Preparation method of fluorine-containing silane wafer surface treatment liquid

By using a combination of fluorine-containing silanes and silane coupling agents in the wafer surface treatment solution, the problems of adhesion and contamination residues caused by traditional cleaning solutions during high aspect ratio wafer spin-drying are solved, achieving more effective cleaning and Dry to avoid gate collapse.

CN118726006APending Publication Date: 2024-10-01SHANGHAI SINYANG SEMICONDUCTOR MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310341616.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

After traditional cleaning solutions are used to process high aspect ratio wafers, the gate electrode may collapse during the drying process, and the cleaning solution is difficult to completely remove, leaving behind contaminants that affect device performance.

Method used

Using a wafer surface treatment solution containing fluorine-containing silane and silane coupling agent, 0.005%-1% fluorine-containing silane, 0.1%-20% silane coupling agent and organic solvent (such as isopropyl alcohol, propylene glycol methyl ether acetate ) is mixed according to a specific ratio to form a surface treatment liquid that increases the contact angle of IPA and avoids adhesion and collapse.

Benefits of technology

The treated wafer surface changes from hydrophilic to hydrophobic, which reduces the risk of adhesion during the drying process, avoids gate collapse, and improves the cleaning effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004158293820000061
    Figure BDA0004158293820000061
  • Figure BDA0004158293820000071
    Figure BDA0004158293820000071
  • Figure BDA0004158293820000081
    Figure BDA0004158293820000081
Patent Text Reader

Abstract

The invention discloses a preparation method of a fluorine-containing silane wafer surface treatment liquid. The preparation method comprises the following step: mixing the raw materials of the wafer surface treatment liquid to obtain the wafer surface treatment liquid. Raw materials of the wafer surface treatment liquid comprise the following components in percentage by mass: 0.005%-1% of fluorine-containing silane, 0.1%-20% of a silane coupling agent and an organic solvent, the sum of the mass fractions of the components is 100%. The organic solvent is supplemented to the balance; after a wafer is treated by the wafer surface treatment liquid prepared by the preparation method disclosed by the invention, the IPA contact angle is obviously increased, and grid electrodes are not adhered in the drying process, so that the occurrence of grid electrode collapse is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a fluorine-containing silane wafer surface treatment liquid. Background Art

[0002] With the continuous development of the semiconductor industry, integrated circuits are gradually developing towards high integration and ultra-fine line widths. Therefore, more and more high aspect ratio structures are involved in the chip manufacturing process (in the semiconductor industry, structures with a depth / height and width ratio greater than or equal to 10 are generally defined as high aspect ratio). High aspect ratio structures not only face huge challenges during etching and deposition, but also have great problems in cleaning after etching. On the one hand, the current mainstream cleaning method is still wet cleaning based on water chemistry. For these micro-nano structures with small openings but large depths, it is difficult for liquids to enter the bottom of the grooves to achieve the purpose of cleaning; on the other hand, once the cleaning liquid enters the deep grooves, it is difficult to remove the liquid under the action of surface tension, resulting in residual contaminants, which become a potential threat to subsequent processes, and even cause device failure in severe cases. At the same time, the capillary force existing during the drying process of these high aspect ratio structures may also cause the collapse of these structures, resulting in device failure.

[0003] In the traditional IPA (isopropyl alcohol) spin-drying process, when the gate AR (aspect ratio) is greater than or equal to 10, a large force will be generated between the IPA and the gate (from the surface tension of IPA), and the gate will adhere to the gate during the spin-drying process, causing the gate to collapse during the drying process. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the problem that gate collapse occurs during the spin-drying process after the wafer is treated with a conventional cleaning solution, and a method for preparing a fluorinated silane wafer surface treatment solution is provided. After the wafer is treated with the surface treatment solution prepared by the preparation method of the present invention, the IPA contact angle is significantly increased, and no adhesion occurs between gates during the drying process, thereby avoiding the occurrence of gate collapse.

[0005] The present invention mainly solves the above technical problems through the following technical solutions.

[0006] The present invention provides a method for preparing a wafer surface treatment liquid, which comprises the following steps: mixing raw materials of the wafer surface treatment liquid to obtain the wafer surface treatment liquid;

[0007] The raw materials of the wafer surface treatment liquid include the following components in mass fraction: 0.005%-1% fluorine-containing silane, 0.1%-20% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance;

[0008] The silane coupling agent is Among them, R 1 , R 2 and R 3 are independently H, alkyl, alkoxy, -OH, -NH2, -COOH or -NHC(O)NHR 4 ; said R 1 , R 2 and R 3 At least one is an alkoxy group;

[0009] The R 4 is hydrogen or C1-C6 alkyl;

[0010] The organic solvent is selected from one or more of isopropyl alcohol (IPA), propylene glycol methyl ether acetate (PGMEA), DMF, n-hexane, cyclohexanone, tetrahydrofuran, dichloromethane, acetone and xylene.

[0011] In some embodiments, in the wafer surface treatment solution, the R 4 is hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl. Preferably, the R 4 It is hydrogen or methyl.

[0012] In some embodiments, in the wafer surface treatment liquid, the fluorine-containing silane is selected from one or more of perfluorooctyltrimethoxysilane, perfluorodecyltrimethoxysilane, perfluorodecyltriethoxysilane, fluoropropylmethylcyclotrisiloxane, (3,3,3-trifluoropropyl)trimethoxysilane, (3,3,3-trifluoropropyl)triethoxysilane, (3,3,3-trifluoropropyl)methyldimethoxysilane and (3,3,3-trifluoropropyl)methyldichlorosilane. Preferably, the fluorine-containing silane is selected from one or more of perfluorooctyltrimethoxysilane, perfluorodecyltriethoxysilane and (3,3,3-trifluoropropyl)trimethoxysilane.

[0013] In some embodiments, in the wafer surface treatment solution, the mass fraction of the fluorine-containing silane is 0.01%-0.08%, preferably, the mass fraction of the fluorine-containing silane is 0.01%-0.05%.

[0014] In some embodiments, in the wafer surface treatment solution, the R 1 , R 2 and R 3 are independently C1-C6 alkoxy, -NH2 or -COOH, said R 1 , R 2 and R 3At least one is an alkoxy group; preferably, the C1-C6 alkoxy group is independently methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy or tert-butoxy, such as methoxy.

[0015] In some embodiments, in the wafer surface treatment liquid, the mass fraction of the silane coupling agent is 5%-20%, preferably, the mass fraction of the silane coupling agent is 5%-15%, and more preferably, the mass fraction of the silane coupling agent is 10%.

[0016] In some embodiments, in the wafer surface treatment solution, the silane coupling agent is

[0017] In some embodiments, in the wafer surface treatment solution, the organic solvent is isopropyl alcohol and / or propylene glycol methyl ether acetate.

[0018] In some embodiments, in the wafer surface treatment solution, when the organic solvent is a mixed solution of isopropyl alcohol and propylene glycol methyl ether acetate, the mass ratio of the isopropyl alcohol to the propylene glycol methyl ether acetate is 1:(1-2).

[0019] In some embodiments, the pH of the wafer surface treatment liquid is 7-12.

[0020] In some embodiments, the wafer is a high aspect ratio wafer.

[0021] In some embodiments, the ratio of the depth to width of the wafer is greater than or equal to 10, preferably 10-100, more preferably 10-50, and further preferably 10-15.

[0022] In some schemes, in the wafer surface treatment liquid, the raw materials of the wafer surface treatment liquid include the following components by mass fraction: 0.01%-0.05% fluorine-containing silane, 10% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance;

[0023] The fluorine-containing silane is selected from one or more of perfluorooctyltrimethoxysilane, perfluorodecyltriethoxysilane and (3,3,3-trifluoropropyl)trimethoxysilane;

[0024] The silane coupling agent is

[0025] The organic solvent is isopropyl alcohol and / or propylene glycol methyl ether acetate.

[0026] In some embodiments, in the wafer surface treatment solution, the raw materials of the wafer surface treatment solution include any one of the following components in mass fractions:

[0027] Solution 1: 0.01% perfluorooctyltrimethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance;

[0028] Solution 2: 0.01% perfluorooctyltrimethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;

[0029] Solution 3: 0.05% perfluorooctyltrimethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance;

[0030] Solution 4: 0.05% perfluorooctyltrimethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;

[0031] Solution 5: 0.01% perfluorodecyltriethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance;

[0032] Scheme 6: 0.01% perfluorodecyltriethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;

[0033] Solution 7: 0.05% perfluorodecyltriethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance;

[0034] Solution 8: 0.05% perfluorodecyltriethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;

[0035] Scheme 9: 0.01% (3,3,3-trifluoropropyl)trimethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance;

[0036] Scheme 10: 0.01% (3,3,3-trifluoropropyl)trimethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;

[0037] Scheme 11: 0.05% (3,3,3-trifluoropropyl)trimethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance;

[0038] Scheme 12: 0.05% (3,3,3-trifluoropropyl)trimethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;

[0039] Preferably, the raw materials of the wafer surface treatment liquid are composed of any of the above schemes.

[0040] In some embodiments, the raw materials of the wafer surface treatment solution are mixed at 10°C to 40°C, preferably 20°C to 30°C.

[0041] In some embodiments, the raw materials of the wafer surface treatment solution are mixed and stirred for 0.5-3 hours, preferably 1 hour.

[0042] The term "high aspect ratio" of the present invention; in the semiconductor industry, a structure having a ratio of depth to width greater than or equal to 10 is generally defined as having a high aspect ratio.

[0043] "Room temperature" refers to 20°C to 30°C.

[0044] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0045] The reagents and raw materials used in the present invention are commercially available.

[0046] The positive improvement effect of the present invention is that after the wafer is treated with the fluorine-containing silane wafer surface treatment liquid prepared by the preparation method of the present invention, the IPA contact angle is significantly increased, the surface changes from hydrophilic to hydrophobic, and no adhesion occurs between the gates during the drying process, thereby avoiding the occurrence of gate collapse. DETAILED DESCRIPTION

[0047] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0048] Example 1

[0049] The surface treatment liquid was prepared according to the ingredients and proportions of each example in Table 1, and mixed evenly, specifically stirred at room temperature for 1 hour (without any order of addition).

[0050] Table 1

[0051]

[0052]

[0053] Note: “ / ” means does not exist.

[0054] This test uses TEOS (tetraethoxysilane) and SiN (silicon nitride) for testing. The test method is:

[0055] 1. Cut the wafer with aspect ratio of 10 into 30*30mm test pieces;

[0056] 2. Soak the test piece in IPA cleaning solution for 1 minute; take it out;

[0057] 3. Immerse the test pieces in the surface treatment solutions described in Table 1 for 1 minute, take them out and blow dry them with nitrogen;

[0058] 4. The contact angle test was performed using a contact angle tester (Attension Theta Lite), and the test solution was IPA. The surface roughness was tested at the same time, and the surface of the test piece was observed by electron microscopy. The results are shown in Table 2 below.

[0059] Table 2

[0060]

[0061]

[0062] It can be seen from the test results that after being immersed in the surface treatment liquid prepared by the preparation method of the present application, the IPA contact angle is significantly increased, and no adhesion will occur between the gates during the drying process, thereby avoiding the occurrence of gate collapse.

Claims

1. A method for preparing a wafer surface treatment solution, characterized in that: The method comprises the following steps: mixing the raw materials of the wafer surface treatment liquid to obtain the wafer surface treatment liquid; The raw materials of the wafer surface treatment liquid include the following components in mass fraction: 0.005%-1% fluorine-containing silane, 0.1%-20% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance; The silane coupling agent is Among them, R 1 , R 2 and R 3 are independently H, alkyl, alkoxy, -OH, -NH2, -COOH or -NHC(O)NHR 4 ; said R 1 , R 2 and R 3 At least one is an alkoxy group; R 4 is hydrogen or C1-C6 alkyl; The organic solvent is selected from one or more of isopropyl alcohol, propylene glycol methyl ether acetate, N,N-dimethylformamide, n-hexane, cyclohexanone, tetrahydrofuran, dichloromethane, acetone and xylene.

2. The method for preparing a wafer surface treatment solution according to claim 1, wherein: It meets one or more of the following conditions: (1) The fluorine-containing silane is selected from one or more of perfluorooctyltrimethoxysilane, perfluorodecyltrimethoxysilane, perfluorodecyltriethoxysilane, fluoropropylmethylcyclotrisiloxane, (3,3,3-trifluoropropyl)trimethoxysilane, (3,3,3-trifluoropropyl)triethoxysilane, (3,3,3-trifluoropropyl)methyldimethoxysilane and (3,3,3-trifluoropropyl)methyldichlorosilane; (2) The mass fraction of the fluorine-containing silane is 0.01%-0.08%; (3) R 4 is hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl; and (4) The wafer is a high aspect ratio wafer.

3. The method for preparing a wafer surface treatment solution according to claim 2, wherein: The wafer surface treatment solution meets one or more of the following conditions: (1) The fluorine-containing silane is selected from one or more of perfluorooctyltrimethoxysilane, perfluorodecyltriethoxysilane and (3,3,3-trifluoropropyl)trimethoxysilane; (2) The mass fraction of the fluorine-containing silane is 0.01%-0.05%; and (3) R 4 It is hydrogen or methyl.

4. The method for preparing a wafer surface treatment solution according to claim 3, characterized in that: The wafer surface treatment solution meets one or more of the following conditions: (1) R 1 , R 2 and R 3 are independently C1-C6 alkoxy, -NH2 or -COOH, said R 1 , R 2 and R 3 At least one is an alkoxy group; (2) The mass fraction of the silane coupling agent is 5%-20%; (3) the organic solvent is isopropyl alcohol and / or propylene glycol methyl ether acetate; and (4) The pH value of the wafer surface treatment solution is 7-12.

5. The method for preparing a wafer surface treatment solution according to claim 4, characterized in that: The wafer surface treatment solution meets one or more of the following conditions: (1) R 1 , R 2 and R 3 In the above, C1-C6 alkoxy is independently methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy or tert-butoxy, for example methoxy; (2) The mass fraction of the silane coupling agent is 5%-15%; and (3) When the organic solvent is a mixed solution of isopropyl alcohol and propylene glycol methyl ether acetate, the mass ratio of the isopropyl alcohol to the propylene glycol methyl ether acetate is 1:(1-2).

6. The method for preparing a wafer surface treatment solution according to claim 5, characterized in that: The wafer surface treatment solution meets one or both of the following conditions: (1) The mass fraction of the silane coupling agent is 10%; and (2) The silane coupling agent is 7. The method for preparing a wafer surface treatment solution according to claim 1, characterized in that: The preparation method meets one or both of the following conditions: (1) The raw materials of the wafer surface treatment solution are mixed at 10° C. to 40° C., preferably 20° C. to 30° C.; and (2) The raw materials of the wafer surface treatment solution are mixed and stirred for 0.5-3 hours, preferably 1 hour.

8. The method for preparing a wafer surface treatment solution according to claim 1, wherein: The raw materials of the wafer surface treatment liquid include the following components in mass fraction: 0.01%-0.05% fluorine-containing silane, 10% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance; The fluorine-containing silane is selected from one or more of perfluorooctyltrimethoxysilane, perfluorodecyltriethoxysilane and (3,3,3-trifluoropropyl)trimethoxysilane; The silane coupling agent is The organic solvent is isopropyl alcohol and / or propylene glycol methyl ether acetate.

9. The method for preparing a wafer surface treatment solution according to any one of claims 1 to 8, characterized in that: The raw materials of the wafer surface treatment solution include any of the following components in mass fractions: Solution 1: 0.01% perfluorooctyltrimethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance; Solution 2: 0.01% perfluorooctyltrimethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Solution 3: 0.05% perfluorooctyltrimethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance; Solution 4: 0.05% perfluorooctyltrimethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Solution 5: 0.01% perfluorodecyltriethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance; Solution 6: 0.01% perfluorodecyltriethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Solution 7: 0.05% perfluorodecyltriethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance; Solution 8: 0.05% perfluorodecyltriethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Scheme 9: 0.01% (3,3,3-trifluoropropyl)trimethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance; Scheme 10: 0.01% (3,3,3-trifluoropropyl)trimethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Scheme 11: 0.05% (3,3,3-trifluoropropyl)trimethoxysilane, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance; Scheme 12: 0.05% (3,3,3-trifluoropropyl)trimethoxysilane, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance.

10. The method for preparing a wafer surface treatment solution according to claim 9, characterized in that: The raw materials of the wafer surface treatment liquid are composed of any one of the schemes in claim 9.