may contain a polymerization initiator. The polymerization initiator may be used when the composition for forming anisotropic light-absorbing layer contains a compound that participates in a polymerization reaction, such as a polymerizable liquid crystal compound, and is a compound that can initiate a polymerization reaction of the compound. As a polymerization initiator that initiates the polymerization reaction of the polymerizable liquid crystal compound, a photopolymerization initiator that generates active free radicals by the action of light is preferred from the viewpoint of not depending on the phase state of the thermotropic liquid crystal.

[0208] The photopolymerization initiator may be any compound capable of initiating a polymerization reaction of a polymerizable liquid crystal compound or the like, and a known photopolymerization initiator may be used. Specifically, a photopolymerization initiator capable of generating active free radicals or acids by the action of light may be mentioned, and a photopolymerization initiator capable of generating free radicals by the action of light is preferred. The photopolymerization initiator may be used alone or in combination of two or more.

[0209] The photopolymerization initiator can use a known photopolymerization initiator. For example, as a photopolymerization initiator that generates active free radicals, the following can be used:

[0210] Self-cleavable benzoin compounds, acetophenone compounds, hydroxyacetophenone compounds, α-aminoacetophenone compounds, oxime ester compounds, acylphosphine oxide compounds, azo compounds, etc., and,

[0211] Hydrogen-abstracting benzophenone compounds, alkyl phenone compounds, benzoin ether compounds, benzyl ketal compounds, dibenzosuberone compounds, anthraquinone compounds, xanthone compounds, thioxanthone compounds, halogenated acetophenone compounds, dialkoxyacetophenone compounds, halogenated bisimidazole compounds, halogenated triazine compounds, triazine compounds, etc.

[0212] As the photopolymerization initiator that generates an acid, iodonium salts, sulfonium salts, and the like can be used.

[0213] The photopolymerization initiator is preferably a self-cleavage type photopolymerization initiator from the viewpoint of excellent reaction efficiency at low temperatures, and is particularly preferably an acetophenone compound, a hydroxyacetophenone compound, an α-aminoacetophenone compound, or an oxime ester compound.

[0214] The content of the polymerization initiator in the composition for forming anisotropic light-absorbing layer can be appropriately adjusted according to the type and amount of the polymerizable liquid crystal compound, and is generally 0.1 to 30 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the content of the polymerizable liquid crystal compound. If the content of the polymerization initiator is within the above range, polymerization can be performed without disturbing the orientation of the polymerizable liquid crystal compound.

[0215] The composition for forming an anisotropic layer of light absorption may include a leveling agent. The so-called leveling agent is an additive having the function of adjusting the fluidity of the composition for forming anisotropic layer of light absorption and making the film obtained by coating the composition for forming anisotropic layer of light absorption flatter. The composition for forming anisotropic layer of light absorption may include a fluorine-based leveling agent such as a silicon-based leveling agent, a polyacrylate-based leveling agent, and a perfluoroalkyl-based leveling agent, preferably including a silicon-based leveling agent. By making the composition for forming anisotropic layer of light absorption include a silicon-based leveling agent, it is easy to suppress the agglomeration (blocking) of the anisotropic layer of light absorption. When the composition for forming anisotropic layer of light absorption contains a silicon-based leveling agent, its content can be cited as the range described later as the content in the anisotropic layer of light absorption.

[0216] Silicone-based leveling agents are leveling agents containing silicon atoms, and preferably use leveling agents having a polyorganosiloxane skeleton. As groups bonded to silicon atoms (silicon atoms forming siloxane bonds) in polyorganosiloxane, hydrocarbon groups and the like can be cited. Among them, preferably, alkyl groups having 1 to 10 carbon atoms, alkoxy groups having 1 to 10 carbon atoms, ester groups having 1 to 10 carbon atoms, and aryl groups are preferred, methyl groups and phenyl groups are more preferred, and methyl groups are further preferred. The above-mentioned groups bonded to silicon atoms may be only one type, or may be more than two types. The number of repetitions (degree of polymerization) of the siloxane unit is not particularly limited, but is preferably 2 to 10,000, more preferably 3 to 5,000, and further preferably 5 to 1,000.

[0217] A commercially available silicone leveling agent can be used. Examples of commercially available silicone leveling agents include BYK-300, BYK-302, BYK-306, BYK-307, BYK-310, BYK-313, BYK-315N, BYK-320, BYK-322, BYK-323, BYK-325, BYK-330, BYK-331, BYK-333, BYK-337, BYK-342, BYK-345, BYK-346, BYK-347, BYK-348, BYK-349, BYK-370, BYK-377, BYK-378, BYK-3455, and BYK-UV3510 (all of which are BYK Chemie Japan BYK-UV3500, BYK-UV3505, BYK-UV3510, BYK-UV3530, BYK-UV3570, BYK-UV3575, BYK-UV3576 (BYK Chemie Japan KP-422, KP-416, KP-418, KP-410, KP-411, KP-412, KP-413, KP-423, KP-414, KP-415, KP-420, KP-983 (all manufactured by Shin-Etsu Chemical Co., Ltd.), etc.

[0218] Relative to 100 parts by mass of the polymer of the polymerizable liquid crystal compound contained in the light absorbing anisotropic layer, the silicon-based leveling agent is preferably 0.01 parts by mass or more and 5.0 parts by mass or less, more preferably 0.05 parts by mass or more and 3.0 parts by mass or less, further preferably 0.05 parts by mass or more and 2.0 parts by mass or less, further preferably 0.1 parts by mass or more and 1.0 parts by mass or less, and particularly preferably 0.1 parts by mass or more and 0.5 parts by mass or less. The content of the polymerizable liquid crystal compound polymer and the content of the silicon-based leveling agent can be calculated as the content of the polymerizable liquid crystal compound and the silicon-based leveling agent in the composition for forming the light absorbing anisotropic layer. By making the content of the silicon-based leveling agent within the above range, it is easy to adjust the haze of the optical film within the above range. By making the content of the silicon-based leveling agent less than 5.0 parts by mass, it is easy to suppress the depression when the light absorbing anisotropic layer forming composition is applied to the first protective layer.

[0219] When the composition for forming an anisotropic light-absorbing layer is directly coated on the surface of the first protective layer (when an orientation layer is not used), the composition for forming an anisotropic light-absorbing layer preferably contains an orientation promoter. An orientation promoter refers to a material that promotes the liquid crystal orientation of a polymerizable liquid crystal compound in a desired direction. As an orientation promoter that promotes the orientation of a polymerizable liquid crystal compound in a vertical direction, ionic compounds and nonionic silane compounds formed by non-metallic atoms can be cited. The composition for forming an anisotropic light-absorbing layer that forms an anisotropic light-absorbing layer preferably contains at least one of an ionic compound and a nonionic silane compound formed by non-metallic atoms, and more preferably contains both an ionic compound and a nonionic silane compound formed by non-metallic atoms.

[0220] As the silane compound, a nonionic silane compound described later, an ionic compound containing silane, etc. can be used. By using these silane compounds, the vertical orientation control force can be improved. These silane compounds can be used alone, or in combination of two or more, or mixed with other materials. When the silane compound is a nonionic silane compound, from the viewpoint of easily improving the vertical orientation control force, it is preferably a silane compound having an alkyl group at the molecular end, and more preferably a silane compound having an alkyl group with 3 to 30 carbon atoms.

[0221] When the composition for forming an anisotropic light-absorbing layer contains an ionic compound formed of non-metallic atoms, in the dried coating film of the composition for forming anisotropic light-absorbing layer formed on the first protective layer, a vertical alignment control force for the polymerizable liquid crystal compound is exhibited by electrostatic interaction, and the polymerizable liquid crystal compound tends to be aligned in a direction vertical to the surface of the first protective layer in the dried coating film. Thus, a light-absorbing anisotropic layer as a liquid crystal cured film can be formed while maintaining a vertically aligned state of the polymerizable liquid crystal compound.

[0222] As the ionic compound formed by non-metallic atoms, for example, onium salts (more specifically, quaternary ammonium salts, tertiary sulfonium salts, and quaternary phosphonium salts with positive charges on nitrogen atoms, etc.) can be cited. Among these onium salts, from the viewpoint of further improving the vertical orientation of polymerizable liquid crystal compounds, quaternary onium salts are preferably used, and from the viewpoint of improving availability and mass production, quaternary phosphonium salts or quaternary ammonium salts are more preferably used. Onium salts can have more than two quaternary onium salt sites in the molecule, or can be oligomers or polymers.

[0223] The molecular weight of the ionic compound is preferably 100 to 10,000. If the molecular weight is within the above range, it is easy to improve the vertical alignment of the polymerizable liquid crystal compound while ensuring the coating properties of the light absorption anisotropic layer-forming composition. The molecular weight of the ionic compound is more preferably 5000 or less, and further preferably 3000 or less.

[0224] As the cationic component of the ionic compound, for example, inorganic cations and organic cations can be cited. Among them, organic cations are preferred from the perspective of not being easy to produce orientation defects of polymerizable liquid crystal compounds. As organic cations, for example, imidazolium cations, pyridinium cations, ammonium cations, sulfonium cations and phosphonium cations can be cited.

[0225] Ionic compounds usually have counter anions. As anionic components that become counter ions of the above-mentioned cationic components, for example, inorganic anions and organic anions can be cited. Among them, from the aspect of not being easy to produce the orientation defects of polymerizable liquid crystal compounds, organic anions are preferred. It should be noted that cations and anions do not necessarily correspond one to one.

[0226] Specific examples of the anion component include the following.

[0227] Chloride anion 〔Cl - 〕,

[0228] Bromide anion 〔Br - 〕,

[0229] Iodide anion - 〕,

[0230] Tetrachloroaluminate anion 〔AlCl4 - 〕,

[0231] Heptachlorodialuminate anion〔Al2Cl7 - 〕,

[0232] Tetrafluoroborate anion 〔BF4 - 〕,

[0233] Hexafluorophosphate anion 〔PF6 - 〕,

[0234] Perchlorate anion 〔ClO4 - 〕,

[0235] Nitrate anion 〔NO3 - 〕,

[0236] Acetate anion 〔CH3COO - 〕,

[0237] trifluoroacetate anion 〔CF3COO - 〕,

[0238] Fluorosulfonate anion 〔FSO3 - 〕,

[0239] Methanesulfonate anion 〔CH3SO3 - 〕,

[0240] trifluoromethanesulfonate anion 〔CF3SO3 - 〕,

[0241] p-Toluenesulfonate anion 〔p-CH3C6H4SO3 - 〕,

[0242] Bis(fluorosulfonyl)imide anion〔(FSO2)2N - 〕,

[0243] Bis(trifluoromethanesulfonyl)imide anion〔(CF3SO2)2N - 〕,

[0244] Tris(trifluoromethanesulfonyl)methane anion〔(CF3SO2)3C - 〕,

[0245] Hexafluoroarsenate anion 〔AsF6 - 〕,

[0246] Hexafluoroantimonate anion 〔SbF6 - 〕,

[0247] Hexafluoroniobate anion〔NbF6 - 〕,

[0248] Hexafluorotantalate anion 〔TaF6 - 〕,

[0249] Dimethylphosphinate anion〔(CH3)2POO - 〕,

[0250] (Poly)hydrofluorofluoride anion〔F(HF) n - 〕(for example, n represents an integer from 1 to 3),

[0251] Dicyanamide anion〔(CN)2N - 〕,

[0252] SCN - 〕,

[0253] Perfluorobutanesulfonate anion 〔C4F9SO3 - 〕,

[0254] Bis(pentafluoroethanesulfonyl)imide anion〔(C2F5SO2)2N - 〕,

[0255] Perfluorobutyrate anion 〔C3F7COO-〕, and

[0256] (Trifluoromethanesulfonyl)(trifluoromethylcarbonyl)imide anion〔(CF3SO2)(CF3CO)N - 〕.

[0257] Specific examples of the ionic compound can be appropriately selected from the above-mentioned combinations of cationic components and anionic components. Specific examples of the compound of the combination of a cationic component and anionic component include the following compounds.

[0258] (Pyridinium salt)

[0259] N-Hexylpyridinium hexafluorophosphate,

[0260] N-Octylpyridinium hexafluorophosphate,

[0261] N-Methyl-4-hexylpyridinium hexafluorophosphate,

[0262] N-Butyl-4-methylpyridinium hexafluorophosphate,

[0263] N-octyl-4-methylpyridinium hexafluorophosphate,

[0264] N-hexylpyridinium bis(fluorosulfonyl)imide,

[0265] N-octylpyridinium bis(fluorosulfonyl)imide,

[0266] N-Methyl-4-hexylpyridinium bis(fluorosulfonyl)imide, N-butyl-4-methylpyridinium bis(fluorosulfonyl)imide, N-octyl-4-methylpyridinium bis(fluorosulfonyl)imide, N-hexylpyridinium bis(trifluoromethanesulfonyl)imide, N-octylpyridinium bis(trifluoromethanesulfonyl)imide, N-methyl-4-hexylpyridinium bis(trifluoromethanesulfonyl)imide, N-butyl -4-methylpyridinium bis(trifluoromethanesulfonyl)imide, N-octyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide, N-hexylpyridinium p-toluenesulfonate, N-octylpyridinium p-toluenesulfonate, N-methyl-4-hexylpyridinium p-toluenesulfonate, N-butyl-4-methylpyridinium p-toluenesulfonate, and, N-octyl-4-methylpyridinium p-toluenesulfonate.

[0267] (Imidazolium salt)

[0268] 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium p-toluenesulfonate, 1-butyl-3-methylimidazolium methanesulfonate, and the like.

[0269] (Pyrrolidinium salt)

[0270] N-Butyl-N-methylpyrrolidinium hexafluorophosphate,

[0271] N-butyl-N-methylpyrrolidinium bis(fluorosulfonyl)imide, N-butyl-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide, N-butyl-N-methylpyrrolidinium p-toluenesulfonate and the like.

[0272] (Ammonium salt)

[0273] Tetrabutylammonium hexafluorophosphate,

[0274] Tetrabutylammonium bis(fluorosulfonyl)imide,

[0275] Tetrahexylammonium bis(fluorosulfonyl)imide,

[0276] Trioctylmethylammonium bis(fluorosulfonyl)imide,

[0277] (2-Hydroxyethyl)trimethylammonium bis(fluorosulfonyl)imide,

[0278] Tetrabutylammonium bis(trifluoromethanesulfonyl)imide,

[0279] Tetrahexylammonium bis(trifluoromethanesulfonyl)imide,

[0280] Trioctylmethylammonium bis(trifluoromethanesulfonyl)imide,

[0281] (2-Hydroxyethyl)trimethylammonium bis(trifluoromethanesulfonyl)imide,

[0282] Tetrabutylammonium p-toluenesulfonate,

[0283] Tetrahexyl ammonium p-toluenesulfonate,

[0284] Trioctylmethylammonium p-toluenesulfonate,

[0285] (2-Hydroxyethyl)trimethylammonium p-toluenesulfonate,

[0286] (2-Hydroxyethyl)trimethylammonium dimethylphosphinate,

[0287] 1-(3-Trimethoxysilylpropyl)-1,1,1-tributylammonium bis(trifluoromethanesulfonyl)imide,

[0288] 1-(3-Trimethoxysilylpropyl)-1,1,1-trimethylammonium bis(trifluoromethanesulfonyl)imide,

[0289] 1-(3-Trimethoxysilylbutyl)-1,1,1-tributylammonium bis(trifluoromethanesulfonyl)imide,

[0290] 1-(3-Trimethoxysilylbutyl)-1,1,1-trimethylammonium bis(trifluoromethanesulfonyl)imide,

[0291] N-{(3-triethoxysilylpropyl)carbamoyloxyethyl)}-N,N,N-trimethylammonium bis(trifluoromethanesulfonyl)imide, and

[0292] N-[2-{3-(3-trimethoxysilylpropylamino)-1-oxopropoxy}ethyl]-N,N,N-trimethylammonium bis(trifluoromethanesulfonyl)imide.

[0293] (Phosphonium salt)

[0294] Tributyl(2-methoxyethyl)phosphoniumbis(trifluoromethanesulfonyl)imide,

[0295] Tributylmethylphosphonium bis(trifluoromethanesulfonyl)imide,

[0296] 1,1,1-Trimethyl-1-[(trimethoxysilyl)methyl]phosphonium bis(trifluoromethanesulfonyl)imide,

[0297] 1,1,1-Trimethyl-1-[2-(trimethoxysilyl)ethyl]phosphonium bis(trifluoromethanesulfonyl)imide,

[0298] 1,1,1-Trimethyl-1-[3-(trimethoxysilyl)propyl]phosphonium bis(trifluoromethanesulfonyl)imide,

[0299] 1,1,1-Trimethyl-1-[4-(trimethoxysilyl)butyl]phosphonium bis(trifluoromethanesulfonyl)imide,

[0300] 1,1,1-tributyl-1-[(trimethoxysilyl)methyl]phosphonium bis(trifluoromethanesulfonyl)imide,

[0301] 1,1,1-tributyl-1-[2-(trimethoxysilyl)ethyl]phosphonium bis(trifluoromethanesulfonyl)imide, and

[0302] 1,1,1-tributyl-1-[3-(trimethoxysilyl)propyl]phosphonium bis(trifluoromethanesulfonyl)imide.

[0303] These ionic compounds may be used alone or in combination of two or more.

[0304] From the viewpoint of further improving the vertical alignment of the polymerizable liquid crystal compound, the ionic compound preferably has Si element and / or F element in the molecular structure of the cationic part. If the ionic compound has Si element and / or F element in the molecular structure of the cationic part, it is easy to make the ionic compound segregate on the surface of the light absorption anisotropic layer. Among them, as an ionic compound whose constituent elements are all non-metallic elements, the following ionic compounds (ii) to (iv) are preferred.

[0305] Ionic compounds (ii):

[0306] [Chemical formula 9]

[0307]

[0308] Ionic compounds (iii):

[0309] [Chemical formula 10]

[0310]

[0311] Ionic compounds (iv)

[0312] [Chemical formula 11]

[0313]

[0314] As a method for improving the vertical alignment of polymerizable liquid crystal compounds, for example, a method of treating the surface of a substrate with a surfactant having an alkyl group with a relatively long chain length is known (for example, see Chapter 2 of "Liquid Crystal Handbook" on the Orientation and Physical Properties of Liquid Crystals (published by Maruzen Co., Ltd.)). Such a method of improving the vertical alignment of liquid crystal compounds using a surfactant can also be applied to ionic compounds. That is, by treating the surface of the first protective layer with an ionic compound having an alkyl group with a relatively long chain length, the vertical alignment of the polymerizable liquid crystal compound can be effectively improved.

[0315] Specifically, the ionic compound preferably satisfies the following relationship:

[0316] 5 <M<16。

[0317] M in the above relationship is represented by the following formula.

[0318] M = (the number of covalent bonds from the positively charged atom to the molecular chain terminal of the substituent having the largest number of covalent bonds to the molecular chain terminal among the substituents directly bonded to the positively charged atom) ÷ (the number of positively charged atoms)

[0319] By making the ionic compound satisfy the above relationship, the vertical alignment property of the polymerizable liquid crystal compound can be effectively improved.

[0320] When there are two or more atoms with positive charge in the molecule of the ionic compound, for a substituent containing two or more atoms with positive charge, the number of covalent bonds from the atom with positive charge regarded as the base point to the nearest other atom with positive charge is taken as the "number of covalent bonds from the atom with positive charge to the molecular chain terminal" described in the above definition of M. When the ionic compound is an oligomer or polymer having two or more repeating units, the structural unit is regarded as one molecule and the above M is calculated. When the atom with positive charge is incorporated into a ring structure, the number of covalent bonds from the atom with positive charge via the ring structure to the atom with positive charge or the number of covalent bonds to the terminal of the substituent bonded to the ring structure, whichever has a larger number of covalent bonds, is taken as the "number of covalent bonds from the atom with positive charge to the molecular chain terminal" described in the above definition of M.

[0321] When the composition for forming anisotropic light-absorbing layer contains an ionic compound, the content thereof is preferably 0.01 to 5% by mass, more preferably 0.05 to 4% by mass, and further preferably 0.1 to 3% by mass relative to the solid content of the composition for forming anisotropic light-absorbing layer. If the content of the ionic compound is within the above range, good coating properties of the composition for forming anisotropic light-absorbing layer can be maintained, and the vertical alignment of the polymerizable liquid crystal compound can be effectively promoted.

[0322] When the composition for forming an anisotropic light-absorbing layer contains a nonionic silane compound, there is a tendency that the nonionic silane compound reduces the surface tension of the composition for forming anisotropic light-absorbing layer, and in the dried coating film formed from the composition for forming anisotropic light-absorbing layer on the first protective layer, the nonionic silane compound is present on the surface of the dried coating film opposite to the first protective layer, thereby increasing the vertical alignment control force of the polymerizable liquid crystal compound, and the polymerizable liquid crystal compound is aligned in a direction vertical to the surface of the first protective layer in the dried coating film. As a result, the polymerizable liquid crystal compound can be maintained in a vertically aligned state and the light-absorbing anisotropic layer as a liquid crystal cured film can be formed.

[0323] The nonionic silane compound is a nonionic compound containing Si element. Examples of the nonionic silane compound include silicone polymers such as polysilane, silicone resins such as silicone oil and silicone resin, and organosilicon oligomers, organic inorganic silane compounds such as silsesquioxane and alkoxysilane (more specifically, silane coupling agents, etc.), and silane-containing compounds described in the items of leveling agents.

[0324] The nonionic silane compound may be a silicone monomer type compound or a silicone oligomer (polymer) type compound. When the silicone oligomer is represented in the form of a (monomer)-(monomer) copolymer, examples include copolymers containing a mercaptopropyl group such as 3-mercaptopropyltrimethoxysilane-tetramethoxysilane copolymer, 3-mercaptopropyltrimethoxysilane-tetraethoxysilane copolymer, 3-mercaptopropyltriethoxysilane-tetramethoxysilane copolymer, and 3-mercaptopropyltriethoxysilane-tetraethoxysilane copolymer; and copolymers containing a mercaptomethyl group such as mercaptomethyltrimethoxysilane-tetramethoxysilane copolymer, mercaptomethyltrimethoxysilane-tetraethoxysilane copolymer, mercaptomethyltriethoxysilane-tetramethoxysilane copolymer, and mercaptomethyltriethoxysilane-tetraethoxysilane copolymer. Copolymers; 3-methacryloxypropyl trimethoxysilane-tetramethoxysilane copolymer, 3-methacryloxypropyl trimethoxysilane-tetraethoxysilane copolymer, 3-methacryloxypropyl triethoxysilane-tetramethoxysilane copolymer, 3-methacryloxypropyl triethoxysilane-tetraethoxysilane copolymer, 3-methacryloxypropyl methyl dimethoxysilane-tetramethoxysilane copolymer, 3-methacryloxypropyl methyl dimethoxysilane-tetraethoxysilane copolymer, 3-methacryloxypropyl methyl diethoxysilane-tetramethoxysilane copolymer and 3-methacryloxypropyl methyl dimethoxysilane-tetramethoxysilane copolymer ethoxysilane-tetraethoxysilane copolymers; 3-acryloxypropyl trimethoxysilane-tetramethoxysilane copolymers, 3-acryloxypropyl trimethoxysilane-tetraethoxysilane copolymers, 3-acryloxypropyl triethoxysilane-tetramethoxysilane copolymers, 3-acryloxypropyl triethoxysilane-tetraethoxysilane copolymers, 3-acryloxypropyl methyldimethoxysilane-tetramethoxysilane copolymers, 3-acryloxypropyl methyldimethoxysilane-tetraethoxysilane copolymers, 3-acryloxypropyl methyldiethoxysilane-tetramethoxysilane copolymers acryloxypropyl group-containing copolymers such as 3-acryloxypropylmethyldiethoxysilane-tetraethoxysilane copolymers; vinyltrimethoxysilane-tetramethoxysilane copolymers, vinyltrimethoxysilane-tetraethoxysilane copolymers, vinyltriethoxysilane-tetramethoxysilane copolymers, vinyltriethoxysilane-tetraethoxysilane copolymers, vinylmethyldimethoxysilane-tetramethoxysilane copolymers, vinylmethyldimethoxysilane-tetraethoxysilane copolymers, vinylmethyldiethoxysilane-tetramethoxysilane copolymers, and vinylmethyldiethoxysilane-tetraethoxysilane copolymers;3-aminopropyltrimethoxysilane-tetramethoxysilane copolymer, 3-aminopropyltrimethoxysilane-tetraethoxysilane copolymer, 3-aminopropyltriethoxysilane-tetramethoxysilane copolymer, 3-aminopropyltriethoxysilane-tetraethoxysilane copolymer, 3-aminopropylmethyldimethoxysilane-tetramethoxysilane copolymer, 3-aminopropylmethyldimethoxysilane-tetraethoxysilane copolymer, 3-aminopropylmethyldiethoxysilane-tetramethoxysilane copolymer and 3-aminopropylmethyldiethoxysilane-tetraethoxysilane copolymer, etc. These nonionic silane compounds can be used alone or in combination of two or more. Among them, from the viewpoint of further improving the adhesion with the adjacent layer, a silane coupling agent is preferred. ;

[0325] Silane coupling agent is a compound containing Si element having at least one functional group selected from the group consisting of vinyl, epoxy, styryl, methacrylic group, acrylic group, amino, isocyanurate, urea, mercapto, isocyanate, carboxyl, and hydroxyl at the end, and at least one alkoxysilyl or silanol group. By appropriately selecting these functional groups, it is possible to impart excellent effects such as improvement of the mechanical strength of the light absorption anisotropic layer, surface modification of the light absorption anisotropic layer, and improvement of the adhesion between the light absorption anisotropic layer and the adjacent layer (e.g., the first protective layer). From the viewpoint of adhesion, the silane coupling agent is preferably a silane coupling agent having an alkoxysilyl group and another different reactive group (e.g., the above-mentioned functional group). The silane coupling agent is preferably a silane coupling agent having an alkoxysilyl group and a polar group. If the silane coupling agent has at least one alkoxysilyl group and at least one polar group in its molecule, it is easy to further improve the vertical orientation of the polymerizable liquid crystal compound and significantly obtain a tendency to promote the effect of vertical orientation. As the polar group, for example, an epoxy group, an amino group, an isocyanurate group, a thiol group, a carboxyl group and a hydroxyl group can be cited. The polar group can suitably have a substituent or a protecting group in order to control the reactivity of the silane coupling agent.

[0326] Specific examples of the silane coupling agent include vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tri(2-methoxyethoxy)silane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, 3-glycidoxypropyltrimethoxysilane, 3- Glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyldimethoxymethylsilane, and 3-glycidoxypropylethoxydimethylsilane.

[0327] Examples of commercially available silane coupling agents include KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001, KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-1403, KBM-502, KBM-503, Silane coupling agents manufactured by Shin-Etsu Chemical Co., Ltd. such as KBE-502, KBE-503, KBM-5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103, KBM-573, KBM-575, KBM-9659, KBE-585, KBM-802, KBM-803, KBE-846, and KBE-9007.

[0328] When the composition for forming anisotropic light-absorbing layer contains a nonionic silane compound, the content thereof is preferably 0.01% to 5% by mass, more preferably 0.05% to 4% by mass, and further preferably 0.1% to 3% by mass, relative to the solid content of the composition for forming anisotropic light-absorbing layer. If the content of the nonionic silane compound is within the above range, good coating properties of the composition for forming anisotropic light-absorbing layer can be maintained, and the vertical alignment of the polymerizable liquid crystal compound can be effectively promoted.

[0329] By making the composition for forming anisotropic light-absorbing layer contain both an ionic compound and a nonionic silane compound, in the dried coating film formed from the composition for forming anisotropic light-absorbing layer on the first protective layer, the vertical alignment of the polymerizable liquid crystal compound is further promoted by the electrostatic interaction from the ionic compound and the surface tension reduction effect from the nonionic silane compound. Thus, the polymerizable liquid crystal compound can be maintained in a vertically aligned state with higher accuracy to form a light-absorbing anisotropic layer as a liquid crystal cured film.

[0330] (Orientation Layer)

[0331] The alignment layer facilitates the liquid crystal alignment of the polymerizable liquid crystal compound. The state of the liquid crystal alignment varies depending on the properties of the alignment layer and the polymerizable liquid crystal compound, and their combination can be arbitrarily selected.

[0332] When the orientation layer is formed of an orientation polymer, the orientation control force can be arbitrarily adjusted by the surface state and friction conditions. When the orientation layer is formed of a photo-orientation polymer, the orientation control force can be arbitrarily adjusted by polarized light irradiation conditions, etc. In addition, the liquid crystal orientation can also be controlled by selecting the surface tension, liquid crystal properties and other physical properties of the polymerizable liquid crystal compound.

[0333] As the alignment layer, it is preferred that the alignment layer is insoluble in the solvent used when forming the light absorption anisotropic layer on the alignment layer and has heat resistance in the heating treatment for removing the solvent and aligning the liquid crystal. As the alignment layer, there can be cited a polymer alignment layer formed of an aligning polymer, a photoalignment layer and a groove alignment layer, a stretched film stretched along the alignment direction, etc. In the case of being applied to a long roll film, the photoalignment layer is preferred from the aspect of being able to easily control the alignment direction.

[0334] The thickness of the alignment layer is usually in the range of 10 nm to 5000 nm, preferably in the range of 10 nm to 1000 nm, and more preferably in the range of 30 to 300 nm.

[0335] As the oriented polymer used in the rubbing orientation layer, polyamides, gelatins, polyimides with amide bonds in the molecule and polyamic acids, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinyl pyrrolidone, polyacrylic acid and polyacrylates, etc., which are hydrolyzates thereof, can be cited. Among them, polyvinyl alcohol is preferred. These oriented polymers can be used alone or in combination of two or more.

[0336] The rubbing method includes a method in which a film of an oriented polymer formed by applying an oriented polymer composition to a layer constituting the first protective layer and annealing the oriented polymer composition to constitute the surface of the first protective layer is brought into contact with a rotating rubbing roller wound with a rubbing cloth.

[0337] The photo-alignment layer is formed of a polymer, oligomer or monomer having a photoreactive group. For the photo-alignment layer, the alignment control force can be obtained by irradiating a coating layer formed by coating a composition for forming the photo-alignment layer on a layer constituting the first protective layer with polarized light. From the perspective that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized light, the photo-alignment layer is more preferred.

[0338] The so-called photoreactive group refers to a group that generates liquid crystal orientation ability by irradiation with light. Specifically, it is a group that generates photoreactions such as orientation induction or isomerization reaction, dimerization reaction, photocrosslinking reaction or photodecomposition reaction of molecules generated by irradiation with light, which are the source of liquid crystal orientation ability. Among the photoreactive groups, groups that undergo dimerization reaction or photocrosslinking reaction are preferred from the perspective of excellent orientation. As a photoreactive group capable of the above reaction, it is preferably a group having an unsaturated bond, especially a double bond, and more preferably a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond).

[0339] As photoreactive groups with C=C bonds, for example, vinyl, polyene, stilbene, stilbazolyl, stilbazolinium, chalcone and cinnamoyl groups can be cited. From the perspective of easy control of reactivity and the presentation of orientation control force during photo-orientation, chalcone and cinnamoyl groups are preferred. As photoreactive groups with C=N bonds, groups with structures such as aromatic Schiff bases and aromatic hydrazones can be cited. As photoreactive groups with N=N bonds, groups with azobenzene oxide as the basic structure such as azobenzene, azonaphthyl, aromatic heterocyclic azo, disazo and formazan can be cited. As photoreactive groups with C=O bonds, benzophenone, coumarin, anthraquinone and maleimide groups can be cited. These groups can have substituents such as alkyl, alkoxy, aryl, allyloxy, cyano, alkoxycarbonyl, hydroxyl, sulfonic acid and halogenated alkyl.

[0340] The method of irradiating polarized light may be a method of directly irradiating polarized light from the film surface of the coating layer of the composition for forming the photo-alignment layer, or a method of irradiating polarized light from the substrate layer side and transmitting the polarized light. In addition, the polarized light is particularly preferably substantially parallel light. The wavelength of the irradiated polarized light is the wavelength of the wavelength region in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) with a wavelength range of 250 to 400 nm is particularly preferred. As the light source used in the polarized light irradiation, xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF can be cited, and high-pressure mercury lamps, ultra-high-pressure mercury lamps and metal halide lamps are more preferred. The luminous intensity of ultraviolet light with a wavelength of 313 nm of these lamps is large, so it is preferred. The light from the above-mentioned light source can be irradiated through an appropriate polarizer, thereby irradiating polarized light. As the polarizer, polarizing filters, Glan-Thompson, Glan-Taylor polarizing prisms, and wire grid polarizers can be used.

[0341] (Second protective layer)

[0342] The second protective layer can suppress the diffusion of the dichroic pigment contained in the light absorption anisotropic layer, and suppress the damage of the light absorption anisotropic layer. The second protective layer can, for example, include a layer formed by a resin composition containing a water-soluble polymer (hereinafter, also referred to as "resin composition containing a water-soluble polymer"). A layer formed by a photocurable composition containing an active energy ray-curable resin, etc. The water-soluble polymer is usually very different from the polarity of the dichroic pigment, so the effect of preventing the dichroic pigment from diffusing is excellent, and therefore, the second protective layer is preferably a layer formed by a resin composition containing a water-soluble polymer.

[0343] Examples of water-soluble polymers include polyacrylamide polymers, vinyl alcohol polymers such as polyvinyl alcohol, ethylene-vinyl alcohol copolymers, and (meth)acrylic acid or its anhydride-vinyl alcohol copolymers, carboxyvinyl polymers, polyvinyl pyrrolidone, starches, sodium alginate, or polyethylene oxide polymers, etc. These polymers may be used alone or in combination of two or more.

[0344] When the second protective layer is a layer formed of a resin composition containing a water-soluble polymer, the content of the water-soluble polymer in the layer is preferably 75% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more.

[0345] In the case where the second protective layer is a layer formed of a resin composition containing a water-soluble polymer, a crosslinking structure may be introduced by using a crosslinking agent in order to improve the compactness of the layer. Examples of the crosslinking agent include water-soluble crosslinking agents such as ionic crosslinking agents such as glyoxylate and epoxy crosslinking agents; hydrophobic crosslinking agents such as isocyanate crosslinking agents, polyaldehyde crosslinking agents such as glyoxal and glyoxal derivatives, and metal compound crosslinking agents such as zirconium chloride or titanium lactate for the purpose of imparting water resistance.

[0346] The amount of the crosslinking agent added can be appropriately determined according to the type of the crosslinking agent, etc. For example, it can be 0.1 to 100 parts by mass, preferably 1 to 50 parts by mass, and more preferably 10 to 30 parts by mass relative to 100 parts by mass of the water-soluble polymer. If the content of the crosslinking agent is within the above range, a dense second protective layer can be formed.

[0347] The resin composition containing the water-soluble polymer is usually prepared as a solution obtained by dissolving the water-soluble polymer in a solvent. The solvent may be selected according to the water-soluble polymer used, and typically includes water, alcohol, and a mixture of water and alcohol, and water is preferred.

[0348] The solid content concentration of the resin composition containing a water-soluble polymer obtained by adding a solvent to the components constituting the second protective layer such as a water-soluble polymer and a crosslinking agent is preferably 1 to 50% by mass, more preferably 2 to 30% by mass, and further preferably 3 to 15% by mass. If the solid content concentration of the resin composition containing a water-soluble polymer is within the above range, the viscosity of the composition becomes low, and therefore, the coating property and the workability become good.

[0349] In the resin composition containing a water-soluble polymer, in addition to a water-soluble polymer, a crosslinking agent, and a solvent such as water, other components such as additives may also be included. As other components, for example, preservatives, leveling agents, etc. may be cited. When the resin composition containing a water-soluble polymer includes other components such as additives, the amount thereof is preferably less than 10% by mass, more preferably less than 5% by mass, based on the solid content of the resin composition.

[0350] A resin composition containing a water-soluble polymer prepared by dissolving necessary components such as a water-soluble polymer and a crosslinking agent in a solvent can be applied to the surface of the light-absorbing anisotropic layer opposite to the first protective layer, and the solvent in the coating film can be dried to remove it and cured to form a second protective layer.

[0351] The method of applying the resin composition containing a water-soluble polymer is not particularly limited, and an example thereof includes a method of applying a composition for forming a light absorption anisotropic layer.

[0352] The drying temperature and time for forming the second protective layer from the coating film of the resin composition containing the water-soluble polymer are not particularly limited and can be appropriately determined according to the composition of the resin composition containing the water-soluble polymer used. The drying treatment can be carried out by, for example, blowing hot air, etc., and the temperature is usually in the range of 40 to 100° C., preferably in the range of 60 to 100° C. In addition, the drying time is usually 10 to 600 seconds.

[0353] Examples of the active energy ray-curable resin contained in the photocurable composition include (meth)acrylic resins, urethane resins, (meth)acrylic urethane resins, epoxy resins, and silicone resins. The active energy ray-curable resin is preferably an epoxy resin.

[0354] The photocurable composition can be applied to the surface of the light absorbing anisotropic layer opposite to the first protective layer and irradiated with active energy rays to form a second protective layer. As described above, the surface of the light absorbing anisotropic layer on the side where the second protective layer is to be formed can be subjected to surface treatment.

[0355] The thickness of the second protective layer is preferably 15 μm or less, and may be 0.1 μm to 12 μm or less, preferably 0.5 μm to 10 μm or less, and more preferably 1 μm to 5 μm or less.

[0356] The second protective layer preferably has a tensile modulus of 100 MPa to 5000 MPa, 200 MPa to 4000 MPa, or 300 MPa to 1000 MPa at a temperature of 23° C. and a relative humidity of 55%. The tensile modulus can be measured by the above method.

[0357] (First adhesive layer, second adhesive layer)

[0358] The first adhesive layer and the second adhesive layer (hereinafter, also referred to as "adhesive layer") can be formed using an adhesive composition. An adhesive composition or a reaction product of an adhesive composition is a substance that exhibits adhesiveness by attaching itself to an adherend, and is called a so-called pressure-sensitive adhesive. In addition, an adhesive layer formed using an active energy ray-curable adhesive composition described later can adjust the degree of crosslinking and the adhesive force by irradiating active energy rays.

[0359] As adhesive composition, adhesives with excellent optical transparency known in the past can be used without particular limitation, for example, adhesive compositions containing base polymers such as acrylic polymers, carbamate polymers, silicone polymers, polyvinyl ethers can be used. In addition, adhesive composition can be active energy ray curing adhesive composition or heat curing adhesive composition etc. Among them, adhesive compositions using acrylic resins excellent in transparency, adhesion, re-peelability (reoperability), weatherability, heat resistance etc. as base polymers are preferred. The adhesive layer is preferably composed of the reaction product of the adhesive composition comprising (meth) acrylic resin, crosslinking agent, silane compound, and may also include other components.

[0360] The adhesive composition for forming the adhesive layer can include base polymers such as acrylic polymers, urethane polymers, silicone polymers, polyvinyl ethers, etc. The adhesive composition can be an active energy ray-curable adhesive, a thermosetting adhesive, etc. Among them, an adhesive using a (meth) acrylic resin having excellent transparency, adhesion, re-peelability (re-operability), weather resistance, heat resistance, etc. as a base polymer is preferred. The adhesive layer is preferably composed of a reaction product of an adhesive comprising a (meth) acrylic resin, a crosslinking agent, and a silane compound, and may also include other components.

[0361] The adhesive layer can be formed using an active energy ray-curable adhesive. For active energy ray-curable adhesives, a harder adhesive layer can be formed by adding an ultraviolet curable compound such as a multifunctional acrylate to the above-mentioned adhesive composition and curing it by irradiating ultraviolet rays after forming the adhesive layer. Active energy ray-curable adhesives have the property of being cured by irradiation with energy rays such as ultraviolet rays and electron beams. Active energy ray-curable adhesives also have adhesiveness before energy ray irradiation, and therefore have the property of being able to fit closely to an adherend, being cured by irradiation with energy rays, and adjusting the adhesion.

[0362] The thickness of the first adhesive layer is not particularly limited, and is usually 5 μm to 300 μm, 10 μm to 250 μm, 15 μm to 100 μm, or 20 μm to 50 μm.

[0363] The thickness of the second adhesive layer is not particularly limited, and is usually 5 μm to 100 μm, 10 μm to 80 μm, 12 μm to 50 μm, or 15 μm to 30 μm.

[0364] (Isolator)

[0365] The separator includes a stretched polyester film. The stretched polyester film is preferably a biaxially stretched polyester film. The thickness of the stretched polyester film is preferably 30 μm or more, more preferably 35 μm or more, and may be 40 μm or more, and is usually 100 μm or less.

[0366] The stretched polyester film is a film obtained by uniaxially stretching or biaxially stretching a polyethylene terephthalate (PET) film, and is preferably a film obtained by biaxially stretching a polyethylene terephthalate (PET) film.

[0367] As for the separator, a release treatment may be applied to one side of the stretched polyester film, or the separator may be a laminate of the stretched polyester film and the release force adjusting layer. As the release treatment, a method of forming a release layer by coating a release agent or the like may be cited. As the release agent, a silicone release agent and a fluorine release agent may be cited. The release force adjusting layer may be formed by coating a silane coupling agent, for example.

[0368] The tensile modulus of the stretched polyester film at a temperature of 23° C. and a relative humidity of 55% is preferably 4000 MPa or more, 5000 MPa or more, or 6000 MPa or more, and is usually 20000 MPa or less. The tensile modulus can be measured by the above-mentioned method.

[0369] Example

[0370] The present invention will be described in more detail below by showing Examples and Comparative Examples, but the present invention is not limited to these Examples. Unless otherwise specified, "%" and "part" in Examples and Comparative Examples are mass % and mass parts.

[0371] [Production and preparation of surface protection film]

[0372] (Preparation of Adhesive Composition (a))

[0373] Nitrogen was introduced into a reaction device equipped with a stirrer, a thermometer, a reflux condenser and a nitrogen introduction tube, and the air in the reaction device was replaced with nitrogen. Then, 60 parts of a solvent (ethyl acetate) were added to the reaction device together with 93 parts of 2-ethylhexyl acrylate, 5.5 parts of 8-hydroxyoctyl acrylate and 1.5 parts of acrylic acid. Then, 0.1 parts of azobisisobutyronitrile as a polymerization initiator was added dropwise over 2 hours, and the reaction was carried out at 65° C. for 6 hours to obtain an acrylic resin solution. The weight average molecular weight of the acrylic polymer contained in the acrylic resin solution was about 500,000 as a value converted to standard polystyrene obtained by gel permeation chromatography.

[0374] 2.0 parts of 1-octylpyridinium dodecylbenzenesulfonate as an antistatic agent was added to 100 parts of the acrylic polymer contained in the acrylic resin solution obtained above, and after stirring, 1.5 parts of CORONATE HX (isocyanurate of a hexamethylene diisocyanate compound: manufactured by TOSOH Corporation) was added and stirred and mixed to obtain an adhesive composition (a).

[0375] (Production of surface protection films (1) to (3))

[0376] Stretched polyethylene terephthalate films (hereinafter also referred to as "stretched PET films") (1) to (3) having a thickness of 38 μm, 50 μm, and 75 μm were prepared, and the adhesive composition (a) obtained above was applied thereon, followed by drying at a temperature of 90°C to remove the solvent, thereby forming a second adhesive layer (1) having a thickness of 15 μm, thereby obtaining surface protective films (1) to (3). The thicknesses of the stretched PET films (1), (2), and (3) of the surface protective films (1), (2), and (3) were 38 μm, 50 μm, and 75 μm, respectively.

[0377] (Production of Surface Protection Film (4))

[0378] KBM-5103 (manufactured by Shin-Etsu Silicone) as a silane coupling agent was dissolved in o-xylene to a concentration of 0.25% to prepare a release strength adjusting layer forming composition (1). The release strength adjusting layer forming composition (1) was applied to the surface of a stretched PET film (thickness 38 μm, SP-PLR382050 manufactured by LINTEC) subjected to release treatment on one side, on the side opposite to the surface subjected to release treatment, using a bar coater, and dried in an oven at a temperature of 120° C. for 1 minute to form a release strength adjusting layer (1) having a thickness of 40 nm, which was used as a surface protective film (4).

[0379] (Production of Surface Protection Film (5))

[0380] A surface protective film (5) was produced by the same steps as the surface protective film (4), except that a stretched PET film (thickness 75 μm, CAO manufactured by Fujico) was used in place of a stretched PET film (thickness 38 μm) on one side of which a release treatment was applied.

[0381] (Preparation of surface protection film (6))

[0382] As the surface protection film (6), a stretched PET film (38 μm thick, SP-PLR382050 manufactured by LINTEC) having one surface subjected to a release treatment was prepared.

[0383] (Preparation of surface protection film (7))

[0384] As the surface protection film (6), a stretched PET film (thickness 75 μm, CAO manufactured by Fujico Co., Ltd.) having one surface subjected to a release treatment was prepared.

[0385] [Preparation of Composition for Forming Light Absorption Anisotropic Layer]

[0386] (Preparation of Composition (1) for Forming Light Absorption Anisotropic Layer)

[0387] The components shown below were mixed and stirred at 80° C. for 1 hour to obtain a composition (1) for forming a light absorption anisotropic layer.

[0388] Polymerizable liquid crystal compound (1): 75 parts

[0389] Polymerizable liquid crystal compound (2): 25 parts

[0390] Dichroic pigment (1): 1 part

[0391] Polymerization initiator (Irgacure 369, manufactured by BASF): 6 parts

[0392] Non-liquid crystal compound having a polymerizable group (dipentaerythritol hexaacrylate (6-functional)): 1.5 parts

[0393] Leveling agent (F-556, manufactured by DIC Corporation): 0.25 parts

[0394] Solvent (o-xylene): 300 parts

[0395] The polymerizable liquid crystal compounds (1) and (2) have the structures shown below and were synthesized according to the method described in Lub et al., Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996).

[0396] ·Polymerizable liquid crystal compound (1):

[0397] [Chemical formula 12]

[0398]

[0399] Polymerizable liquid crystal compound (2):

[0400] [Chemical formula 13]

[0401]

[0402] The dichroic dye (1) used was an azo dye described in Examples of JP-A-2013-101328 having the structure shown below: The maximum absorption wavelength of the dichroic dye (1) measured in a chloroform solution was 600 nm.

[0403] Dichroic pigments (1):

[0404] [Chemical formula 14]

[0405]

[0406] (Preparation of Composition for Forming Light Absorption Anisotropic Layer (2))

[0407] A composition (2) for forming a light-absorbing anisotropic layer was prepared by the same procedure as that for preparing the composition (1) for forming a light-absorbing anisotropic layer, except that the solvent (o-xylene) was changed to a solvent (cyclopentanone).

[0408] (Preparation of Composition (3) for Forming Light Absorption Anisotropic Layer)

[0409] The components shown below were mixed and stirred at 80° C. for 1 hour to obtain a composition (3) for forming a light absorption anisotropic layer.

[0410] Polymerizable liquid crystal compound (1): 75 parts

[0411] Polymerizable liquid crystal compound (2): 25 parts

[0412] Dichroic pigment (1): 2.5 parts

[0413] Dichroic pigment (2): 2.5 parts

[0414] Dichroic pigment (3): 2.5 parts

[0415] Polymerization initiator (Irgacure 369, manufactured by BASF): 6 parts

[0416] Leveling agent (polyacrylate compound (BYK-361N; manufactured by BYK-Chemie): 1.2 parts

[0417] Solvent (o-xylene): 250 parts

[0418] As the dichroic dyes (2) and (3), the azo dyes described in Examples of JP-A-2013-101328 were used.

[0419] Dichroic pigments (2):

[0420] [Chemical formula 15]

[0421]

[0422] Dichroic pigments (3):

[0423] [Chemical formula 16]

[0424]

[0425] (Preparation of Composition (4) for Forming Light Absorption Anisotropic Layer)

[0426] The polymerizable liquid crystal compound (3) and the polymerizable liquid crystal compound (4) were mixed in a mass ratio of 90:10 to obtain a mixture. With respect to 100 parts by mass of the obtained mixture, 0.25 parts by mass of a leveling agent "F-556", 1.5 parts by mass of a dichroic pigment (1), 1.5 parts by mass of an ionic compound (molecular weight: 645) shown below prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 parts by mass of a silane coupling agent "KBE-9103" (manufactured by Shin-Etsu Chemical Co., Ltd.), and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butane-1-one (Irgacure 369) as a photopolymerization initiator were added. Furthermore, N-methyl-2-pyrrolidone (NMP) was added in such a manner that the solid content concentration became 13%. The mixture was stirred at 80°C for 1 hour to obtain a composition (4) for forming a light absorbing anisotropic layer.

[0427] ·Polymerizable liquid crystal compounds (3)

[0428] [Chemical formula 17]

[0429]

[0430] ·Polymerizable liquid crystal compounds (4)

[0431] [Chemical formula 18]

[0432]

[0433] Ionic compounds

[0434] [Chemical formula 19]

[0435]

[0436] [Preparation of a resin composition containing a water-soluble polymer]

[0437] According to the following synthetic route, a water-soluble polymer formed of the structural units shown below is obtained.

[0438] [Chemical formula 20]

[0439]

[0440] 20 g of polyvinyl alcohol (manufactured by Wako Pure Chemical Industries, Ltd.) with a molecular weight of 1000, 0.55 mg of N,N-dimethyl-4-aminopyridine as a nucleophile, and 4.6 g of triethylamine were dissolved in 400 g of dimethyl sulfoxide, and the temperature was raised to 60°C while stirring. Then, a solution obtained by dissolving 10.5 g of methacrylic anhydride in 50 g of dimethyl sulfoxide was added dropwise over 1 hour, and the mixture was heated and stirred at 60°C for 14 hours to react. After the obtained reaction solution was cooled to room temperature, 481 g of methanol was added to the reaction solution, and the mixture was stirred in a completely mixed manner, thereby adjusting the ratio (mass) of the reaction solution to methanol to 1:1. 1500 mL of acetone was slowly added to the solution, thereby crystallizing the water-soluble polymer by crystallization. The solution containing the obtained white crystals was filtered, washed sufficiently with acetone, and then vacuum dried to obtain 20.2 g of a water-soluble polymer. The obtained water-soluble polymer was dissolved in water to prepare a 3% water-soluble polymer aqueous solution as a resin composition containing a water-soluble polymer.

[0441] [Preparation of photocurable composition]

[0442] The components shown below were mixed and degassed to prepare a photocurable composition. The photocationic polymerization initiator was blended in the form of a 50% propylene carbonate solution, and the amount thereof is expressed as a solid content.

[0443] Cationic polymerizable compound (1) [3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane (trade name: OXT-221, manufactured by Toagosei Co., Ltd.)]: 60.0 parts

[0444] Cationic polymerizable compound (2) [3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate (trade name: CEL2021P, manufactured by Daicel Corporation)]: 32.5 parts

[0445] Cationic polymerizable compound (3) [1,2-epoxy-4-(2-oxacyclopropyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol (trade name: EHPE3150, manufactured by Daicel Corporation)]: 7.5 parts

[0446] Photocationic polymerization initiator [CPI-100P (San-Apro Co., Ltd., 50 mass % solution)]: 2.3 parts

[0447] Photosensitizer [9,10-dibutoxyanthracene]: 1.0 part

[0448] Photosensitizing agent [1,4-diethoxynaphthalene]: 1.0 part

[0449] [Preparation of Adhesive Composition (b)]

[0450] A mixed solution of 81.8 parts of ethyl acetate, 90.0 parts of butyl acrylate, 5.0 parts of methyl acrylate and 5.0 parts of acrylic acid was added to a reaction vessel equipped with a condenser, a nitrogen introduction tube, a thermometer and a stirrer, and the internal temperature was raised to 55°C while replacing the air in the device with nitrogen to make it oxygen-free. Then, the entire amount of a solution obtained by dissolving 0.15 parts of azobisisobutyronitrile (polymerization initiator) in 10 parts of ethyl acetate was added. After adding the polymerization initiator, the temperature was maintained for 1 hour. Then, while the internal temperature was maintained at 54 to 56°C, ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr. The addition of ethyl acetate was stopped at the time when the concentration of the (meth)acrylic resin reached 35%, and the temperature was kept until 6 hours from the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the (meth)acrylic resin to 20%, thereby preparing an acrylic resin solution. The weight average molecular weight Mw of the obtained acrylic resin was 1.6 million, and the molecular weight distribution Mw / Mn was 4.5. It should be noted that Mw and Mn were measured by converting to standard polystyrene in a GPC apparatus using two columns of TOSOH (S) in series, tetrahydrofuran as an eluent, and a sample concentration of 2 mg / mL, a sample introduction amount of 100 μL, a temperature of 40°C, and a flow rate of 1 mL / min.

[0451] To 100 parts of the solid content of the acrylic resin solution obtained above, 0.15 parts (based on the effective ingredient) of a crosslinking agent (manufactured by TOSOH Corporation: trade name "CORONATE L" (an ethyl acetate solution of a trimethylolpropane adduct of toluene diisocyanate (solid content concentration of 75%)) and 0.2 parts of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name "KBM-403") were added, and ethyl acetate was further added in such a manner that the solid content concentration became 13%, thereby obtaining an adhesive composition (b).

[0452] [Production of a separator with an adhesive layer]

[0453] (Manufacturing of Spacer (1) with Adhesive Layer)

[0454] As the separator (1), a release-treated stretched PET film (SP-PLR382050 manufactured by Lintec Corporation, thickness 38 μm) was used, and the above-obtained adhesive composition (b) was applied to the release-treated surface of the stretched PET film and dried to form a first adhesive layer (1) having a thickness of 20 μm. Thus, a separator (1) with an adhesive layer having a layer structure of separator (1) / first adhesive layer (1) was obtained.

[0455] (Manufacturing of Spacer (2) with Adhesive Layer)

[0456] As the separator (2), a stretched PET film (75 μm thick, CAO manufactured by Fujico Co., Ltd.) subjected to a release treatment on one side was used, and the adhesive composition (b) obtained above was applied to the release-treated surface of the stretched PET film and dried to form a first adhesive layer (2) having a thickness of 25 μm. Thus, a separator (2) with an adhesive layer having a layer structure of separator (2) / first adhesive layer (2) was obtained.

[0457] (Manufacturing of Spacer (3) with Adhesive Layer)

[0458] KBE-903 (manufactured by Shin-Etsu Silicone) as a silane coupling agent was dissolved in o-xylene to a concentration of 0.25% to prepare a release force adjustment layer forming composition (2). The release force adjustment layer forming composition (2) was applied to the release treated surface of a stretched PET film (thickness: 38 μm) (manufactured by LINTEC SP-PLR382050) using a bar coater, and dried in an oven at 120° C. for 1 minute to form a release force adjustment layer (2) having a thickness of 40 nm. This was used as a separator (3).

[0459] The adhesive composition (b) obtained above was applied onto the release force adjustment layer (2) of the separator (3) and dried to form a first adhesive layer (1) having a thickness of 20 μm. Thus, a separator (3) with an adhesive layer having a layer structure of separator (3) / first adhesive layer (1) was obtained.

[0460] (Manufacturing of the spacer (4) with adhesive layer)

[0461] The demolding surface of a stretched PET film (SP-PLR382050 manufactured by LINTEC, with a thickness of 38 μm) subjected to demolding treatment was subjected to corona treatment three times and the resulting product was used as an insulator (4). The corona treatment was carried out using a corona treatment device (AGF-B10, manufactured by Kasuga Electric Co., Ltd.) under conditions of an output power of 0.3 kW and a treatment speed of 3 m / min. The adhesive composition (b) obtained above was applied to the corona-treated surface and dried to form a first adhesive layer (1) with a thickness of 20 μm. Thus, an insulator (4) with an adhesive layer having a layer structure of insulator (4) / first adhesive layer (1) was obtained.

[0462] [Example 1]

[0463] A cellulose triacetate film (KC2UA, manufactured by KONICA MINOLTA Co., Ltd., with a thickness of 25 μm) as the first protective layer (1) was subjected to a corona treatment once under the conditions of an output of 0.3 kW and a treatment speed of 3 m / min using a corona treatment device (AG F-B10, manufactured by Kasuga Electric Co., Ltd.). The corona-treated surface of the cut-out first protective layer was coated with the composition for forming an anisotropic light-absorbing layer (1) prepared above using a bar coater, and then dried in a drying oven set at a temperature of 100° C. for 1 minute. Subsequently, ultraviolet rays (under a nitrogen atmosphere, wavelength: 365 nm, cumulative light intensity at a wavelength of 365 nm: 500 mJ / cm 2 ), thereby forming a light absorption anisotropic layer (1) in which the polymerizable liquid crystal compound and the dichroic pigment are vertically oriented relative to the coating plane. The thickness of the light absorption anisotropic layer (1) is 1.0 μm. Thus, a first laminate (1) having a layer structure of first protective layer (1) / light absorption anisotropic layer (1) is obtained.

[0464] Next, the light absorption anisotropic layer (1) of the first laminate (1) was subjected to a corona treatment, and then the resin composition containing a water-soluble polymer prepared above was applied using a bar coater, and dried at 100° C. for 2 minutes to form a second protective layer (1) having a thickness of 1 μm and composed of a film of a water-soluble polymer. Thus, a second laminate (1) having a layer structure of first protective layer (1) / light absorption anisotropic layer (1) / second protective layer (1) was obtained.

[0465] The second protective layer (1) side of the second laminate (1) is bonded to the first adhesive layer (1) side of the spacer (1) with an adhesive layer, and the first protective layer (1) side of the second laminate is bonded to the second adhesive layer (1) side of the surface protective film (1) to obtain an optical laminate (1). The layer structure of the optical laminate (1) is surface protective film (1) (stretched PET film (1) / second adhesive layer (1)) / first protective layer (1) / light absorption anisotropic layer (1) / second protective layer (1) / first adhesive layer (1) / spacer (1).

[0466] [Example 2]

[0467] An optical laminate (2) was obtained by the same procedure as in Example 1, except that the second adhesive layer (1) of the surface protective film (1) and the first protective layer (1) side of the second laminate were subjected to one corona treatment using a corona treatment device (AGF-B10, manufactured by Kasuga Electric Co., Ltd.) at an output of 0.3 kW and a treatment speed of 3 m / min. The layer structure of the optical laminate (2) was surface protective film (1) (stretched PET film (1) / second adhesive layer (1)) / first protective layer (1) / light absorption anisotropic layer (1) / second protective layer (1) / first adhesive layer (1) / spacer (1).

[0468] [Example 3]

[0469] After corona treatment, the photocurable composition was applied to the light absorption anisotropic layer (1) of the first laminate (1) using a bar coater so that the accumulated light amount of UVA was about 500 mJ / cm 2 The photocurable composition was cured by irradiating with ultraviolet light in a manner of 0.1% (measured value obtained by measuring device: UV PowerPuckII manufactured by FusionUV) to form a second protective layer (2). The thickness of the second protective layer (2) was 3 μm. Thus, a second laminate (2) having a layer structure of first protective layer (1) / light absorption anisotropic layer (1) / second protective layer (2) was obtained.

[0470] An optical laminate (3) was obtained by the same procedure as in Example 1 except that the second laminate (2) was used instead of the second laminate (1). The layer structure of the optical laminate (3) was surface protective film (1) (stretched PET film (1) / second adhesive layer (1)) / first protective layer (1) / light absorption anisotropic layer (1) / second protective layer (2) / first adhesive layer (1) / spacer (1).

[0471] [Example 4]

[0472] An optical laminate (4) was obtained by the same procedure as in Example 1 except that a cycloolefin polymer (COP) film (ZF14-023, manufactured by Zeon Co., Ltd., Japan, with a thickness of 23 μm) was used as the first protective layer (2) instead of the first protective layer (1), and a light absorption anisotropic layer-forming composition (2) was used instead of the light absorption anisotropic layer-forming composition (1). The thickness of the light absorption anisotropic layer (2) was 1.0 μm. The layer structure of the optical laminate (4) was surface protective film (1) (stretched PET film (1) / second adhesive layer (1)) / first protective layer (2) / light absorption anisotropic layer (2) / second protective layer (1) / first adhesive layer (1) / spacer (1).

[0473] [Example 5]

[0474] An optical laminate (5) was obtained by the same procedure as in Example 4 except that a cycloolefin polymer (COP) film (ZF14-023, manufactured by Zeon Co., Ltd., Japan, with a thickness of 13 μm) was used as the first protective layer (3) instead of the first protective layer (2). The layer structure of the optical laminate (5) was surface protective film (1) (stretched PET film / second adhesive layer (1)) / first protective layer (3) / light absorption anisotropic layer (2) / second protective layer (1) / first adhesive layer (1) / spacer (1).

[0475] [Example 6]

[0476] An optical layered body (6) was obtained by the same procedure as in Example 5 except that the surface protective film (2) was used instead of the surface protective film (1). The layer structure of the optical layered body (6) was surface protective film (2) (stretched PET film (2) / second adhesive layer (1)) / first protective layer (3) / light absorption anisotropic layer (2) / second protective layer (1) / first adhesive layer (1) / spacer (1).

[0477] [Example 7]

[0478] An optical layered body (7) was obtained by the same procedure as in Example 5 except that the surface protective film (3) was used instead of the surface protective film (1). The layer structure of the optical layered body (7) was surface protective film (3) (stretched PET film (3) / second adhesive layer (1)) / first protective layer (3) / light absorption anisotropic layer (2) / second protective layer (1) / first adhesive layer (1) / spacer (1).

[0479] [Example 8]

[0480] An optical layered body (8) was obtained by the same procedure as in Example 7 except that a separator (2) with an adhesive layer was used instead of the separator (1) with an adhesive layer. The layer structure of the optical layered body (8) was surface protective film (3) (stretched PET film (3) / second adhesive layer (1)) / first protective layer (3) / light absorption anisotropic layer (2) / second protective layer (1) / first adhesive layer (2) / separator (2).

[0481] [Example 9]

[0482] (Production of the first protective layer (4) with stretched PET film)

[0483] The following components were mixed and stirred at 50° C. for 4 hours to obtain a hard coat layer-forming composition (hereinafter also referred to as “HC layer-forming composition”).

[0484] A multifunctional acrylate compound having the following structure (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK ester A-DPH" (dipentaerythritol hexaacrylate): 50 parts

[0485] [Chemical formula 21]

[0486]

[0487] Urethane acrylate polymer (manufactured by DAICEL Allnex Ltd., “EBEC RYL 4858”, number of functional groups: 2, weight average molecular weight: 450, number of functional groups per unit molecular weight: 44.4×10 -4 ): 50 copies

[0488] Radical polymerization initiator (manufactured by BASF, "Irgacure 907" (2-[4-(methylthio)benzoyl]-2-(4-morpholinyl)propane)): 3 parts

[0489] Solvent (methyl ethyl ketone): 10 parts

[0490] The release-treated surface of a stretched PET film (SP-PLR382050 manufactured by LINTEC) was subjected to corona treatment, and then the HC layer-forming composition prepared above was applied by a bar coating method (#2 30 mm / s). The coating film of the HC layer-forming composition obtained was irradiated with an exposure dose of 500 mJ / cm using a UV irradiation device (SPOT CURE SP-7; manufactured by USHIO INC.). 2The first protective layer (4) was formed by ultraviolet rays (based on 365 nm) of a stretched PET film. The hard coating layer was used as the first protective layer (4). The thickness was measured using a laser microscope (OLS3000 manufactured by Olympus Corporation). Thus, the first protective layer (3) with a stretched PET film having a layer structure of stretched PET film / first protective layer (4) was obtained.

[0491] The first laminate (2) was obtained by the same procedure as that for the preparation of the first laminate (1) described in Example 1, except that the first protective layer (4) with a stretched PET film was used instead of the first protective layer (1), and the light absorption anisotropic layer-forming composition (3) was used instead of the light absorption anisotropic layer-forming composition (1). The thickness of the light absorption anisotropic layer (3) was 1.0 μm. The first laminate (2) had a layer structure of the first protective layer (4) with a stretched PET film (stretched PET film / first protective layer (4)) / light absorption anisotropic layer (3).

[0492] The second laminate (3) was obtained by the steps described in Example 1 except that the first laminate (2) was used instead of the first laminate (1). The second laminate (3) had a layer structure of a first protective layer (4) having a stretched PET film (stretched PET film / first protective layer (4)) / light absorption anisotropic layer (3) / second protective layer (1).

[0493] After the second protective layer (1) side of the second laminate (3) is bonded to the first adhesive layer (1) side of the separator (1) with an adhesive layer, the stretched PET film of the second laminate (3) is peeled off and removed. The first protective layer (4) thus exposed is bonded to the second adhesive layer (1) side of the surface protective film (1) to obtain an optical laminate (9). The layer structure of the optical laminate (9) is surface protective film (1) (stretched PET film (1) / second adhesive layer (1)) / first protective layer (4) / light absorption anisotropic layer (3) / second protective layer (1) / first adhesive layer (1) / separator (1).

[0494] [Example 10]

[0495] An optical layered body (10) was obtained by the same procedure as in Example 9 except that the surface protective film (3) was used instead of the surface protective film (1), and the separator (2) with an adhesive layer was used instead of the separator (1) with an adhesive layer. The layer structure of the optical layered body (10) was surface protective film (3) (stretched PET film (3) / second adhesive layer (1)) / first protective layer (4) / light absorption anisotropic layer (3) / second protective layer (1) / first adhesive layer (2) / separator (2).

[0496] [Example 11]

[0497] After the release strength adjusting layer (1) of the surface protection film (4) was subjected to corona treatment, the HC layer forming composition prepared above was applied by a bar coating method (#2 30 mm / s). The coating film of the HC layer forming composition was irradiated with an exposure dose of 500 mJ / cm using a UV irradiation device (SPOT CURE SP-7; manufactured by USHIO INC.). 2 The first protective layer (4) was formed by applying ultraviolet light (based on 365 nm) to the surface of the substrate to form a hard coating layer with a thickness of 2 μm. The hard coating layer was used as the first protective layer (4). The thickness was measured using a laser microscope (OLS3000 manufactured by Olympus Corporation). Thus, a first protective layer (4) with a surface protective film (4) having a layer structure of surface protective film (4) / first protective layer (4) was obtained.

[0498] A light absorbing anisotropic layer (3) is formed on the first protective layer (4) with a surface protective film (4) instead of the first protective layer (1) by the steps described in Example 9. After the surface of the light absorbing anisotropic layer (3) opposite to the first protective layer (4) is subjected to corona treatment, the resin composition containing a water-soluble polymer prepared above is applied using a rod coater and dried at a temperature of 100° C. for 2 minutes to form a second protective layer (1) with a thickness of 1 μm formed by a film of a water-soluble polymer. The second protective layer (1) is bonded to the first adhesive layer (1) of a spacer (3) with an adhesive layer to obtain an optical laminate (11). The layer structure of the optical laminate (11) is surface protective film (4) (stretched PET film) / first protective layer (4) / light absorbing anisotropic layer (3) / second protective layer (1) / first adhesive layer (1) / spacer (3).

[0499] [Example 12]

[0500] An optical layered body (12) was obtained by the same procedure as in Example 11 except that the surface protective film (5) was used instead of the surface protective film (4), and the separator (1) with an adhesive layer was used instead of the separator (3) with an adhesive layer. The layer structure of the optical layered body (12) was surface protective film (5) (stretched PET film) / first protective layer (4) / light absorption anisotropic layer (3) / second protective layer (1) / first adhesive layer (1) / separator (1).

[0501] [Comparative Example 1]

[0502] An optical layered body (c1) was obtained by the same procedure as in Example 12 except that the surface protective film (6) was used instead of the surface protective film (5) and the light absorption anisotropic layer-forming composition (1) was used instead of the light absorption anisotropic layer-forming composition (3). The layer structure of the optical layered body (c1) was surface protective film (6) (stretched PET film) / first protective layer (4) / light absorption anisotropic layer (1) / second protective layer (1) / first adhesive layer (1) / separator (1).

[0503] [Comparative Example 2]

[0504] An optical layered body (c2) was obtained by the same procedures as in Example 10, except that when the second adhesive layer (1) of the surface protective film (3) and the first protective layer (4) were bonded together, the respective bonding surfaces were subjected to corona treatment, the light absorption anisotropic layer-forming composition (1) was used instead of the light absorption anisotropic layer-forming composition (3), and the separator (4) with an adhesive layer was used instead of the separator (2) with an adhesive layer. The layer structure of the optical layered body (c2) was surface protective film (3) (stretched PET film (3) / second adhesive layer (1)) / first protective layer (4) / light absorption anisotropic layer (1) / second protective layer (1) / first adhesive layer (1) / separator (4).

[0505] 〔Reference Example 1〕

[0506] (Preparation of Composition for Forming Photo-Alignment Layer)

[0507] The following components described in JP-A-2013-033249 were mixed, and the obtained mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a photo-alignment layer.

[0508] Photo-alignable polymer having the structure shown below: 2 parts

[0509] [Chemical formula 22]

[0510]

[0511] Solvent (o-xylene): 98 parts

[0512] (Formation of Photo-Alignment Layer)

[0513] After the surface of the cycloolefin polymer (COP) film (ZF14-050, manufactured by Zeon Co., Ltd., Japan, with a thickness of 50 μm) as the first protective layer (5) was subjected to corona treatment, the composition for forming a photo-alignment layer prepared above was applied, and dried at a temperature of 120° C. to obtain a dry film. Polarized UV light was irradiated onto the dry film to form a photo-alignment layer, thereby obtaining a film with a photo-alignment layer. In the polarized UV light treatment, a UV irradiation device (SP OT CURE SP-7; manufactured by USHIO INC.) was used under the condition that the intensity measured at a wavelength of 365 nm was 100 mJ. The thickness of the photo-alignment layer was 100 nm.

[0514] On the photo-alignment layer of the film with the photo-alignment layer, the composition for forming a light-absorbing anisotropic layer (3) was applied by a bar coater, and heated and dried in a drying oven at a temperature of 120° C. for 1 minute, thereby causing the polymerizable liquid crystal compound to phase-transform into a liquid phase, and then cooled to room temperature to cause the polymerizable liquid crystal compound to phase-transform into a smectic liquid crystal state. Next, a UV irradiation device (SPOT CURE SP-7; manufactured by USHIO INC.) was used to expose the film at an exposure dose of 1000 mJ / cm 2 The layer formed by the composition (3) for forming an anisotropic light-absorbing layer is irradiated with ultraviolet rays (based on 365 nm), thereby polymerizing the polymerizable liquid crystal compound contained in the dried film while maintaining the smectic liquid crystal state of the polymerizable liquid crystal compound to form a horizontally oriented anisotropic light-absorbing layer (4). After corona treatment on the anisotropic light-absorbing layer (4), the resin composition containing the water-soluble polymer prepared above is coated with a rod coater and dried at a temperature of 100° C. for 2 minutes to form a second protective layer (1) with a thickness of 1 μm formed by a film of the water-soluble polymer. Furthermore, the first adhesive layer (1) of the spacer (1) with an adhesive layer is bonded to the surface protective film (1) to obtain an optical laminate (r1). The layer structure of the optical laminate (r1) is surface protection film (1) (stretched PET film (1) / second adhesive layer (1)) / first protective layer (5) (COP film) / photo-alignment layer / light absorption anisotropic layer (4) / second protective layer (1) / first adhesive layer (1) / spacer (1).

[0515] 〔Reference Example 2〕

[0516] The first protective layer (2) (COP film, ZF14-023) was subjected to corona treatment, and the composition for forming anisotropic light absorption layer (4) was applied using a bar coater. After heating at 120° C. for 60 seconds, ultraviolet rays (in nitrogen atmosphere, cumulative light intensity at a wavelength of 365 nm: 500 mJ / cm) were irradiated from the coated surface using a high-pressure mercury lamp (Unicure VB-15201BY-A, manufactured by USHIO IN C.).2 ), thereby forming a light absorption anisotropic layer (5). The thickness of the light absorption anisotropic layer (5) was measured using an ellipsometer (M-220 manufactured by JASCO Corporation) and found to be 1.2 μm.

[0517] An optical laminate (r2) was obtained by the same procedure as in Example 1, except that a surface protective film (3) was used instead of the surface protective film (1), and a laminate in which a light absorption anisotropic layer (5) was formed on the first protective layer (2) obtained above was used instead of the laminate of the first protective layer (1) and the light absorption anisotropic layer (1). The layer structure of the optical laminate (r2) was surface protective film (3) (stretched PET film (3) / second adhesive layer (1)) / first protective layer (2) / light absorption anisotropic layer (5) / second protective layer (1) / first adhesive layer (1) / spacer (1).

[0518] [Measurement of thickness]

[0519] The thickness is measured using a contact-type film thickness meter or a laser microscope (OL S3000 manufactured by Olympus Corporation).

[0520] [Measurement of distance D]

[0521] In the optical laminate, the distance D from the surface of the first protective layer on the surface protection film side to the surface of the second protective layer on the first pressure-sensitive adhesive layer side was measured from the layer cross section using a laser microscope (OLS3000 manufactured by Olympus Corporation).

[0522] [Measurement of absorbance]

[0523] The laminated structure of the first protective layer / light absorption anisotropic layer / second protective layer in the optical laminate is bonded to a glass of 4 cm×4 cm×0.7 mm thick via a pressure-sensitive adhesive (manufactured by LINTEC) having a thickness of 25 μm, and this is used as a test piece (1). The laminated structure is such that the second protective layer side is arranged on the glass side. In Reference Example 1, the laminated structure of the COP film / photo-orientation layer / light absorption anisotropic layer (r1) of the optical laminate is bonded via the above-mentioned pressure-sensitive adhesive in such a way that the light absorption anisotropic layer (r1) side becomes the above-mentioned glass side, thereby preparing a test piece (1). The test piece (1) is placed in an ultraviolet-visible spectrophotometer ("UV-2450" manufactured by Shimadzu Corporation), and the absorbance is measured to determine Ax and Ax (z=60). Since the absorbance of the first protective layer and the second protective layer can be regarded as 0 (zero), Ax and Ax (z=60) measured for the measurement sample (1) can be regarded as the absorbance of the light absorption anisotropic layer.

[0524] The x-axis refers to an arbitrary direction in the plane of the light absorption anisotropic layer, the y-axis refers to the direction perpendicular to the x-axis in the film plane, and the z-axis refers to the thickness direction of the light absorption anisotropic layer. Ax is the absorbance at the maximum absorption wavelength of the light absorption anisotropic layer, and represents the absorbance of linearly polarized light vibrating in the x-axis direction. Ax(z = 60) is the absorbance at the maximum absorption wavelength when the light absorption anisotropic layer is rotated 60° around the y-axis, and represents the absorbance of linearly polarized light vibrating in the x-axis direction.

[0525] When measuring the absorbance, the test piece (1) is set in a UV-visible spectrophotometer ("UV-2450" manufactured by Shimadzu Corporation), and after calibration so that the absorbance at a wavelength of 800 nm becomes zero, Ax is measured. For Ax(z = 60), similarly, the test piece (1) is set and tilted, and after calibration so that the absorbance at a wavelength of 800 nm becomes zero, Ax(z = 60) is measured.

[0526] The satisfaction of the relationship (Az > (Ax + Ay) / 2) of the above formula (1) for the light absorption anisotropic layer is judged by the following steps.

[0527] In a state where the test piece (1) is rotated 30° and 60° in a manner including the y-axis, the same linearly polarized light as when measuring Ax is made incident, whereby Ax(z = 30°) and Ax(z = 60°) are measured. Similarly, in a state where the test piece (1) is rotated 30° and 60° in a manner including the x-axis, the same linearly polarized light as when measuring Ay is made incident, whereby Ay(z = 30°) and Ay(z = 60°) are measured.

[0528] In the case where there is no absorption anisotropy in the x-y plane, that is, when Ax and Ay are equal, Ax(z = 30°) = Ay(z = 30°) and Ax(z = 60°) = Ay(z = 60°). Therefore, Ax(z = 30°) and Ay(z = 30°) are denoted as A(z = 30°), Ax(z = 60°) and Ay(z = 60°) are denoted as A(z = 60°), and Ax(z = 90°) and Ay(z = 90°) are denoted as A(z = 90°).

[0529] In the case where the relationship of A(z = 30°) < A(z = 60°) holds, the relationship of A(z = 30°) < A(z = 60°) < A(z = 90°) = Az holds. Therefore, if A(z = 30°) > (Ax + Ay) / 2 or A(z = 60°) > (Ax + Ay) / 2, it is judged that the relationship of the above formula (1) is satisfied. The results are shown in Tables 1 to 3.

[0530] [Measurement of peel forces F1 and F2]

[0531] The peel force F1 and the peel force F2 were measured by the following procedure using a test piece (2) cut out from the optical layered body to a size of 25 mm in width×100 mm in length.

[0532] (Measurement of peel force F1)

[0533] The spacer is peeled off from the test piece (2) and the exposed first adhesive layer is attached to the glass substrate. Then, the surface protective film is peeled off 50 mm from the end in the length direction. In this state, during the low-speed peeling test, the upper and lower clamps of the tensile testing machine (AUTOGRAPH AG-1S testing machine, manufactured by Shimadzu Corporation) are used to clamp one end of the length direction of the test piece (2), and the glass substrate is clamped by the other clamping part. In an environment with a temperature of 23°C and a relative humidity of 50%, the test piece (2) is stretched and peeled off at a tensile speed of 300 mm / min in a 180° direction, and the peeling force at this time is recorded in the figure. In the high-speed peel test, a high-speed peel tester (VPA-H100, manufactured by Kyowa Interface Science) was used. One end of the surface protective film peeled off above in the longitudinal direction (one side with a width of 25 mm) was clamped by one clamping part of the high-speed peel tester, and the glass substrate was clamped by another clamping part of the high-speed peel tester. Under the conditions of temperature 23°C and relative humidity 50%, the film was stretched and peeled off at a peeling speed of 10,000 mm / min in the 180° direction. The peeling force at this time was recorded in the graph. Since the data immediately after the start of the measurement and before the end of the measurement are unstable, the data of 20% after the start of the measurement and the data of 20% after the end of the measurement were removed, and the average value was calculated only from the relatively stable middle part of 60% and was taken as the peeling force F1 [N / 25mm].

[0534] (Measurement of peel force F2)

[0535] On the entire surface of one side of a glass substrate (EAGLE XG, manufactured by Corning), a double-sided tape (Nicetack (trade name), manufactured by NICHI BAN CO., LTD.) with a width of 25 mm and a length of 22 cm was pasted in parallel with the long side direction, and the surface protective film side of the test piece (2) was adhered. Then, the separator was peeled off 50 mm from the end in the length direction. In this state, the separator was peeled off from the first adhesive layer in the same way as the measurement of the peeling force F1, and the peeling force at this time was recorded in the figure. Since the data just after the measurement and before the measurement is about to end are unstable, 20% of the data after the start of the measurement and 20% of the data after the end of the measurement were removed, and the average value was calculated only from the relatively stable middle part of 60%, which was used as the peeling force F2 [N / 25mm].

[0536] [Evaluation of peelability]

[0537] The optical laminate was cut into a size of 2.5 cm × 20 cm as a test piece (3). The surface protective film side of the test piece (3) was placed on a suction workbench and fixed by vacuum suction. In this state, the separator was peeled off along the long side of the test piece (3) at a low speed (about 300 mm / min) and a high speed (about 10000 mm / min) along the 180° direction. The peelability at each peeling speed and the appearance after peeling were evaluated according to the following criteria.

[0538] A: There is no abnormality in peelability and no abnormality in appearance after peeling.

[0539] B: When the separator was peeled off, the surface protection film side sometimes floated off the suction stage. However, if the separator was peeled off once and then peeled off again, it could be peeled off well, and no abnormality was observed in the appearance after peeling.

[0540] C: When the separator was peeled off, the surface protection film side sometimes floated off the suction stage. In addition, a crack-like stripe pattern was generated in any of the first protective layer, the light absorption anisotropic layer, the second protective layer, and the first pressure-sensitive adhesive layer of the optical laminate.

[0541] D: When the separator was peeled off, the surface protective film side floated from the suction workbench and the separator could not be peeled off. In addition, a large number of crack-like stripe patterns were generated in any of the first protective layer, the light absorption anisotropic layer, the second protective layer, and the first adhesive layer of the optical laminate, and sometimes fractured.

[0542] [Bending test]

[0543] The optical laminate was cut into a size of 100 mm in length and 10 mm in width using a super cutter to form a test piece (4). The test piece (4) was subjected to a bendability test using a cylindrical mandrel method using a bending resistance tester (manufactured by TR Giken Co., Ltd.). In the bendability test, the test piece (4) was wrapped around a cylindrical shaft (mandrel) having a diameter of 2 mm so that the surface protective film became the inner side, and the long side of the test piece (4) was bent at a temperature of 25°. Then, the long side of the test piece (4) was restored to the state before the test piece was bent, and the visual recognizability of the bent portion was confirmed and evaluated according to the following criteria.

[0544] A: No decrease in the visibility of the bent portion of the test piece (4) was observed before and after the bendability test.

[0545] B: A slight decrease in the visibility of the bent portion of the test piece (4) was observed before and after the bendability test.

[0546] C: A decrease in the visibility of the bent portion of the test piece (4) was observed before and after the bendability test.

[0547] [Table 1]

[0548]

[0549] [Table 2]

[0550]

[0551] [Table 3]

[0552]

Claims

1. An optical laminate comprising a surface protective film, a first protective layer, a light absorption anisotropic layer, a second protective layer, a first adhesive layer and a separator laminated in this order, The surface protection film and the separator both comprise a stretched polyester film. The light absorption anisotropic layer comprises a polymer of a polymerizable liquid crystal compound and a dichroic pigment, and satisfies the following relationships (1) to (3): The peeling force F1 [N / 25 mm] between the surface protection film and the first protection layer, and the peeling force F2 [N / 25 mm] between the separator and the first adhesive layer satisfy the relationship of the following formulas (4) to (6): The distance from the surface of the first protective layer on the surface protection film side to the surface of the second protective layer on the first adhesive layer side is 30 μm or less. Az>(Ax+Ay) / 2 (1) 0.001≤Ax≤0.1 (2) Ax(z=60°) / Ax≥5 (3) 0.05≤F1≤0.30 (4) 0.02≤F2≤0.15 (5) 0.02≤F1-F2 (6) In formulas (1) to (3), Ax, Ay, and Az are absorbances of the absorption maximum wavelength of the light absorption anisotropic layer within the wavelength range of 380 nm to 780 nm, and respectively represent absorbances of linearly polarized light vibrating in the x-axis direction, y-axis direction, and z-axis direction, Ax(z=60°) is the absorbance at the absorption maximum wavelength and represents the absorbance of linearly polarized light vibrating in the x-axis direction when the light absorption anisotropic layer is rotated 60° about the y-axis as the rotation axis. in, The x-axis is any direction within the plane of the light absorption anisotropic layer. The y-axis is a direction orthogonal to the x-axis in the plane of the light absorption anisotropic layer, The z-axis is a direction orthogonal to the x-axis and the y-axis.

2. The optical laminate according to claim 1, wherein: The stretched polyester film included in the surface protection film has a thickness of 30 μm or more.

3. The optical laminate according to claim 1, wherein: The stretched polyester film included in the separator has a thickness of 30 μm or more.

4. The optical laminate according to claim 1, wherein: The surface protection film is a laminate of a stretched polyester film and a second adhesive layer.

5. The optical laminate according to claim 1, wherein: The stretched polyester films included in the surface protection film and the separator are both biaxially stretched polyester films.

6. The optical laminate according to claim 1, wherein: The surface protection film is in direct contact with the first protection layer.

7. The optical laminate according to claim 1, wherein: The first protective layer is directly in contact with the light-absorbing anisotropic layer, or only an alignment layer is provided between the first protective layer and the light-absorbing anisotropic layer.

8. The optical laminate according to claim 1, wherein: The light absorption anisotropic layer is directly in contact with the second protective layer.

9. The optical layered body according to claim 1, wherein: The polymerizable liquid crystal compound is a liquid crystal compound that forms a smectic phase.

10. The optical layered body according to claim 1, wherein: The first protective layer has a thickness of 28 μm or less.

11. The optical laminate according to claim 1, wherein: The second protective layer has a thickness of 15 μm or less. 12 . A wound body obtained by winding the optical layered body according to claim 1 .