Tungsten / molybdate fluorescent material applied to indoor plant illumination and silicon-based solar cell spectrum conversion

By doping Bi3+ fluorescent materials, the problem of mismatch between the solar spectrum and the absorption spectrum of solar cells is solved, the efficiency of solar cells is improved, and specific wavelengths of light are provided for plants to promote plant growth.

CN118725864AActive Publication Date: 2024-10-01YANBIAN UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410763710.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-07
Filing Date
2024-06-13
Publication Date
2024-10-01
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

In the existing technology, the solar spectrum does not match the absorption spectrum of silicon-based solar cells, resulting in low solar cell conversion efficiency. Indoor plant cultivation requires specific wavelengths of light to promote plant growth, but traditional light sources cannot effectively meet this requirement.

Method used

Develop a Bi3+-doped fluorescent material with the chemical formula A9M2(1-x-y)N4O24:xBi,yR. It is used for plant lighting and solar cell spectrum conversion. It emits blue light, red light to near-infrared light through ultraviolet light excitation, matching the plant's Photosynthesis needs and solar cell absorption needs.

Benefits of technology

It improves the conversion efficiency of solar cells and the growth rate of plants, provides efficient plant supplementary lighting, and simplifies the material preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004891799490000011
    Figure HDA0004891799490000011
  • Figure HDA0004891799490000012
    Figure HDA0004891799490000012
  • Figure HDA0004891799490000013
    Figure HDA0004891799490000013
Patent Text Reader

Abstract

The invention discloses a tungsten / molybdate fluorescent material applied to indoor plant illumination and silicon-based solar cell spectrum conversion, and belongs to the technical field of fluorescent material science. The chemical formula is A9M2 (1-x-y) N4O24: xBi, yR, and A is one or more of Sr, Ca and Ba; m is one or more of La, Gd and Y; n is one or a combination of W and Mo; o is an oxygen element; r is one or a combination of Yb and Nd; 0.01 < = x < = 0.25; 0.00 < = y < = 0.11. The device is used for indoor plant illumination and silicon-based solar cell spectrum conversion. 400-500 nm blue light and 600-700 nm red light which are correspondingly absorbed by chlorophyll a, chlorophyll b, carotenoid, phytochrome PR and PFR can be provided; and ultraviolet and visible light are absorbed and converted into near-infrared light, so that the utilization rate of sunlight is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to indoor plant cultivation lighting and silicon-based solar cell fluorescent materials, belonging to the technical field of fluorescent material science. Background Art

[0002] With the continuous development of society, the global population has gradually increased, and material conditions have gradually improved, which has led to an increasing demand for food. At the same time, the rapid development of urbanization and industrialization has led to less and less land resources for farming. At this time, indoor plant cultivation has attracted much attention due to its relatively stable growth environment and is not affected by increasingly frequent bad weather. It has become one of the important ways to solve the problem of food shortage. Indoor plant cultivation mainly uses phosphor-converted light-emitting diodes and hydroponic systems to better control and produce plants. Among them, light-emitting diodes are mainly used to provide the light required by plants. It is well known that light can promote plant growth, provide a source of energy for plant growth, and accelerate plant growth by promoting photosynthesis. In photosynthesis, light is mainly used by chlorophyll a, chlorophyll b, carotenoids, and photosensitive pigments P in plants. R and P FR Among them, chlorophyll a, chlorophyll b and carotenoids mainly absorb blue light of 400nm to 500nm and deep red light of about 660nm, and photosensitive pigment P R , P FR It mainly absorbs deep red light at 660nm and far red light near 730nm, which shows that plants are selective in absorbing light. Compared with traditional plant lighting sources such as incandescent lamps, fluorescent lamps, and metal halide lamps, phosphor-converted light-emitting diodes can better meet the needs of plants for light of specific wavelengths. Therefore, it is of great research value and significance to find phosphors with excellent performance that can be used for plant lighting.

[0003] As the global demand for energy increases, there is an urgent need to find clean energy that can replace fossil energy. Solar energy is one of the best alternative energy sources that is free, inexhaustible, and environmentally friendly. Therefore, it is particularly important to make better use of solar energy. In past studies, silicon-based solar cells are the most common type of photovoltaic cells that convert solar energy into electrical energy. However, the mismatch between the solar spectrum and the cell absorption spectrum greatly limits the conversion efficiency of solar cells. Spectral down-conversion can convert high-energy ultraviolet visible light into low-energy near-infrared light, reducing energy loss, which is of great significance for improving the conversion efficiency of solar cells. Therefore, the development of efficient spectral down-conversion luminescent materials is of great research and significance. Summary of the invention

[0004] The purpose of this invention is to meet the development of agricultural lighting and to prepare new high-efficiency fluorescent materials, and to solve the mismatch between the solar spectrum and the battery absorption spectrum, and to greatly improve the conversion efficiency of solar cells. We provide Bi-doped 3+ The fluorescent material is consistent with the light excitation position of the LED chip, and the emission band is wide. After being excited by ultraviolet light, it can emit blue light, orange light, red light to near infrared light. In photosynthesis, light is mainly absorbed by chlorophyll a, chlorophyll b, carotenoids, and photosensitive pigments P in plants. R and P FR Chlorophyll a, chlorophyll b and carotenoids mainly absorb blue and purple light of 400-500nm, while photosensitive pigment P R , P FR It mainly absorbs deep red light of 660nm and far red light around 730nm. The above wavelengths of light are beneficial to the synthesis of plant carbohydrates and can also accelerate the growth and development of plants. Therefore, efficient plant supplementary lighting generally uses 400-500nm blue light and 600-700nm red light. 3+ The emission position covers the above range and meets the above conditions, so it is a new type of fluorescent material used in agricultural lighting. 3+ , Yb 3+ / Nd 3+ The co-doped phosphor, under ultraviolet light excitation, has an emission spectrum in the near-infrared region near 1100nm that matches the optimal absorption spectrum of crystalline silicon solar cells. It can absorb ultraviolet and visible light and convert it into near-infrared light, thereby improving the utilization rate of sunlight. Therefore, it is also a high-efficiency fluorescent material for spectral conversion of solar cells.

[0005] To achieve the purpose of the present invention, the present invention adopts the following technical scheme, which is applied to plant lighting and silicon-based solar cell spectrum conversion fluorescent materials, and its chemical expression is A9M 2(1-x-y) N4O 24 :xBi,yR, wherein A is one or more of Sr, Ca, and Ba; M is one or more of La, Gd, and Y; N is one or a combination of W and Mo; O is oxygen; R is one or a combination of Yb and Nd; 0.01≤x≤0.25; 0.00≤y≤0.11.

[0006] Further including:

[0007] S9M 2(1-x-y) W4O 24 :xBi,yR (M=La, Gd, Y; R=Yb, Nd; 0.01≤x≤0.25; 0.00≤y≤0.11);

[0008] Ca9M 2(1-x) W4O 24 :xBi(M=La, Gd, Y; 0.01≤x≤0.25)

[0009] 9Mh 2(1-x) W4O 24 :xBi(M=La, Gd, Y; 0.01≤x≤0.25)

[0010] S9M 2(1-x) Mo4O 24 :xBi(M=La, Gd, Y; 0.01≤x≤0.25)

[0011] This type of phosphor can achieve emission ranging from blue light, orange light, red light to near infrared light, and can be used in plant lighting and spectral conversion fluorescent materials for silicon-based solar cells, such as Sr9La 1.50 W4O 24 :0.25Bi 3+ With red emission, Sr9Y 1.90 W4O 24 :0.05Bi 3+ With blue light emission, Sr9La 1.47 W4O 24 :0.25Bi 3+ ,0.015Yb 3+ With near infrared emission, etc., further, such phosphors include but are not limited to:

[0012] S9L 1.5 W4O 24 :0.25Bi 3+ 、Sr9Gd 1.9 W4O 24 :0.05Bi 3+ ,Sr9Y 1.9 W4O 24 :0.05Bi 3+ 、Ca9La 1.9 W4O 24 :0.05Bi 3+ , Ca9Gd 1.9 W4O 24 :0.05Bi 3+ , Ca9Y 1.9 W4O 24 :0.05Bi 3+ 、Ba9La 1.9 W4O 24 :0.05Bi 3 + 、Ba9Gd 1.9 W4O 24:0.05Bi 3+ ,Ba9Y 1.9 W4O 24 :0.05Bi 3+ 、Sr9La 1.9 Mo4O 24 :0.05Bi 3+ 、Sr9Gd 1.9 Mo4O 24 :0.05Bi 3+ ,Sr9Y 1.9 Mo4O 24 :0.05Bi 3+ 、Sr9La 1.47 W4O 24 :0.25Bi 3+ ,0.015Yb 3+ 、Sr9La 1.36 W4O 24 :0.25Bi 3 + ,0.07Nd 3+ wait.

[0013] The preparation method of the above-mentioned tungsten / molybdate fluorescent material is a conventional high-temperature solid-phase sintering method. The raw materials of the fluorescent material are all oxides and inorganic salts of various elements, including but not limited to oxides and carbonates, and are all obtained by a high-temperature solid-phase method. The specific dosage is calculated according to the chemical formula of the fluorescent material, ground, calcined, cooled and ground to obtain the fluorescent material of the present invention. The calcination temperature is 600-1400°C and the calcination time is 4-8 hours. The calcination temperature and time are slightly different depending on the basic materials of the fluorescent powder.

[0014] The tungsten / molybdate fluorescent material obtained by the present invention is used for indoor plant lighting and spectrum conversion of silicon-based solar cells. The chlorophyll a, chlorophyll b, carotenoids, and photosensitive pigments P in plant photosynthesis used for indoor plant lighting are R and P FR Absorbs the corresponding specific wavelength of 400-500nm blue light and / or 600-700nm red light; used for spectrum conversion of silicon-based solar cells: absorbs ultraviolet and visible light and converts them into near-infrared light, thereby improving the utilization rate of sunlight.

[0015] Performance evaluation:

[0016] (1) Optical absorption and emission properties: The excitation spectrum and emission spectrum of the phosphor sample obtained by the present invention were obtained using an Edinburgh FLS-1000 fluorescence spectrometer. The emission spectrum measured two wavelength ranges of 450nm-900nm and 600nm-1700nm. The excitation light source used was a 450W xenon lamp. All tests were performed at room temperature. The emission spectrum of the phosphor of the present invention has a large overlap with the absorption spectrum of plant chlorophyll, phytochrome, etc., and can be applied to the field of plant lighting.

[0017] (2) At the same time, it involves converting high-energy ultraviolet and visible light into low-energy near-infrared light, reducing energy loss and significantly improving the conversion efficiency of solar cells.

[0018] The raw materials of the invention are simple and easy to obtain, and the preparation method is simple. The invention is an ideal candidate material for indoor plant cultivation lighting and spectrum conversion phosphor for silicon-based solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 :Sr9La in Example 1 1.5 W4O 24 :0.25Bi 3+ Excitation spectrum of the material (λ em =714nm) and emission spectrum (λ ex =396nm).

[0020] Figure 2 : Sr9Gd in Example 2 1.9 W4O 24 :0.05Bi 3+ Excitation spectrum of the material (λ em =494nm) and emission spectrum (λ ex =351nm).

[0021] Figure 3 : Sr9Y in Example 3 1.9 W4O 24 :0.05Bi 3+ Excitation spectrum of the material (λ em =525nm) and emission spectrum (λ ex =336nm).

[0022] Figure 4 : Sr9La in Example 4 1.9 Mo4O 24 :0.05Bi 3+ Excitation spectrum of the material (λ em =520nm) and emission spectrum (λ ex =276nm).

[0023] Figure 5 : Ba9La in Example 5 1.9 W4O 24 :0.05Bi 3+ Excitation spectrum of the material (λ em =492nm) and emission spectrum (λ ex =342nm).

[0024] Figure 6 : Ca9Gd in Example 6 1.9 Mo4O 24 :0.05Bi 3+ Excitation spectrum of the material (λ em =505nm) and emission spectrum (λ ex =291nm).

[0025] Figure 7 : Ca9La in Example 7 1.9 Mo4O 24 :0.05Bi 3+ Excitation spectrum of the material (λ em =508nm) and emission spectrum (λ ex =291nm).

[0026] Figure 8 : Ca9Gd in Example 8 1.9 W4O 24 :0.05Bi 3+ Excitation spectrum of the material (λ em =492nm) and emission spectrum (λ ex =313nm).

[0027] Fig. 9 : Ca9Y in Example 9 1.9 W4O 24 :0.05Bi 3+ Excitation spectrum of the material (λ em =536nm) and emission spectrum (λ ex =327nm).

[0028] Fig.10 : Ca9La in Example 10 1.9 W4O 24 :0.05Bi 3+ Excitation spectrum of the material (λ em =710nm) and emission spectrum (λ ex =365nm).

[0029] Fig.11 :Sr9La in Example 11 1.36 W4O 24 :0.25Bi3+ ,0.07Nd 3+ Excitation spectrum of the material (λ em =1070nm) and emission spectrum (λ ex =396nm).

[0030] Fig.12 : Sr9La in Example 12 1.47 W4O 24 :0.25Bi 3+ ,0.015Yb 3+ Excitation spectrum of the material (λ em =982nm) and emission spectrum (λ ex =396nm).

[0031] Fig.13 :Sr9La in Example 1 1.5 W4O 24 :0.25Bi 3+ (λ ex =396nm), Sr9Gd in Example 2 1.9 W4O 24 :0.05Bi 3+ (λ ex =351nm) emission spectrum of materials and absorption spectrum of plant pigments.

[0032] Fig.14 :Sr9La in Example 12 1.47 W4O 24 :0.25Bi 3+ ,0.015Yb 3+ Excitation and emission spectra of materials, solar spectrum, and response curves of c-Si solar cell spectra. DETAILED DESCRIPTION

[0033] Embodiments of the present invention are described below, but the present invention is by no means limited to the following embodiments.

[0034] Embodiment 1:

[0035] The raw materials SrCO3, La2O3, WO3, Bi2O3 are pressed into Sr9La 1.5 W4O 24 :0.25Bi 3+ The chemical ratio was weighed and evenly mixed in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1400°C for 6 hours. After cooling, fine grinding was performed to obtain Sr9La 1.5 W4O 24 :0.25Bi 3+Fluorescent material. It can effectively emit red light to near infrared light under ultraviolet light excitation. Test results are shown in Figure 1 , the emission spectrum of the material and the absorption spectrum of the plant pigment are compared Fig.13 .

[0036] Embodiment 2:

[0037] The raw materials SrCO3, Gd2O3, WO3, Bi2O3 are pressed into Sr9Gd 1.9 W4O 24 :0.05Bi 3+ The chemical ratio was weighed and evenly mixed in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1400°C for 4 hours. After cooling, fine grinding was performed to obtain Sr9Gd 1.9 W4O 24 :0.05Bi 3+ Fluorescent material. Test results are shown in Figure 2 Comparison of the emission spectrum of the material and the absorption spectrum of the plant pigment can be seen in Fig.13 .

[0038] Embodiment 3:

[0039] The raw materials SrCO3, Y2O3, WO3, Bi2O3 are pressed into Sr9Y 1.9 W4O 24 :0.05Bi 3+ The stoichiometric ratio was weighed and evenly mixed in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1250°C for 6 hours. After cooling, fine grinding was performed to obtain Sr9Y 1.9 W4O 24 :0.05Bi 3+ Fluorescent material. Test results are shown in Figure 3 .

[0040] Embodiment 4:

[0041] The raw materials SrCO3, La2O3, MoO3, Bi2O3 are pressed into Sr9La 1.98 Mo4O 24 :0.01Bi 3+ The stoichiometric ratio was weighed and evenly mixed in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1400°C for 6 hours. After cooling, fine grinding was performed to obtain Sr9La 1.98 Mo4O 24 :0.01Bi 3+ Fluorescent material. Test results are shown in Figure 4 .

[0042] Embodiment 5:

[0043] The raw materials BaCO3, La2O3, WO3, Bi2O3 are pressed into Ba9La 1.9 W4O 24 :0.05Bi 3+ The stoichiometric ratio was weighed and mixed evenly in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 600°C for 2 hours, and then raised to 1200°C for calcination for 2 hours. After cooling, fine grinding was performed to obtain Ba9La 1.9 W4O 24 :0.05Bi 3+ Fluorescent material. Test results are shown in Figure 5 .

[0044] Embodiment 6:

[0045] The raw materials Ca2CO3, Gd2O3, MoO3, Bi2O3 are pressed into Ca9Gd 1.9 Mo4O 24 :0.05Bi 3+ The chemical ratio was weighed and mixed evenly in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1400°C for 4 hours. After cooling, fine grinding was performed to obtain Ca9Gd 1.9 Mo4O 24 :0.05Bi 3+ Fluorescent material. Test results are shown in Figure 6 .

[0046] Embodiment 7:

[0047] The raw materials Ca2CO3, La2O3, MoO3, Bi2O3 are pressed into Ca9La 1.9 Mo4O 24 :0.05Bi 3+ The chemical ratio was weighed and mixed evenly in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1400°C for 4 hours. After cooling, fine grinding was performed to obtain Ca9La 1.9 Mo4O 24 :0.05Bi 3+ Fluorescent material. Test results are shown in Figure 7 .

[0048] Embodiment 8:

[0049] The raw materials Ca2CO3, Gd2O3, WO3, Bi2O3 are pressed into Ca9Gd 1.9 W4O 24:0.05Bi 3+ The chemical ratio was weighed and mixed evenly in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1400°C for 4 hours. After cooling, fine grinding was performed to obtain Ca9Gd 1.9 W4O 24 :0.05Bi 3+ Fluorescent material. Test results are shown in Figure 8 .

[0050] Embodiment 9:

[0051] The raw materials Ca2CO3, Y2O3, WO3, Bi2O3 are pressed into Ca9Y 1.9 W4O 24 :0.05Bi 3+ The chemical ratio was weighed and mixed evenly in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1250°C for 6 hours. After cooling, fine grinding was performed to obtain Ca9Y 1.9 W4O 24 :0.05Bi 3+ Fluorescent material. Test results are shown in Fig. 9 .

[0052] Embodiment 10:

[0053] The raw materials Ca2CO3, La2O3, WO3, Bi2O3 are pressed into Ca9La 1.9 W4O 24 :0.05Bi 3+ The chemical ratio was weighed and mixed evenly in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1400°C for 6 hours. After cooling, fine grinding was performed to obtain Ca9La 1.9 W4O 24 :0.05Bi 3+ Fluorescent material. Test results are shown in Fig.10 .

[0054] Embodiment 11:

[0055] The raw materials SrCO3, La2O3, WO3, Bi2O3, Nd2O3 are pressed into Sr9La 1.36 W4O 24 :0.25Bi 3+ ,0.07Nd 3+ The chemical ratio was weighed and evenly mixed in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1400°C for 6 hours. After cooling, fine grinding was performed to obtain Sr9La1.36 W4O 24 :0.25Bi 3+ ,0.07Nd 3+ Fluorescent material. It can effectively emit red light to near infrared light under ultraviolet light excitation. Test results are shown in Fig.11 .

[0056] Embodiment 12:

[0057] The raw materials SrCO3, La2O3, WO3, Bi2O3, Yb2O3 are pressed into Sr9La 1.47 W4O 24 :0.25Bi 3+ ,0.015Yb 3+ The chemical ratio was weighed and evenly mixed in a mortar for 30 minutes. The obtained fractions were placed in a corundum crucible with a lid and then placed in a calcining furnace for calcination at 1400°C for 6 hours. After cooling, fine grinding was performed to obtain Sr9La 1.47 W4O 24 :0.25Bi 3+ ,0.015Yb 3+ Fluorescent material. It can effectively emit red light to near infrared light under ultraviolet light excitation. Test results are shown in Fig.12 The excitation and emission spectra of the material, the solar spectrum, and the response curves of the c-Si solar cell spectrum are shown in Fig.14 .

[0058] Sample doped with Bi 3+ The excitation position is in the range of 200-550nm, which is consistent with the excitation position of the LED chip, and the emission band is wide. After being excited by ultraviolet light, it can emit blue light, orange light, red light to near infrared light. 3+ The emission spectrum of phosphor and the absorption spectrum of plant photosensitive pigments chlorophyll a, chlorophyll b, carotenoids, P R , P FR There is a large overlap and can be applied to the field of plant lighting. 3+ The excitation peaks of Bi are mostly located at 300nm~400nm, and 3+ Because of its 3 P1→ 1 The S0 transition has a broad emission band in the visible region, so Bi 3+ It acts as a sensitizer, absorbs ultraviolet light and then transfers energy to rare earth ions, thereby improving the conversion efficiency of silicon-based solar cells. The raw materials of the invention are cheap, the process is simple, it is easy to prepare, and it has stable chemical properties, good luminous performance, and low heat generation. It is an ideal candidate material for indoor plant cultivation lighting and silicon-based solar cell spectrum conversion phosphor.

Claims

1. A fluorescent material for spectrum conversion used in plant lighting and silicon-based solar cells, characterized in that: Its chemical formula is A9M 2(1-x-y) N4O 24 :xBi,yR, wherein A is one or more of Sr, Ca, and Ba; M is one or more of La, Gd, and Y; N is one or a combination of W and Mo; O is oxygen; R is one or a combination of Yb and Nd; 0.01≤x≤0.25; 0.00≤y≤0.

11.

2. A fluorescent material for spectrum conversion used in plant lighting and silicon-based solar cells according to claim 1, characterized in that: It includes the following chemical expressions: Sr9M 2(1-x-y) W4O 24 :xBi, yR, M=La, Gd, Y; R=Yb, Nd; 0.01≤x≤0.25; 0.00≤y≤0.11; or Ca9M 2(1-x) W4O 24 :xBi, M=La, Gd, Y; 0.01≤x≤0.25; or Ba9M 2(1-x) W4O 24 :xBi, M=La, Gd, Y; 0.01≤x≤0.25; Sr9M 2(1-x) Mo4O 24 :xBi,M,La,Gd,Y;0.01≤x≤0.25。 3. A fluorescent material for spectrum conversion used in plant lighting and silicon-based solar cells according to claim 1, characterized in that: Include one or more of the following: Sr9La 1.5 W4O 24 :0.25Bi 3+ 、Sr9Gd 1.9 W4O 24 :0.05Bi 3+ 、Sr9Y 1.9 W4O 24 :0.05Bi 3+ 、Ca9La 1.9 W4O 24 :0.05Bi 3+ 、Ca9Gd 1.9 W4O 24 :0.05Bi 3+ 、Ca9Y 1.9 W4O 24 :0.05Bi 3+ 、Ba9La 1.9 W4O 24 :0.05Bi 3+ 、Ba9Gd 1.9 W4O 24 :0.05Bi 3+ 、Ba9Y 1.9 W4O 24 :0.05Bi 3+ 、Sr9La 1.9 Mo4O 24 :0.05Bi 3+ 、Sr9Gd 1.9 Mo4O 24 :0.05Bi 3+ 、Sr9Y 1.9 Mo4O 24 :0.05Bi 3+ 、Sr9La 1.47 W4O 24 :0.25Bi 3+ ,0.015Yb 3+ 、Sr9La 1.36 W4O 24 :0.25Bi 3 + ,0.07Nd 3+ 。 4. A method for preparing a fluorescent material for plant lighting and spectrum conversion of silicon-based solar cells according to any one of claims 1 to 3, characterized in that: The high-temperature solid-phase sintering method is adopted. The raw materials are oxides and / or inorganic salts of various elements. The specific dosage is calculated according to the chemical formula of the fluorescent material, ground, calcined, and ground after cooling. The calcination temperature is 600-1400°C and the calcination time is 4-8 hours.

5. The use of a fluorescent material for plant lighting and silicon-based solar cell spectrum conversion as described in any one of claims 1 to 3 is used for indoor plant lighting and / or silicon-based solar cell spectrum conversion.

6. The use according to claim 5, wherein the chlorophyll a, chlorophyll b, carotenoids, and photosensitive pigments P in indoor plant lighting and plant photosynthesis R and P FR Absorbs the corresponding specific wavelengths of 400-500nm blue light and / or 600-700nm red light; used for spectrum conversion of silicon-based solar cells: absorbs ultraviolet and / or visible light and converts it into near-infrared light, thereby improving the utilization rate of sunlight.

Citation Information

Patent Citations

  • Red tungstate fluorescent material as well as preparation method and application thereof

    CN115537199A