LF furnace refining desulfurization method for tire cord steel
By optimizing the LF furnace refining desulfurization process and using high-efficiency desulfurizers, the problems of high energy consumption and low sulfur removal efficiency in traditional methods have been solved, and efficient desulfurization and environmental protection of cord steel have been achieved.
Patent Information
- Application Number
- CN202410689446.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The traditional LF furnace refining desulfurization method has high energy consumption, which leads to increased production costs, serious environmental pollution, low sulfur removal efficiency, and requires frequent adjustments to maintain stable sulfur removal efficiency, which increases manpower and energy consumption.
By optimizing the desulfurization process and efficient use of desulfurization agents, we adopt furnace preparation, uniform placement of cord steel, preheating operation, stirring system and online monitoring system to ensure that the desulfurization agent and molten steel are fully mixed and reacted, adjust operating parameters in real time, and take samples regularly. Analyze to control the sulfur content, prepare desulfurizers of iron oxide powder, calcium oxide and coke powder, and perform sintering treatment to improve high temperature resistance.
It significantly reduces production costs and energy consumption, reduces carbon dioxide emissions, improves sulfur removal efficiency and molten steel quality, reduces labor costs and equipment operating costs, and achieves a more efficient production process.
Smart Images

Figure CN118726699A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cord steel desulfurization, in particular to an LF furnace refining and desulfurization method for cord steel. Background Art
[0002] Cord steel is a widely used building material, commonly used in the production of curtain tracks, blinds, and curtains. It is usually made of metal materials and has high strength and durability. The characteristics of cord steel include corrosion resistance, oxidation resistance, and durability. Therefore, it is widely used in home decoration and construction.
[0003] In the steel production, refining and desulfurization of cord steel is a crucial process link, among which the LF furnace refining and desulfurization method of cord steel is a commonly used method. In the traditional LF furnace refining and desulfurization method, the energy consumption of LF furnace operation is relatively high, which increases production costs, and high energy consumption will increase carbon dioxide and greenhouse gas emissions, aggravate the impact on the environment, and aggravate the problem of global climate change. In addition, high energy consumption will cause resource consumption and have a negative impact on the environment. At the same time, the traditional LF furnace refining and desulfurization method has low sulfur removal efficiency in the cord steel refining process, resulting in additional process adjustments, increased energy consumption, and further increased production costs. Frequent adjustments are required during the production process to maintain a stable sulfur removal efficiency, resulting in increased labor costs and energy consumption.
[0004] Therefore, those skilled in the art provide a method for refining and desulfurizing cord steel in an LF furnace to solve the problems raised in the above background technology. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a LF furnace refining and desulfurization method for cord steel, which solves the problem that the energy consumption of LF furnace operation in the traditional LF furnace refining and desulfurization method is high, which increases production costs. The high energy consumption will increase the emission of carbon dioxide and greenhouse gases, aggravate the impact on the environment, and aggravate the problem of global climate change. In addition, the high energy consumption will cause resource consumption and have a negative impact on the environment.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions: A LF furnace refining and desulfurization method for cord steel, comprising the following steps:
[0007] Step 1: Furnace preparation: Check the integrity of LF furnace equipment, furnace lining and bricks;
[0008] Step 2: Placement of cord steel: The operator evenly loads the cord steel into the LF furnace by operating mechanical tools;
[0009] Step 3: Preheating operation: Start the LF furnace, raise the furnace temperature to a suitable operating temperature, and then carry out refining treatment;
[0010] Step 4: Desulfurizer: Prepare an appropriate amount of desulfurizer and ensure that the quality and ratio meet the requirements;
[0011] Step 5: Start the stirring system: Start the stirring system of the LF furnace to promote the full mixing of the desulfurizer;
[0012] Step 6. Online monitoring system inspection: monitor the desulfurization effect in real time and adjust the operating parameters in time to ensure accurate monitoring of the sulfur content in the molten steel;
[0013] Step 7: Desulfurization treatment: adding a desulfurizer to carry out a desulfurization reaction;
[0014] Step 8: Adjust the desulfurization agent delivery speed: According to the real-time monitoring data and the desulfurization reaction situation, adjust the desulfurization agent delivery speed to ensure that the desulfurization agent and the molten steel are fully mixed and reacted;
[0015] Step 9. Regular sampling and analysis: Through regular sampling and analysis, monitor the desulfurization effect and adjust the operating parameters in time to ensure that the quality of molten steel meets the standard requirements.
[0016] Step 1: Pre-furnace preparation can avoid the damage of furnace lining and bricks leading to the penetration of slag and the infiltration of molten steel, so as to ensure the stability of the furnace environment; Step 2: By evenly adding cord steel, the temperature in the furnace can be evenly distributed, which is beneficial to the subsequent refining treatment; Step 3: Preheating operation can increase the temperature in the furnace, promote the reaction rate of desulfurizer and molten steel, and improve the desulfurization effect; Step 4: Desulfurizer is a chemical substance used to adsorb and reduce sulfur in molten steel. By adding desulfurizer, the sulfur content in molten steel can be reduced; Step 5: The stirring system can fully mix the desulfurizer and molten steel, increase the contact area, accelerate the desulfurization reaction rate, and improve the desulfurization effect; Step 6: Online monitoring system The system can monitor the sulfur content in molten steel in real time, help operators understand the desulfurization effect, and adjust the desulfurizer feeding speed and other operating parameters in time to meet the desulfurization requirements; Step 7, the desulfurizer reacts with the sulfur in the molten steel to form volatile compounds, and removes sulfur in the molten steel to achieve the purpose of desulfurization; Step 8, by adjusting the feeding speed, the amount of desulfurizer fed can be controlled to make it fully contact with the molten steel and improve the desulfurization effect; Step 9, regular sampling and analysis can be performed on the molten steel after desulfurization to detect the sulfur content, and the operating parameters can be adjusted according to the analysis results to ensure that the molten steel quality meets the requirements, reduce the sulfur content in the cord steel, and improve the quality and performance of the steel.
[0017] Preferably, in step 2, the mechanical tool includes a crane and a forklift, and the operator operates the crane and the forklift to slowly and steadily load the cord steel into the interior of the LF furnace.
[0018] Preferably, in step three, the suitable temperature range for refining treatment is 1200° C. to 1300° C., and the time range for refining treatment is 1 h to 2 h.
[0019] Preferably, in step 4, the preparation process of the desulfurizing agent is as follows:
[0020] S1. Raw material preparation: prepare iron oxide powder, calcium oxide (quicklime), and coke powder;
[0021] S2. Mixing ratio: Evenly mix the iron oxide powder, calcium oxide and coke powder in a ratio of 3:2:1 of iron oxide powder:calcium oxide:coke powder;
[0022] S3, mixing: fully mix the iron oxide powder, calcium oxide and coke powder in the ingredients to ensure that the raw materials are evenly distributed;
[0023] S4, processing: pressing the mixed raw materials into granular or block-shaped desulfurizer;
[0024] S5, sintering: putting the processed desulfurizer into the furnace for sintering;
[0025] S6. Cooling and packaging: After sintering, the desulfurizer is cooled to room temperature and then packaged for easy storage and transportation.
[0026] S1. Raw material preparation: Iron oxide powder is mainly used to adsorb and reduce sulfur in molten steel, calcium oxide is used to provide an alkaline environment, and coke powder is used as a reducing agent to promote the desulfurization reaction; S2. Ratio: According to the ratio of iron oxide powder: calcium oxide: coke powder of 3:2:1, the ratio is determined according to the chemical properties of the desulfurizer and the requirements of the desulfurization reaction; S3. Mixing: The mixing process can be completed by mechanical stirring to ensure that the components are evenly dispersed to avoid uneven mixing leading to unstable desulfurization effect; S4. During the processing, a press can be used to press the mixed raw materials into the required shape and size for subsequent use and delivery; S5. Sintering refers to the heat treatment of the desulfurizer at high temperature to form a solid structure and improve its high temperature resistance and corrosion resistance. During the sintering process, the chemical composition of the raw materials will change to form a compound with a better desulfurization effect; S6. Cooling and packaging. The cooling process can be achieved by natural cooling or other cooling equipment. Appropriate packaging materials can be used for packaging to protect the desulfurizer from moisture, pollution and damage to ensure that its quality and performance are not affected.
[0027] Preferably, in the step 4, the reaction equation in the preparation process of the desulfurizing agent is:
[0028] The chemical reaction equation of iron oxide and coke is:
[0029] (Fe2O3+3C→2Fe+3CO),
[0030] Among them, Fe2O3 is iron oxide, C is coke, Fe is iron, and CO is carbon monoxide;
[0031] The decomposition reaction equation of calcium oxide is:
[0032] (CaO→Ca 2+ +O 2- ),
[0033] Among them, CaO is calcium oxide, Ca 2+ is calcium metal, O 2- It is oxygen;
[0034] The reaction equation of calcium oxide and iron oxide is:
[0035] (CaO+Fe2O3→CaO·Fe2O3),
[0036] Among them, CaO is calcium oxide, Fe2O3 is iron oxide, and CaO·Fe2O3 is calcium iron ore.
[0037] The reduction reaction between iron oxide and coke generates ferrous oxide (Fe3O4) and carbon dioxide (CO2). Coke participates in the reaction as a reducing agent, reducing iron oxide to ferrous oxide; the decomposition reaction of calcium oxide, by heating calcium oxide (quicklime), decomposes it into calcium oxide and carbon dioxide; the reaction between calcium oxide and ferrous oxide generates calcium ferrite (CaFeO3) and ferrous oxide (FeO).
[0038] Preferably, in step 4, the iron oxide powder, calcium oxide and coke powder are mixed by a mechanical agitator, the stirring speed range of the mechanical agitator is 100 r / min to 500 r / min, and the stirring time range is 10 min to 30 min.
[0039] Mixing with a mechanical agitator can improve the uniformity of the raw materials, ensure that the iron oxide powder, calcium oxide and coke powder are fully contacted and mixed, and improve the reaction rate and effect. The stirring speed and time should be adjusted according to the actual situation to ensure the thoroughness of the mixing and the sufficiency of the reaction. During the mixing process, the stirring speed should be appropriately selected. Too low a stirring speed will lead to uneven mixing, while too high a stirring speed will cause particle breakage and excessive mixing. The stirring time should be determined according to the properties of the raw materials and the mixing effect to ensure that the raw materials are fully mixed. Mixing with a mechanical agitator can improve the preparation quality of the desulfurizer, ensure its uniform composition, and improve the desulfurization effect and stability of the desulfurizer.
[0040] Preferably, in step five, the stirring system is composed of a stirrer, a driving device and a control system, the stirring speed range of the stirrer is 50 r / min to 150 r / min, and the stirring time range of the stirrer is 10 min to 30 min.
[0041] The agitator is a device used to stir the molten steel in the LF furnace. Through stirring, the desulfurizer and molten steel can be fully mixed, the contact area can be increased, the desulfurization reaction rate can be accelerated, and the desulfurization effect can be improved. The selection of stirring speed and time should be determined according to the actual situation and desulfurization requirements to ensure the adequacy and uniformity of stirring.
[0042] Preferably, in step six, the monitoring system comprises a temperature sensor, an oxygen content sensor, an electromagnetic stirring system, a chemical composition analyzer, a pressure sensor and a control system; the temperature sensor is used to monitor the temperature changes in the furnace, including the molten steel temperature and the furnace body temperature; the oxygen content sensor is used to monitor the oxygen content in the furnace, help control the oxygen supply, and affect the redox reaction in the furnace; the electromagnetic stirring system stirs the molten steel through an electromagnetic force field to promote the uniform distribution of heat and chemical substances; the chemical composition analyzer is used to monitor the chemical composition of the molten steel in real time; the pressure sensor is used to monitor the pressure changes in the furnace, and help control the atmosphere in the furnace and the reaction in the furnace; the control system is used to integrate the sensor data, monitor the parameters in the furnace in real time, and control and adjust according to the set control strategy.
[0043] Temperature sensor: by real-time monitoring of temperature, the changes in the thermal state in the furnace can be understood, providing a basis for the control and regulation of the desulfurization process; oxygen content sensor: by monitoring the oxygen content, the oxygen supply can be adjusted to control the redox environment in the furnace, which plays an important role in the desulfurization process; the electromagnetic stirring system can improve the temperature distribution and composition uniformity of the molten steel and improve the desulfurization effect; chemical composition analyzer: through the chemical composition analyzer, the quality and composition changes of the molten steel can be understood in time, providing accurate data for the control and regulation of the desulfurization process; pressure sensor: by monitoring the pressure changes, the supply and discharge of gas can be adjusted to maintain a suitable furnace atmosphere and ensure the normal progress of the desulfurization process; the control system can automatically adjust the stirring speed, oxygen supply and other operating parameters according to the real-time monitoring data and preset parameters to achieve the best desulfurization effect.
[0044] Preferably, in step seven, the reaction equation for desulfurization treatment is:
[0045] [CaO (固体) +S (液态) →CaS (固体) ],
[0046] In this reaction, calcium oxide (solid) reacts with sulfur (liquid) in molten steel to generate calcium sulfide (solid), thus achieving the desulfurization process.
[0047] Preferably, in step eight, the method for adjusting the desulfurization agent delivery rate is as follows:
[0048] A. Monitor the desulfurization effect: Before adjusting the feeding speed, monitor and evaluate the desulfurization effect by monitoring the sulfur content in the molten steel;
[0049] B. Adjust the delivery speed as needed: According to the real-time monitoring data and desulfurization effect, the delivery speed of the desulfurizer can be gradually adjusted;
[0050] C. Consider the temperature and stirring of the molten steel: When adjusting the feeding speed, the temperature of the molten steel and whether it is sufficiently stirred should be considered to ensure that the desulfurizer can fully react with the sulfur in the molten steel;
[0051] D. Regular inspection and adjustment: Regularly inspect the desulfurization equipment and delivery system to ensure that they operate normally and can deliver desulfurizer at the set speed.
[0052] The present invention provides a LF furnace refining and desulfurization method for cord steel, which has the following beneficial effects:
[0053] 1. The present invention can significantly reduce production costs by optimizing the desulfurization process and the efficient use of desulfurizers, reducing energy consumption and time consumption. At the same time, reducing the production cycle can reduce labor costs and equipment operating costs in the production process, achieve reductions in energy consumption and time consumption, and improve production efficiency. Reducing energy consumption helps reduce carbon dioxide emissions and other pollutants, which is beneficial to environmental protection and sustainable development.
[0054] 2. The present invention can improve the accuracy and stability of operations, reduce labor costs, and reduce operation complexity by introducing automation technology and intelligent monitoring systems. Automation technology and intelligent monitoring systems can realize automation and intelligent management of the production process, reduce human intervention, and improve production efficiency. The automation system can operate sustainably, reduce downtime in production, and improve production line utilization. The automation technology and intelligent monitoring system can monitor parameters and data in the production process in real time, adjust production parameters in time, and ensure stable product quality. The intelligent monitoring system can detect problems in the production process in time, reduce product defect rates, and improve product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 is a flow chart of the method of the present invention;
[0056] Figure 2 The present invention is a flow chart for preparing the desulfurizing agent. DETAILED DESCRIPTION
[0057] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0058] Embodiment 1:
[0059] Please see attached Figure 1 , Attachment Figure 2 The embodiment of the present invention provides a LF furnace refining and desulfurization method for cord steel, comprising the following steps:
[0060] Step 1: Furnace preparation
[0061] Before operating the LF furnace, check the integrity of the LF furnace equipment, furnace lining and bricks to ensure safe operation;
[0062] Step 2: Placement of cord steel
[0063] Operators use cranes and forklifts to slowly and steadily load the cord steel into the LF furnace;
[0064] Step 3: Preheating operation
[0065] Start the LF furnace, raise the furnace temperature to 1200℃, and then carry out refining treatment;
[0066] Step 4: Preparation of desulfurizer
[0067] Prepare iron oxide powder, calcium oxide (quicklime), and coke powder, and mix them in a ratio of 3:2:1 to prepare a desulfurizer;
[0068] Step 5: Start the mixing system
[0069] Start the stirring system of the LF furnace at a stirring speed of 100r / min and stir for 10 minutes to ensure that the desulfurizer is fully mixed;
[0070] Step 6: Online monitoring system inspection
[0071] Monitor the desulfurization effect in real time and adjust the operating parameters to ensure accurate monitoring of the sulfur content in molten steel;
[0072] Step 7: Desulfurization
[0073] Adding desulfurizing agent to carry out desulfurization reaction;
[0074] Step 8: Adjust the desulfurization agent delivery speed
[0075] According to the real-time monitoring data and desulfurization reaction conditions, gradually adjust the feeding speed to ensure sufficient mixing reaction and improve the desulfurization effect;
[0076] Step 9: Regular sampling and analysis
[0077] Take samples regularly for analysis, monitor the desulfurization effect, and adjust the operating parameters to ensure that the molten steel quality meets the standard requirements;
[0078] Summary: Through careful furnace preparation, precise desulfurizer preparation and adjustment of the delivery speed, efficient refining and desulfurization of cord steel can be achieved to ensure that the quality of molten steel meets the standards.
[0079] Embodiment 2:
[0080] Please see attached Figure 1 , Attachment Figure 2 The embodiment of the present invention provides a LF furnace refining and desulfurization method for cord steel, comprising the following steps:
[0081] Step 1: Furnace preparation
[0082] Check the integrity of LF furnace equipment, lining and bricks to ensure safe operation;
[0083] Step 2: Placement of cord steel
[0084] Load the cord steel evenly into the LF furnace;
[0085] Step 3: Preheating operation
[0086] Start the LF furnace, raise the furnace temperature to 1300℃, and then carry out refining treatment;
[0087] Step 4: Preparation of desulfurizer
[0088] Prepare the desulfurizer in a ratio of 3:2:1, stir at a speed of 500r / min, stir for 30min to ensure sufficient mixing;
[0089] Step 5: Start the mixing system
[0090] Start the stirring system of the LF furnace at a stirring speed of 150r / min for 30 minutes to improve the desulfurization effect;
[0091] Step 6: Online monitoring system inspection
[0092] Monitor the desulfurization effect in real time and adjust the operating parameters in time to ensure accurate monitoring of the sulfur content in molten steel;
[0093] Step 7: Desulfurization
[0094] Adding desulfurizing agent to carry out desulfurization reaction;
[0095] Step 8: Adjust the desulfurization agent delivery speed
[0096] Adjust the feeding speed according to the real-time monitoring data and desulfurization reaction conditions to ensure that the desulfurizer and molten steel are fully mixed and reacted to improve the desulfurization effect;
[0097] Step 9: Regular sampling and analysis
[0098] Through regular sampling and analysis, the desulfurization effect is monitored and the operating parameters are adjusted in time to ensure that the molten steel quality meets the standard requirements;
[0099] Summary: Through high-temperature and high-speed operation and fine control, the cord steel can be quickly and efficiently refined and desulfurized, thus improving production efficiency and desulfurization effect.
[0100] Embodiment three:
[0101] Please see attached Figure 1 , Attachment Figure 2 The embodiment of the present invention provides a LF furnace refining and desulfurization method for cord steel, comprising the following steps:
[0102] Step 1: Furnace preparation
[0103] Before operating the LF furnace, conduct strict equipment inspection to ensure safety;
[0104] Step 2: Placement of cord steel
[0105] Use the automatic conveying system to quickly load the cord steel into the LF furnace;
[0106] Step 3: Preheating operation
[0107] Raise the LF furnace temperature to 1250°C and perform refining treatment within a suitable temperature range;
[0108] Step 4: Preparation of desulfurizer
[0109] preparing iron oxide powder, calcium oxide and coke powder, mixing them in proportion, and preparing them by an automated machine;
[0110] Step 5: Start the mixing system
[0111] The stirring system starts automatically and stirs according to the preset parameters to ensure that the desulfurizer is fully mixed;
[0112] Step 6: Online monitoring system inspection
[0113] Real-time monitoring of desulfurization effect, automatic adjustment of operating parameters, and accurate monitoring of sulfur content;
[0114] Step 7: Desulfurization
[0115] Automatically add desulfurizer to achieve desulfurization reaction;
[0116] Step 8: Adjust the desulfurization agent delivery speed
[0117] Automatically adjust the delivery speed according to monitoring data and reaction conditions to optimize the desulfurization effect;
[0118] Step 9: Regular sampling and analysis
[0119] The system takes samples regularly for analysis, automatically monitors the desulfurization effect, and automatically adjusts the operating parameters;
[0120] Summary: Through the application of automated equipment and systems, efficient refining and desulfurization of cord steel can be achieved, and production efficiency and operation accuracy can be improved.
[0121] Embodiment 4:
[0122] Please see attached Figure 1 , Attachment Figure 2 The embodiment of the present invention provides a LF furnace refining and desulfurization method for cord steel, comprising the following steps:
[0123] Step 1: Furnace preparation
[0124] Conduct a comprehensive LF furnace equipment inspection to ensure safe operation;
[0125] Step 2: Placement of cord steel
[0126] Manually load the cord steel into the LF furnace one by one;
[0127] Step 3: Preheating operation
[0128] Control the LF furnace temperature at 1300°C for refining treatment;
[0129] Step 4: Preparation of desulfurizer
[0130] The desulfurizer was prepared by manually mixing iron oxide powder, calcium oxide and coke powder in a ratio of 3:2:1;
[0131] Step 5: Start the mixing system
[0132] Manually start the stirring system of the LF furnace and manually adjust the stirring speed and time;
[0133] Step 6: Online monitoring system inspection
[0134] Manually monitor the desulfurization effect and manually adjust the operating parameters;
[0135] Step 7: Desulfurization
[0136] Manually add desulfurizer to carry out desulfurization reaction;
[0137] Step 8: Adjust the desulfurization agent delivery speed
[0138] Manually adjust the delivery speed based on manual monitoring data and response conditions;
[0139] Step 9: Regular sampling and analysis
[0140] Manual sampling and analysis, monitoring of desulfurization effect, and manual adjustment of operating parameters;
[0141] Summary: The desulfurization of cord steel is achieved by traditional manual operation. The operation process is cumbersome, but it can ensure that the quality of molten steel meets the standard requirements.
[0142] Embodiment five:
[0143] Please see attached Figure 1 , Attachment Figure 2 The embodiment of the present invention provides a LF furnace refining and desulfurization method for cord steel, comprising the following steps:
[0144] Step 1: Intelligent equipment inspection
[0145] Use intelligent technology to automatically detect LF furnace equipment to ensure equipment integrity and operational safety;
[0146] Step 2: Automated cord steel delivery
[0147] Through the automated conveying system, the cord steel is quickly and accurately loaded into the LF furnace;
[0148] Step 3: Intelligent temperature control
[0149] Using advanced intelligent control system, the temperature of LF furnace is precisely controlled within the range of 1200℃ to 1300℃ to achieve refining treatment;
[0150] Step 4: Preparation of intelligent desulfurizer
[0151] An automated production line is used to achieve a fully automated process of mixing iron oxide powder, calcium oxide and coke powder in proportion to prepare desulfurizer;
[0152] Step 5: Intelligent mixing system
[0153] The intelligent stirring system automatically adjusts the stirring speed and time according to the real-time monitoring data to ensure that the desulfurizer is fully mixed;
[0154] Step 6: Intelligent online monitoring system
[0155] Use high-precision sensors and intelligent monitoring systems to monitor the desulfurization effect in real time and automatically adjust operating parameters to ensure that the molten steel quality meets standard requirements;
[0156] Step 7: Intelligent desulfurization treatment
[0157] Automatically add desulfurizer through intelligent control system to achieve efficient desulfurization reaction;
[0158] Step 8: Intelligently adjust the desulfurization agent delivery speed
[0159] According to intelligent monitoring data and reaction conditions, the desulfurization agent delivery speed is automatically adjusted to optimize the desulfurization effect;
[0160] Step 9: Intelligent timed sampling and analysis
[0161] Utilize intelligent sampling and analysis system to automatically monitor desulfurization effect and realize intelligent control and adjustment throughout the process;
[0162] Summary: Through the application of intelligent equipment and systems, efficient refining and desulfurization of cord steel can be achieved, and production efficiency, operation accuracy and quality control level can be improved, which is a modern and intelligent production method.
[0163] Summary:
[0164] Embodiment 1: The LF furnace treatment of cord steel is carried out by traditional manual operation, the operation process is relatively complicated, relies on manual monitoring and adjustment, and the production efficiency is low;
[0165] Embodiment 2: Introducing an automated conveying system and an online monitoring system to improve production efficiency and operating accuracy, but manual operation and adjustment are still required;
[0166] Embodiment 3: Through the application of automated equipment and systems, efficient refining and desulfurization of cord steel is achieved, and production efficiency and operation accuracy are improved;
[0167] Embodiment 4: The traditional manual operation method is adopted. The operation process is cumbersome, but it can ensure that the quality of molten steel meets the standard requirements;
[0168] Embodiment 5: Using intelligent equipment and systems to achieve efficient refining and desulfurization of cord steel, and improve production efficiency, operation accuracy and quality control level.
[0169] Experimental data table and specific parameters:
[0170]
[0171]
[0172] Comparative experimental design:
[0173] Comparative experiment 1: The influence of stirring speed on the refining effect of cord steel
[0174] Experimental group A: stirring speed 100r / min
[0175] Experimental group B: stirring speed 150r / min
[0176] Experimental group C: stirring speed 200r / min
[0177] Comparative experiment 2: Comparison of desulfurization effects at different temperatures
[0178] Experimental group X: temperature 1200℃, desulfurization agent feeding rate 10kg / min
[0179] Experimental group Y: temperature 1250℃, desulfurization agent feeding rate 10kg / min
[0180] Experimental group Z: temperature 1300℃, desulfurizer feeding rate 10kg / min
[0181] Comparative experiment 3: Comparative refining effect under manual operation and automatic operation Experimental group I: manual operation mode, temperature 1250℃, stirring speed 120r / min Experimental group II: automatic operation mode, temperature 1250℃, stirring speed 120r / min Experimental data table of comparative experiment 1:
[0182] Experimental Group Stirring speed Temperature(℃) Desulfurization agent feeding speed (kg / min) Sulfur content (%) A 100r / min 1250 10 0.05 B 150r / min 1250 10 0.04 C 200r / min 1250 10 0.03
[0183] Comparative experiment 2 experimental data table:
[0184] Experimental Group Stirring speed Temperature(℃) Desulfurization agent feeding speed (kg / min) Sulfur content (%) X 120r / min 1200 10 0.06 Y 120r / min 1250 10 0.04 Z 200r / min 1300 10 0.03
[0185] Experimental data table of comparative experiment three:
[0186] Experimental Group Operation Mode Stirring speed temperature Desulfurization agent delivery speed Sulfur content Ⅰ Manual Operation 120r / min 1250℃ 10kg / min 0.05% Ⅱ Automatic operation 120r / min 1250℃ 10kg / min 0.03%
[0187] Experimental structure analysis and summary:
[0188] Comparative experiment 1: The influence of stirring speed on the refining effect of cord steel
[0189] Result analysis: With the increase of stirring speed, the sulfur content of cord steel gradually decreases, indicating that a higher stirring speed is beneficial to improving the refining effect.
[0190] Summary: In actual production, a higher stirring speed can be considered to improve the refining effect of cord steel.
[0191] Comparative experiment 2: Comparison of desulfurization effects at different temperatures
[0192] Result analysis: With the increase of temperature, the sulfur content of cord steel gradually decreases, indicating that higher temperature is conducive to improving the desulfurization effect.
[0193] Summary: When desulfurizing cord steel, a higher temperature can be considered to improve the desulfurization effect.
[0194] Comparative experiment 3: Comparison of refining effects under manual operation and automatic operation
[0195] Result analysis: The sulfur content of cord steel in the automatic operation mode is significantly lower than that in the manual operation mode, indicating that automatic operation can improve the refining effect.
[0196] Summary: The introduction of an automated operating system can improve production efficiency and operating accuracy, and help improve the quality of cord steel.
[0197] Comprehensive analysis:
[0198] From the above experiments, it can be seen that the stirring speed, temperature and operation mode have a significant impact on the refining effect of cord steel. Higher stirring speed and temperature are conducive to reducing the sulfur content of cord steel and improving the refining effect. The introduction of an automated operating system can improve production efficiency and operating accuracy, thereby improving the quality of cord steel. In actual production, the process parameters can be adjusted according to the experimental results and the production process can be optimized to achieve better cord steel refining effects and quality control levels.
[0199] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A LF furnace refining and desulfurization method for cord steel, It is characterized in that The following steps are involved: Step 1: Furnace preparation: Check the integrity of LF furnace equipment, furnace lining and bricks; Step 2: Placement of cord steel: The operator evenly loads the cord steel into the LF furnace by operating mechanical tools; Step 3: Preheating operation: Start the LF furnace, raise the furnace temperature to a suitable operating temperature, and then carry out refining treatment; Step 4: Desulfurizer: Prepare an appropriate amount of desulfurizer and ensure that the quality and ratio meet the requirements; Step 5: Start the stirring system: Start the stirring system of the LF furnace to promote the full mixing of the desulfurizer; Step 6. Online monitoring system inspection: monitor the desulfurization effect in real time and adjust the operating parameters in time to ensure accurate monitoring of the sulfur content in the molten steel; Step 7: Desulfurization treatment: adding a desulfurizer to carry out a desulfurization reaction; Step 8: Adjust the desulfurization agent delivery speed: According to the real-time monitoring data and the desulfurization reaction situation, adjust the desulfurization agent delivery speed to ensure that the desulfurization agent and the molten steel are fully mixed and reacted; Step 9. Regular sampling and analysis: Through regular sampling and analysis, monitor the desulfurization effect and adjust the operating parameters in time to ensure that the quality of molten steel meets the standard requirements.
2. The LF furnace refining and desulfurization method of cord steel according to claim 1, It is characterized in that In the step 2, the mechanical tools include a crane and a forklift, and the operator operates the crane and the forklift to slowly and steadily load the cord steel into the interior of the LF furnace.
3. The LF furnace refining and desulfurization method of a cord steel according to claim 1, It is characterized in that In the step three, the suitable temperature range for the refining treatment is 1200° C. to 1300° C., and the time range for the refining treatment is 1 h to 2 h.
4. The LF furnace refining and desulfurization method of a cord steel according to claim 1, It is characterized in that In the step 4, the preparation process of the desulfurizing agent is as follows: S1. Raw material preparation: prepare iron oxide powder, calcium oxide (quicklime), and coke powder; S2. Mixing ratio: Evenly mix the iron oxide powder, calcium oxide and coke powder in a ratio of 3:2:1 of iron oxide powder:calcium oxide:coke powder; S3, mixing: fully mix the iron oxide powder, calcium oxide and coke powder in the ingredients to ensure that the raw materials are evenly distributed; S4, processing: pressing the mixed raw materials into granular or block-shaped desulfurizer; S5, sintering: putting the processed desulfurizer into the furnace for sintering; S6. Cooling and packaging: After sintering, the desulfurizer is cooled to room temperature and then packaged for easy storage and transportation.
5. The LF furnace refining and desulfurization method of cord steel according to claim 1, It is characterized in that In the step 4, the reaction equation in the preparation process of the desulfurizing agent is: The chemical reaction equation of iron oxide and coke is: (Fe 2 O 3 +3C→2Fe+3CO), Among them, Fe 2 O 3 is iron oxide, C is coke, Fe is iron, and CO is carbon monoxide; The decomposition reaction equation of calcium oxide is: (CaO→Ca 2+ +O 2- ), Among them, CaO is calcium oxide, Ca 2+ is calcium metal, O 2- It is oxygen; The reaction equation of calcium oxide and iron oxide is: (CaO+Fe 2 O 3 →CaO·Fe 2 O 3 ), Among them, CaO is calcium oxide, Fe 2 O 3 It is iron oxide, CaO·Fe 2 O 3 It's calcium iron ore.
6. The LF furnace refining and desulfurization method of cord steel according to claim 1, It is characterized in that In the step 4, the iron oxide powder, calcium oxide and coke powder are mixed by a mechanical stirrer, the stirring speed range of the mechanical stirrer is 100r / min to 500r / min, and the stirring time range is 10min to 30min.
7. The LF furnace refining and desulfurization method for cord steel according to claim 1, It is characterized in that In the step 5, the stirring system is composed of a stirrer, a driving device and a control system. The stirring speed range of the stirrer is 50 r / min to 150 r / min, and the stirring time range of the stirrer is 10 min to 30 min.
8. The LF furnace refining and desulfurization method for cord steel according to claim 1, It is characterized in that In step six, the monitoring system comprises a temperature sensor, an oxygen content sensor, an electromagnetic stirring system, a chemical composition analyzer, a pressure sensor and a control system; the temperature sensor is used to monitor the temperature changes in the furnace, including the molten steel temperature and the furnace body temperature; the oxygen content sensor is used to monitor the oxygen content in the furnace, help control the oxygen supply, and affect the progress of the redox reaction in the furnace; the electromagnetic stirring system stirs the molten steel through an electromagnetic force field to promote the uniform distribution of heat and chemical substances; the chemical composition analyzer is used to monitor the chemical composition of the molten steel in real time; the pressure sensor is used to monitor the pressure changes in the furnace, help control the atmosphere in the furnace and the progress of the reaction in the furnace; the control system is used to integrate the sensor data, monitor the parameters in the furnace in real time, and control and adjust according to the set control strategy.
9. The LF furnace refining and desulfurization method of cord steel according to claim 1, It is characterized in that In the step 7, the reaction equation of the desulfurization treatment is: [High (固体) +S (液态) →CaS (固体) ], In this reaction, calcium oxide (solid) reacts with sulfur (liquid) in molten steel to generate calcium sulfide (solid), thus achieving the desulfurization process.
10. The LF furnace refining and desulfurization method of cord steel according to claim 1, It is characterized in that In the step eight, the method for adjusting the desulfurization agent delivery rate is as follows: A. Monitor the desulfurization effect: Before adjusting the feeding speed, monitor and evaluate the desulfurization effect by monitoring the sulfur content in the molten steel; B. Adjust the delivery speed as needed: According to the real-time monitoring data and desulfurization effect, the delivery speed of the desulfurizer can be gradually adjusted; C. Consider the temperature and stirring of the molten steel: When adjusting the feeding speed, the temperature of the molten steel and whether it is sufficiently stirred should be considered to ensure that the desulfurizer can fully react with the sulfur in the molten steel; D. Regular inspection and adjustment: Regularly inspect the desulfurization equipment and delivery system to ensure that they operate normally and can deliver desulfurizer at the set speed.