Application of wafer surface treatment liquid
By adding fluorine-containing compounds, silane coupling agents and organic solvents to the wafer surface treatment liquid, the isopropyl alcohol contact angle is increased, which solves the problems of collapse and contamination of high aspect ratio structures caused by traditional treatment liquids, and realizes the drying process. stability and cleanliness.
Patent Information
- Application Number
- CN202310338372.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional wafer surface treatment solutions can easily cause gate collapse and contaminant residues in high aspect ratio structures during the cleaning and drying processes, affecting device performance.
Provide a wafer surface treatment solution containing 0.005-1% fluorine-containing compound, 0.1-20% silane coupling agent and organic solvent. The isopropyl alcohol contact angle is increased to avoid adhesion during the drying process and ensure a high aspect ratio. Structural stability.
It effectively avoids gate collapse, ensures the stability of high aspect ratio structures during the drying process, reduces contaminant residues, and improves the reliability of subsequent processes.
Smart Images

Figure BDA0004157270020000051 
Figure BDA0004157270020000061 
Figure BDA0004157270020000062
Abstract
Description
Technical Field
[0001] The invention relates to application of a wafer surface treatment liquid. Background Art
[0002] With the continuous development of the semiconductor industry, integrated circuits are gradually developing towards high integration and ultra-fine line widths. Therefore, more and more high aspect ratio structures are involved in the chip manufacturing process (in the semiconductor industry, structures with a depth / height and width ratio greater than or equal to 10 are generally defined as high aspect ratio). High aspect ratio structures not only face huge challenges during etching and deposition, but also have great problems in cleaning after etching. On the one hand, the current mainstream cleaning method is still wet cleaning based on water chemistry. For these micro-nano structures with small openings but large depths, it is difficult for liquids to enter the bottom of the grooves to achieve the purpose of cleaning; on the other hand, once the cleaning liquid enters the deep grooves, it is difficult to remove the liquid under the action of surface tension, resulting in residual contaminants, which become a potential threat to subsequent processes, and even cause device failure in severe cases. At the same time, the capillary force existing during the drying process of these high aspect ratio structures may also cause the collapse of these structures, resulting in device failure.
[0003] In the traditional IPA (isopropyl alcohol) spin-drying process, when the gate AR (aspect ratio) is greater than or equal to 10, the gate will adhere to the gate during the spin-drying process, causing the gate to collapse during the drying process. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the defect that the conventional wafer surface treatment liquid causes the gate to collapse during the spin-drying process of cleaning the wafer, and to provide an application of a wafer surface treatment liquid. After the wafer is cleaned by the wafer surface treatment liquid of the present invention, the isopropanol contact angle is significantly increased, and the gates will not adhere to each other during the drying process, thereby avoiding the occurrence of gate collapse.
[0005] The present invention solves the above technical problems through the following technical solutions.
[0006] The present invention provides an application of a wafer surface treatment liquid in cleaning wafers. The raw materials of the wafer surface treatment liquid include the following components in mass fractions: 0.005-1% of a fluorine-containing compound, 0.1-20% of a silane coupling agent and an organic solvent; the sum of the mass fractions of the components is 100%; the organic solvent makes up the balance;
[0007] The organic solvent is selected from one or more of isopropyl alcohol (IPA), propylene glycol methyl ether acetate (PGMEA), N,N-dimethylformamide (DMF), n-hexane, cyclohexanone, tetrahydrofuran, dichloromethane, acetone and xylene;
[0008] The silane coupling agent is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, 3-glycidylpropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, vinyltrimethoxysilane, dodecyltrimethoxysilane and 3-isocyanatepropyltrimethoxysilane.
[0009] In some embodiments, the fluorine-containing compound is selected from one or more of hydrogen fluoride, ammonium fluoride, ammonium bifluoride, tetramethylammonium fluoride, fluorosulfonic acid and trihydroxyethylammonium fluoride, perfluorooctylethylene, perfluorodecene, perfluorohexylethylene, perfluorooctene, perfluorobutylethylene and 1H,1H,2H-perfluoro-1-hexene;
[0010] Preferably, the fluorine-containing compound is hydrogen fluoride or fluorosulfonic acid.
[0011] In some embodiments, the mass fraction of the fluorine-containing compound is 0.005-0.10%;
[0012] Preferably, the mass fraction of the fluorine-containing compound is 0.01-0.05%.
[0013] In some embodiments, the silane coupling agent is 3-aminopropyltriethoxysilane.
[0014] In some embodiments, the mass fraction of the silane coupling agent is 1-15%;
[0015] Preferably, the mass fraction of the silane coupling agent is 5-10%.
[0016] In some embodiments, the organic solvent is selected from one or more of isopropyl alcohol, propylene glycol methyl ether acetate and N,N-dimethylformamide;
[0017] Preferably, the organic solvent is isopropyl alcohol and / or propylene glycol methyl ether acetate.
[0018] In some embodiments, when the organic solvent is isopropanol and propylene glycol methyl ether acetate, the mass ratio of the propylene glycol methyl ether acetate to the isopropanol is (1-2):1.
[0019] In some embodiments, the pH value of the wafer surface treatment solution is 7-12.
[0020] In some schemes, the raw materials of the wafer surface treatment solution include the following components by mass fraction: 0.01-0.05% fluorine-containing compound, 5-10% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance;
[0021] The organic solvent is selected from isopropyl alcohol (IPA) and / or propylene glycol methyl ether acetate (PGMEA);
[0022] The silane coupling agent is 3-aminopropyltriethoxysilane;
[0023] The fluorine-containing compound is hydrogen fluoride and / or fluorosulfonic acid.
[0024] In some embodiments, the raw materials of the wafer surface treatment solution include any one of the following components in mass fractions:
[0025] Solution 1: 0.01% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance;
[0026] Solution 2: 0.01% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance;
[0027] Solution 3: 0.05% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance;
[0028] Solution 4: 0.05% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance;
[0029] Scheme 5: 0.01% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;
[0030] Scheme 6: 0.01% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;
[0031] Scheme 7: 0.05% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;
[0032] Scheme 8: 0.05% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;
[0033] Scheme 9: 0.01% fluorosulfonic acid, 5.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance;
[0034] Scheme 10: 0.01% fluorosulfonic acid, 10.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance;
[0035] Scheme 11: 0.05% fluorosulfonic acid, 5.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance;
[0036] Scheme 12: 0.05% fluorosulfonic acid, 10.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance.
[0037] Preferably, the raw materials of the wafer surface treatment liquid are composed of any of the above schemes.
[0038] In some embodiments, the wafer surface treatment liquid is used to clean the etched wafer, preferably, it includes the following steps:
[0039] (1) Soaking the etched wafer in an isopropyl alcohol cleaning solution (e.g., soaking for 1 minute);
[0040] (2) Soaking the wafer obtained in step (1) in the wafer surface treatment solution as described above (for example, soaking for 1 minute) and then drying.
[0041] In some embodiments, the wafer is a high aspect ratio wafer.
[0042] In some embodiments, the ratio of the depth to width of the wafer is greater than or equal to 10, preferably 10-100, and more preferably 10-50.
[0043] The term "high aspect ratio" of the present invention: In the semiconductor industry, a structure whose ratio of depth to width is greater than or equal to 10 is generally defined as having a high aspect ratio.
[0044] The "room temperature" of the present invention refers to 25±5°C.
[0045] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0046] The reagents and raw materials used in the present invention are commercially available.
[0047] The positive improvement effect of the present invention is that after the wafer surface treatment liquid of the present invention cleans the wafer, the isopropyl alcohol contact angle is significantly increased, and no adhesion occurs between the gates during the drying process, thereby avoiding the occurrence of gate collapse. DETAILED DESCRIPTION
[0048] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0049] The surface treatment liquid was prepared according to the ingredients and proportions of each example in Table 1, mixed evenly, and stirred at room temperature for 1 hour (without any order of addition).
[0050] Table 1
[0051]
[0052]
[0053] Note: “ / ” means does not exist.
[0054] This test was conducted using TEOS (tetraethoxysilane) and SiN (silicon nitride) wafers.
[0055] Experimental methods:
[0056] 1. Cut the wafer with aspect ratio of 10 into 30*30mm test pieces;
[0057] 2. Soak the test piece in isopropyl alcohol cleaning solution for 1 minute and take it out;
[0058] 3. Immerse the test pieces in the surface treatment solutions described in Table 1 for 1 min, take them out and blow dry;
[0059] 4. The contact angle of the test piece was tested using a contact angle tester (Attension Theta Lite). The test solution was isopropanol. The surface roughness was tested at the same time, and the surface of the test piece was observed using an electron microscope. The results are shown in Table 2 below.
[0060] Table 2
[0061]
[0062]
[0063] The test results show that after being immersed in the surface treatment liquid, the isopropyl alcohol contact angle increases significantly, and the gates will not stick together during the drying process, thus avoiding the collapse of the gates.
Claims
1. Application of a wafer surface treatment liquid in cleaning a wafer, characterized in that: The raw materials of the wafer surface treatment liquid include the following components in mass fraction: 0.005-1% fluorine-containing compound, 0.1-20% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance; The organic solvent is selected from one or more of isopropyl alcohol, propylene glycol methyl ether acetate, N,N-dimethylformamide, n-hexane, cyclohexanone, tetrahydrofuran, dichloromethane, acetone and xylene; The silane coupling agent is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, 3-glycidylpropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, vinyltrimethoxysilane, dodecyltrimethoxysilane and 3-isocyanatepropyltrimethoxysilane.
2. The use according to claim 1, characterized in that The raw materials of the wafer surface treatment solution meet one or more of the following requirements: (1) The fluorine-containing compound is selected from one or more of hydrogen fluoride, ammonium fluoride, ammonium bifluoride, tetramethylammonium fluoride, fluorosulfonic acid, trihydroxyethylammonium fluoride, perfluorooctylethylene, perfluorodecene, perfluorohexylethylene, perfluorooctene, perfluorobutylethylene and 1H,1H,2H-perfluoro-1-hexene; (2) The silane coupling agent is 3-aminopropyltriethoxysilane; (3) the organic solvent is selected from one or more of isopropyl alcohol, propylene glycol methyl ether acetate and N,N-dimethylformamide; (4) the mass fraction of the fluorine-containing compound is 0.005-0.10%; and (5) The mass fraction of the silane coupling agent is 1-15%.
3. The use according to claim 2, characterized in that The raw materials of the wafer surface treatment solution meet one or more of the following requirements: (1) The fluorine-containing compound is hydrogen fluoride and / or fluorosulfonic acid; (2) the organic solvent is isopropanol and / or propylene glycol methyl ether acetate; preferably, when the organic solvent is isopropanol and propylene glycol methyl ether acetate, the mass ratio of the propylene glycol methyl ether acetate to the isopropanol is (1-2):1; (3) The mass fraction of the fluorine-containing compound is 0.01-0.05%; (4) the mass fraction of the silane coupling agent is 5-10%; and (5) The pH value of the wafer surface treatment solution is 7-12.
4. The use according to any one of claims 1 to 3, characterized in that: The raw materials of the wafer surface treatment liquid include the following components in mass fraction: 0.01-0.05% fluorine-containing compound, 5-10% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance; The organic solvent is selected from isopropyl alcohol and / or propylene glycol methyl ether acetate; The silane coupling agent is 3-aminopropyltriethoxysilane; The fluorine-containing compound is hydrogen fluoride and / or fluorosulfonic acid.
5. The use according to claim 4, characterized in that The raw materials of the wafer surface treatment solution include any one of the following components in mass fractions: Solution 1: 0.01% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance; Solution 2: 0.01% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance; Solution 3: 0.05% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance; Solution 4: 0.05% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and isopropanol, with isopropanol making up the balance; Scheme 5: 0.01% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Scheme 6: 0.01% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Scheme 7: 0.05% hydrogen fluoride, 5.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Scheme 8: 0.05% hydrogen fluoride, 10.0% 3-aminopropyltriethoxysilane and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Scheme 9: 0.01% fluorosulfonic acid, 5.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance; Scheme 10: 0.01% fluorosulfonic acid, 10.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance; Scheme 11: 0.05% fluorosulfonic acid, 5.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance; Scheme 12: 0.05% fluorosulfonic acid, 10.0% 3-aminopropyltriethoxysilane and propylene glycol methyl ether acetate, with propylene glycol methyl ether acetate making up the balance.
6. The use according to claim 5, characterized in that The raw materials of the wafer surface treatment liquid are composed of any one of the schemes in claim 5.
7. The use according to any one of claims 1 to 6, characterized in that: The wafer surface treatment liquid can be used to clean the etched wafer.
8. The use according to claim 7, characterized in that It includes the following steps: (1) Soaking the etched wafer in an isopropyl alcohol cleaning solution; (2) Soaking the wafer obtained in step (1) in the wafer surface treatment solution and then drying.
9. The use according to any one of claims 1 to 8, characterized in that: The wafer is a high aspect ratio wafer.
10. The use according to claim 9, characterized in that The ratio of the depth to the width of the wafer is greater than or equal to 10.