Metal ceramic forming cutter and preparation method thereof
By adjusting the material component ratio and process flow of cermet forming tools, and adopting powder premixing and negative pressure vacuum sintering processes, the problems of high preparation cost and insufficient bending strength are solved, and efficient preparation with high performance on existing production lines is achieved. Cermet molding tools with hardness and high bending strength reduce costs.
Patent Information
- Application Number
- CN202410839136.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
AI Technical Summary
The preparation cost of existing cermet forming tools is high and they cannot meet the requirements of high hardness and high bending strength, especially when the requirements for hardness and bending strength are high in bearing processing, resulting in increased costs.
Using raw material powders such as TiCN, Co powder, Ni powder and quaternary solid solution powder, through the processes of powder premixing, ball milling, press molding and negative pressure vacuum sintering, the material component ratio and process flow are adjusted to improve the bending strength while reducing the Preparation costs.
Without increasing the cost and hardness of raw materials, it effectively improves the bending strength of cermet forming tools, reduces preparation costs, meets specific bearing processing needs, and can be completed on existing production lines, saving production costs.
Smart Images

Figure CN118726787A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal powder processing and casting, and in particular to a metal ceramic forming tool and a preparation method thereof. Background Art
[0002] Metal ceramic forming tool is a tool product formed by casting metal ceramic material. Metal ceramic forming tool is a high-end cutting tool that combines the advantages of metal material and ceramic material to improve processing efficiency and processing quality. The main components of this tool are ceramic phase (usually alumina, silicon carbide, etc.) and metal bonding phase (such as nickel, cobalt, molybdenum, etc.). The two are combined through powder metallurgy and other process methods to form a metal ceramic composite material with excellent performance. The metal ceramic material is then processed and cast to finally obtain a metal ceramic forming tool.
[0003] The characteristics of metal ceramic forming tools include:
[0004] 1. High hardness and wear resistance: The ceramic phase provides extremely high hardness, allowing the tool to maintain good edge stability and reduce wear when cutting and processing hard materials at high speeds.
[0005] 2. High temperature stability: Compared with traditional metal tools, metal ceramics can still maintain their hardness and strength at high temperatures, are suitable for high-speed cutting and dry cutting, and reduce the use of coolant.
[0006] 3. Good chemical stability and anti-adhesion: When processing materials such as alloy steel and stainless steel that are prone to built-up edge, the surface of the metal ceramic tool is not easy to chemically react with the workpiece material, reducing tool adhesion and wear.
[0007] 4. Lower density and thermal expansion coefficient: This helps to improve processing accuracy and reduce thermal deformation, especially in precision machining and high-speed machining.
[0008] 5. Design flexibility: By adjusting the ratio of ceramic phase to metal phase and using different sintering processes, tool performance can be designed to meet specific processing requirements.
[0009] Metal ceramic forming tools are widely used in the automotive, aerospace, mold manufacturing and other industries to process difficult-to-process materials such as heat-resistant alloys, high-strength steels, titanium alloys, etc. However, metal ceramic tools are also brittle and sensitive to impact loads, so the cutting conditions need to be controlled during use to avoid sudden load changes that may cause tool breakage.
[0010] Especially in the processing of special bearings, because of the high requirements on the hardness and bending strength of metal ceramic forming tools, higher requirements are often placed on metal ceramic materials.
[0011] However, metal ceramic material is a composite material, which combines the high hardness, high temperature resistance, corrosion resistance and other characteristics of ceramic materials with the advantages of good toughness, ductility and conductivity of metal materials. Any improvement in the requirements for the performance of metal ceramic materials may lead to an increase in costs. Existing metal ceramic materials are usually made by mixing ceramic powder (such as oxides, carbides, nitrides, etc.) with metal or alloy powders, and then using powder metallurgy technology (including pressing, sintering and other steps). In order to improve the bending strength and hardness of metal ceramic forming tools made of metal ceramic materials, it is necessary to have higher requirements for ceramic powder and metal powder from the source. For example, the current general micron-level powder size no longer meets the requirements for these performance improvements. It must be refined to nano-level powder to make the ceramic powder and metal powder mixed more fully. In the subsequent pressing and vacuum sintering process, the metal ceramic material formed by smelting after mixing can have better hardness and better bending strength. However, such operation greatly increases the input cost in terms of raw material preparation, plus the cost of targeted modifications in some process steps and adaptive adjustments of the production line. In order to meet the metal ceramic forming tools required for specific bearing processing, the cost will be huge. Summary of the invention
[0012] The present invention aims to provide a metal ceramic forming tool, so as to achieve the goal of effectively improving the bending strength on the basis of the original production line without additionally increasing the raw material cost and without affecting the hardness.
[0013] In order to achieve the above object, the present invention adopts the following technical scheme:
[0014] Solution 1: A method for preparing a metal ceramic forming tool, comprising the following steps:
[0015] Step 1: Prepare raw material powders, and prepare metal ceramic materials according to the following mass fractions of raw material powders: TiCN: 45-60 parts, average particle size 0.8-1.0 μm; Co powder 4-12 parts, Ni powder 4-12 parts; quaternary solid solution powder 8-15 parts, ultrafine carbide or nitride 0.1-2 parts;
[0016] Step 2: premixing powders. Premix all the powders including the metal powder and the ceramic powder, and then add the premixed powders into a stainless steel ball mill for mixed ball milling for 35-75 hours, so that the various powders are fully mixed into uniform powders. After sufficient mixing, add a paraffin molding agent accounting for 2%-4% of the weight of the powder to the mixed powder in the mixed ball mill to obtain a metal ceramic powder.
[0017] Step 3: pressing and molding the metal ceramic powder at 200-300 MPa to obtain a compact;
[0018] Step 4: negative pressure vacuum sintering, place the pressed green sheet in a sintering furnace, degrease at 20-600℃ under negative pressure, then sinter at 600-1200℃ under vacuum degree of 0.1-2.5kpa, sinter at 1200℃ to the final firing temperature in a nitrogen atmosphere, vacuum degree of 0.1-3kpa, keep warm for 1-2 hours, and cool down by filling with gas at 0.2-1MPa to obtain a metal ceramic forming tool.
[0019] Preferably, the quaternary solid solution powder refers to a solid solution powder with a composition of (W, Ta, Ti, Mx) C, wherein Mx is other metal elements: 850 parts of tungsten powder, 420 parts of tantalum powder, 420 parts of titanium powder, 420 parts of other metal powders and 150 parts of graphite powder are weighed, and the raw materials and tungsten carbide balls are loaded into a stainless steel vacuum ball mill for high-energy ball milling, with a ball-to-material ratio of 10:1, a ball milling speed of 300 rpm, and a ball milling time of 36 hours. The reaction product is then placed in a high-temperature atmosphere furnace, and a thermal chemical reaction is carried out at 800°C for 60 minutes under a nitrogen-hydrogen mixed gas atmosphere to obtain a (W, Ta, Ti, Mx) C solid solution with an average particle size of 95-105 nm. Among them, the (W, Ta, Ti, Mx) C solid solution with an average particle size of 100 nm is the best.
[0020] Preferably, the Mx is Nb or Mo. The other metal elements added are NbC (niobium carbide) or Mo powder, which can improve the high temperature performance, mechanical properties and corrosion resistance of the material by refining the grains, producing precipitation strengthening effect and improving the microstructure.
[0021] Preferably, in the powder premixing, first weigh 170 parts of 200nm face-centered cubic cobalt powder, take 330 parts of quaternary solid solution powder (W, Ta, Ti, Mx)C solid solution, 15 parts of dispersant, weigh 500 parts of 300nm Ti (C0.7, N0.3) powder, mix with all the previous powders, put into a vacuum ball mill, add WC-Co alloy balls at a ball-to-material ratio of 1:5, add 250-350ml of alcohol per 1kg of the mixture, add 2%-4% paraffin, and then perform high-speed ball milling with cold water cooling the ball mill body for 72h; the slurry after vacuum ball milling is discharged and spray-dried to obtain a metal ceramic powder with uniform particle size and good fluidity.
[0022] Preferably, the dispersant is a mixture of CeO2 and VC in a mass ratio of 3:1, and the average particle size is 200nm. The dispersant is set in this way to reduce the agglomeration of the formed bonding wetting phase powder, improve the wettability, increase the load capacity, and enable the bonding wetting phase powder to extend the storage performance, providing more operating time for the subsequent formation of metal ceramic powder.
[0023] Preferably, during the compression molding process, the obtained metal ceramic powder is loaded into a mold and compression molded using a bidirectional press, with bidirectional pressurization and pressure maintained for 15 seconds. A secondary pressurization process is used with a pressing force of 260 MPa. After molding, the pressed green body is trimmed and the appearance quality is inspected.
[0024] The obtained metal ceramic powder is loaded into a mold and molded by a bidirectional press. The bidirectional press is maintained for 15 seconds. The obtained blank has a single weight of 50 parts. The pressed blank is trimmed after molding by a secondary pressurization process.
[0025] Preferably, during the negative pressure vacuum sintering process, an integrated sintering method is adopted, and the heating rate is: 0.2-2°C / min for 20-600°C, 3-8°C / min for 600-1200°C, and 4-7°C / min for 1200-final firing temperature; the final firing temperature is kept for 1-2h, and the temperature is lowered by filling with inert gas at a cooling rate of 10-20°C / min.
[0026] Option 2: The present invention also provides a metal ceramic forming tool, which is prepared by the aforementioned metal ceramic forming tool preparation method; the metal ceramic forming tool is composed of the following mass parts of raw material powder to configure metal ceramic powder, which is pressed into a compact and then sintered under negative pressure; the metal ceramic material is: TiCN: 45-60 parts, average particle size 0.8-1.0μm; Co powder 4-12 parts, Ni powder 4-12 parts; quaternary solid solution powder 8-15 parts, ultrafine carbide or nitride 0.1-2 parts.
[0027] Preferably, the ultrafine carbide is VC and / or Cr3C2 less than 100 nm. Vanadium carbide and chromium carbide both have melting points, good wear resistance and corrosion resistance, and are often used as additives for metal alloys to improve the hardness and thermal stability of the alloys. At ultrafine scale, VC and Cr3C2, due to their extremely small particle size, exhibit more excellent performance than similar carbides of conventional size, such as higher surface area, better dispersibility, and better comprehensive mechanical properties and thermal stability.
[0028] Preferably, the nitride is TiN with a size less than 100 nm. Titanium nitride (TiN) as a metal additive can significantly improve the physical, chemical and mechanical properties of the material, has good bonding strength, and can improve hardness and wear resistance.
[0029] The advantages of this solution are:
[0030] Based on the original production line, the present invention uses a clever material composition ratio and preparation process without increasing the raw material cost and without affecting the hardness, so that the prepared metal ceramic forming tool can effectively improve the bending strength and effectively reduce the preparation cost.
[0031] The present invention sets the raw material powder components and ratios so that TiCN as a matrix only needs to meet the particle size of the micron level, and other powders are also processed according to conventional requirements. There is no need for additional processing requirements for the raw material powders, and the mixed material powder can be obtained after sufficient mixing through the setting of the subsequent powder premixing step, thereby effectively saving the processing cost of the raw material powders.
[0032] More importantly, the entire preparation process can be completed using the existing production line, without the need to purchase additional production lines, effectively saving production costs. By setting up the negative pressure vacuum sintering step, it is possible to increase the sintering negative pressure, vacuum and sintering steps without changing the original equipment, so that the prepared metal ceramic forming tool has better hardness and bending strength without increasing the preparation cost, so that it can meet the specific bearing processing needs.
[0033] The invention effectively solves the problem that the existing metal ceramic forming tool has high preparation cost and cannot achieve high hardness and high bending strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The process flow chart of an embodiment of the present invention.
[0035] Figure 2 1 is a metallographic diagram of a metal ceramic forming tool in an embodiment of the present invention.
[0036] Figure 3 This is the metallographic diagram of the metal-ceramic forming tool purchased from abroad. DETAILED DESCRIPTION
[0037] The following is further described in detail through specific implementation methods:
[0038] Embodiment 1
[0039] The embodiment is basically as shown in the attached Figure 1 As shown: The preparation method of the metal ceramic forming tool in this embodiment includes the following steps:
[0040] S1. Prepare raw powders. Prepare metal ceramic materials according to the following mass proportions of raw powders: TiCN: 45-60 parts, average particle size 0.8-1.0μm; Co powder 4-12 parts, Ni powder 4-12 parts; quaternary solid solution powder 8-15 parts, ultrafine carbide or nitride 0.1-2 parts; all the above powders do not require additional processing, and all use powder particles of the current industry common size, without additional raw material costs.
[0041] The ultrafine carbide in this embodiment refers to VC and / or Cr3C2 with an average particle size of less than 100 nm, and the ultrafine nitride refers to TiN with an average particle size of less than 100 nm. Both can be purchased directly from the market and play the role of connecting phases.
[0042] The above-mentioned raw material powder settings of various components and mass proportions can increase toughness without affecting hardness, so that the bending strength of the processed metal-ceramic material and metal-ceramic forming tool can be significantly improved without affecting hardness.
[0043] S2, premixing powders, premixing all the powders including the metal powder and the ceramic powder, and then adding the premixed powders into a stainless steel ball mill for mixed ball milling for 35-75 hours, so that various powders are fully mixed into uniform powders. After sufficient mixing, adding a paraffin molding agent accounting for 2%-4% of the mass of the powders to the powders in the mixed ball mill to obtain a mixed powder, so that the mixed powder can form a fixed, average, minimum unit of metal ceramic particles composed of ceramic powder and metal powder in a specific ratio, that is, forming metal ceramic powder;
[0044] S3, pressing and molding, pressing the metal ceramic powder at 200-300 MPa to obtain a compact; wherein pressing at 260 MPa is optimal;
[0045] S4, negative pressure vacuum sintering, place the pressed blank in a sintering furnace, degrease at negative pressure at 20-600℃, then vacuum sinter at 600-1200℃ at a vacuum degree of 0.1-2.5kpa, sinter in a nitrogen atmosphere from 1200℃ to the final firing temperature, vacuum degree of 0.1-3kpa, keep warm for 1-2 hours, cool down with a gas of 0.2-1MPa, adopt an integrated sintering method, heating rate: 20-600℃ at 0.2-2℃ / min, 600-1200℃ at 3-8℃ / min, 1200-final firing temperature at 4-7℃ / min; keep the final firing temperature for 1-2h, cool down with inert gas, cooling rate of 10-20℃ / min, to obtain a metal ceramic forming tool. Compared with simple low-pressure sintering or single vacuum sintering, the negative pressure vacuum sintering of the present invention is a multi-step continuous sintering process, which firstly performs negative pressure degreasing to make the metal ceramic material in the green compact more compact, then performs vacuum sintering to gradually change the quality of the metal ceramic material, and then continues to increase the temperature and sinter in a nitrogen environment to reduce the release of nitrogen under high temperature conditions and the generation of pores, so that the sintering space always maintains a negative pressure state, making the green compact dense and compact, so that each metal ceramic particle in the green compact can get sufficient reaction time, and no other impurities are added during the sintering process, and finally the green compact is sintered in a vacuum environment for 1-2 hours to form a metal ceramic tool.
[0046] Among them, the quaternary solid solution powder in this embodiment refers to a solid solution powder with a composition of (W, Ta, Ti, Mx)C, wherein Mx is the Nb element provided from NbC, and the quaternary solid solution powder (W, Ta, Ti, Mx)C is a solid solution powder of (W, Ta, Ti, Nb)C: 850 parts of tungsten powder, 420 parts of tantalum powder, 420 parts of titanium powder, 420 parts of NbC powder and 150 parts of graphite powder are weighed, and the raw materials and tungsten carbide balls are loaded into a stainless steel vacuum ball mill for high-energy ball milling, the ball-to-material ratio is 10:1, the ball milling speed is 300 rpm, and the ball milling time is 36 hours. Then the reaction product is placed in a high-temperature atmosphere furnace, and a thermal chemical reaction is carried out at 800°C for 60 minutes under a nitrogen-hydrogen mixed gas atmosphere to obtain a (W, Ta, Ti, Nb)C solid solution with an average particle size of 95-105nm. Among them, the (W, Ta, Ti, Nb) C solid solution with an average particle size of 100 nm is the best. The other metal element added is NbC (niobium carbide), which improves the material's high temperature performance, mechanical properties and corrosion resistance by refining the grains, producing precipitation strengthening effects and improving the microstructure.
[0047] The role of the quaternary solid solution powder prepared in this way is to make the required components more evenly distributed. Its composition contains TaC, which can improve the intermittent cutting performance of metal ceramic materials, and NbC can improve the wettability of the matrix bonding phase and the ceramic phase, regulate the phase change, promote the interface bonding, and has the effect of refining the grains. This scheme adopts a mass ratio of 8-15 parts, among which 13 parts is the best. The bending strength of the metal ceramic forming tool obtained at this mass ratio is the best.
[0048] Specifically, in the premixing of powders in S2, first weigh 170 parts of 200nm face-centered cubic cobalt powder, take 330 parts of quaternary solid solution powder (W, Nb, Ta)C solid solution, 15 parts of dispersant (CeO2 and VC are mixed in a mass ratio of 3:1, with an average particle size of 200nm), weigh 500 parts of 300nm Ti (C0.7, N0.3) powder, mix with all the previous powders, put into a vacuum ball mill, add WC-Co alloy balls at a ball-to-material ratio of 1:5, add 250-350ml of alcohol for every 1kg of the mixture, add 2%-4% paraffin, and then perform high-speed ball milling for 72h while the ball mill body is cooled with cold water; the slurry after vacuum ball milling is discharged and spray-dried to obtain a metal ceramic powder with uniform particle size and good fluidity.
[0049] The dispersant is a mixture of CeO2 and VC in a mass ratio of 3:1, and the average particle size is 200nm. The dispersant is set in this way to reduce the agglomeration of the formed bonding wetting phase powder, improve the wettability, increase the load, and enable the bonding wetting phase powder to extend the storage performance, providing more operating time for the subsequent formation of metal ceramic powder.
[0050] In the S3 pressing process: the obtained metal ceramic powder is loaded into the mold, and a bidirectional press is used for compression molding, bidirectional pressurization is applied, and the pressure is maintained for 15 seconds (the blank has a single weight of 50 parts), and a secondary pressurization process is used, and the pressing force is 260MPa. After molding, the pressed blank is trimmed and the appearance quality is inspected;
[0051] The metal ceramic forming tool prepared by the above method has a hardness of HRA90-93, a bending strength of 2000-2300MPa, and a fracture toughness of 10-12.5MPa·m 1 / 2 .
[0052] Under the premise of taking into account both the preparation cost and the performance of metal ceramic forming tools, that is, under the following conditions:
[0053] S1, prepare raw material powders, and prepare metal ceramic materials according to the following raw material powders by mass: TiCN: 55 parts, average particle size 1.0 μm; Co powder 8 parts, Ni powder 8 parts; quaternary solid solution powder 13 parts, ultrafine carbide VC 1 part;
[0054] S2, pre-mixing the powders and ball milling for 75 hours to fully mix the various powders into uniform powders. After fully mixing, adding a paraffin molding agent accounting for 3% of the weight of the powders to the mixed powders in the mixed ball mill to obtain a mixed powder, so that the mixed powders can form a fixed, average, minimum unit of metal ceramic particles composed of ceramic powder and metal powder in a specific ratio, that is, forming metal ceramic powder;
[0055] S3, pressing and molding, pressing and molding the metal ceramic powder at 260 MPa to obtain a compact;
[0056] S4, negative pressure vacuum sintering, place the pressed green sheet in the sintering furnace, gradually heat up to 600℃ for negative pressure degreasing, then gradually increase the temperature from 600℃ to 1200℃ for vacuum sintering at a vacuum degree of 2.5kpa, sinter from 1200℃ to the final firing temperature in a nitrogen atmosphere, vacuum degree of 1.8kpa, keep warm for 2 hours, charge 0.8MPa to cool down, adopt the integrated sintering method, heating rate: 20-600℃ adopts 1.8℃ / min, 600-1200℃ adopts 4℃ / min, 1200-final firing temperature adopts 6℃ / min. The final firing temperature is kept warm for 2h, and the inert gas nitrogen or argon (Ar) is charged to cool down, and the cooling rate is 16℃ / min to the metal ceramic forming tool.
[0057] Among them, the quaternary solid solution powder in this embodiment refers to a solid solution powder with a composition of (W, Ta, Ti, Nb)C. 850 parts of tungsten powder, 420 parts of tantalum powder, 420 parts of titanium powder, 420 parts of NbC powder and 150 parts of graphite powder are weighed, and the raw materials and tungsten carbide balls are loaded into a stainless steel vacuum ball mill for high-energy ball milling. The ball-to-material ratio is 10:1, the ball milling speed is 300 rpm, and the ball milling time is 36 hours. The reaction product is then placed in a high-temperature atmosphere furnace and subjected to a thermal chemical reaction at 800°C for 60 minutes in a nitrogen-hydrogen mixed gas atmosphere to obtain a (W, Ta, Ti, Nb)C solid solution with an average particle size of 100 nm.
[0058] In the powder premixing in S2, first weigh 170 parts of 200nm face-centered cubic cobalt powder, take 330 parts of quaternary solid solution powder (W, Ta, Ti, Nb)C solid solution, 15 parts of dispersant, weigh 500 parts of 300nm Ti (C0.7, N0.3) powder, mix with all the previous powders, put into a vacuum ball mill, add WC-Co alloy balls at a ball-to-material ratio of 1:5, add 300ml of alcohol for every 1kg of the mixture, add 3% paraffin, and then perform high-speed ball milling with cold water cooling the ball mill body for 72h; the slurry after vacuum ball milling is discharged and spray-dried to obtain a metal ceramic powder with uniform particle size and good fluidity.
[0059] In the S3 pressing process: the obtained metal ceramic powder is loaded into the mold, and a bidirectional press is used for compression molding, bidirectional pressurization is applied, and the pressure is maintained for 15 seconds (the blank has a single weight of 50 parts), and a secondary pressurization process is used, and the pressing force is 260MPa. After molding, the pressed blank is trimmed and the appearance quality is inspected;
[0060] The hardness of the metal ceramic forming tool finally prepared by the above method is HRA92.2, the bending strength is 2000MPa, and the fracture toughness is 10.15MPa·m 1 / 2 , imported forming tools with the same hardness of HRA92.2 and bending strength of 2000MPa were selected for comparison.
[0061] like Figure 2 and Figure 3 As shown, Figure 2 is a metallographic diagram of a metal ceramic forming tool prepared under the aforementioned optimal conditions of the present invention, Figure 3 This is the metallographic diagram of a metal ceramic forming tool with the same performance purchased from abroad at a high price. Figure 2 and Figure 3 It can be seen that the properties of the metal ceramic forming tool prepared by the present invention are comparable to those of the metal ceramic forming tool purchased at a high price from abroad, both of which have good uniformity and grain structure, and both have low porosity. Figure 3 , the present invention Figure 2 Has better interface clarity.
[0062] When the basic performance of two metal ceramic forming tools is equivalent, the processing and preparation cost of the present invention is much lower than that of imported forming tools with the same performance, and the preparation cost is reduced by about 50%. The present invention can be operated using existing production lines, effectively saving production inputs, and has no special requirements for various metal powders and ceramic powders as raw materials, and does not require additional processing. Existing general-purpose particle size powders can meet the requirements, effectively saving raw material costs. The forming tool prepared by this method takes into account hardness and bending strength, has good performance, and the preparation cost is greatly reduced, and has a strong prospect for promotion and application.
[0063] Embodiment 2
[0064] Different from the first embodiment, in this embodiment, the quaternary solid solution powder in this embodiment refers to a solid solution powder with a composition of (W, Ta, Ti, Mx) C, wherein Mx is other metal elements, and in this embodiment, Mx is Mo: 850 parts of tungsten powder, 420 parts of tantalum powder, 420 parts of molybdenum powder, 420 parts of titanium powder and 150 parts of graphite powder are weighed, and the raw materials and tungsten carbide balls are put into a stainless steel vacuum ball mill for high-energy ball milling, the ball-to-material ratio is 10:1, the ball milling speed is 300 rpm, and the ball milling time is 36 hours. Then, the reaction product is placed in a high-temperature atmosphere furnace, and a thermal chemical reaction is carried out at 800°C for 60 minutes under a nitrogen-hydrogen mixed gas atmosphere to obtain a (W, Ta, Ti, Mo) C solid solution with an average particle size of 95-105 nm. Among them, the (W, Ta, Ti, Mo) C solid solution with an average particle size of 100 nm is the best. The other metal element added is Mo provided by Mo2C (molybdenum carbide), which can improve the wettability of the matrix bonding phase and the ceramic phase and has the effect of refining the grains.
[0065] This solution adopts a mass ratio of 8 to 15 parts, among which 13 parts is the best. The bending strength of the metal ceramic forming tool obtained at this mass ratio is the best.
[0066] Specifically, before pre-mixing the powders in S2, weigh 170 parts of 200nm face-centered cubic cobalt powder, 330 parts of quaternary solid solution powder (W, Ta, Ti, Mo) C solid solution, 15 parts of dispersant (CeO2 and VC are mixed in a mass ratio of 3:1, with an average particle size of 200nm), weigh 500 parts of 300nm Ti (C0.7, N0.3) powder, mix them with all the previous powders, put them into a vacuum ball mill, add WC-Co alloy balls at a ball-to-material ratio of 1:5, add 250-350ml of alcohol for every 1kg of the mixture, add 2%-4% paraffin, and then perform high-speed ball milling for 72h while the ball mill body is cooled with cold water; the slurry after vacuum ball milling is discharged and spray-dried to obtain a metal ceramic powder with uniform particle size and good fluidity.
[0067] This embodiment uses a quaternary solid solution different from that of the first embodiment, and can also produce metal ceramic forming tools with good performance, and compared with existing tools with the same performance, the production cost is effectively reduced.
[0068] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A method for preparing a metal ceramic forming tool, characterized in that: The following steps are involved: Step 1: Prepare raw material powders, and prepare metal ceramic materials according to the following mass fractions of raw material powders: TiCN: 45-60 parts, average particle size 0.8-1.0 μm; Co powder 4-12 parts, Ni powder 4-12 parts; quaternary solid solution powder 8-15 parts, ultrafine carbide or nitride 0.1-2 parts; Step 2: premixing powders. Premix all the powders including the metal powder and the ceramic powder, and then add the premixed powders into a stainless steel ball mill for mixed ball milling for 35-75 hours, so that the various powders are fully mixed into uniform powders. After sufficient mixing, add a paraffin molding agent accounting for 2%-4% of the weight of the powder to the mixed powder in the mixed ball mill to obtain a metal ceramic powder. Step 3: pressing and molding the metal ceramic powder at 200-300 MPa to obtain a compact; Step 4: negative pressure vacuum sintering, place the pressed green sheet in a sintering furnace, degrease at 20-600℃ under negative pressure, then sinter at 600-1200℃ under vacuum degree of 0.1-2.5kpa, sinter at 1200℃ to the final firing temperature in a nitrogen atmosphere, vacuum degree of 0.1-3kpa, keep warm for 1-2 hours, and cool down by filling with gas at 0.2-1MPa to obtain a metal ceramic forming tool.
2. The method for preparing a metal ceramic forming tool according to claim 1, characterized in that: Quaternary solid solution powder refers to a solid solution powder with a composition of (W, Ta, Ti, Mx)C, wherein Mx is other metal elements: 850 parts of tungsten powder, 420 parts of tantalum powder, 420 parts of titanium powder, 420 parts of other metal powders and 150 parts of graphite powder are weighed, and the raw materials are loaded into a stainless steel vacuum ball mill together with tungsten carbide balls for high-energy ball milling, with a ball-to-material ratio of 10:1, a ball milling speed of 300 rpm, and a ball milling time of 36 hours. The reaction product is then placed in a high-temperature atmosphere furnace, and a thermal chemical reaction is carried out at 800°C for 60 minutes under a nitrogen-hydrogen mixed gas atmosphere to obtain a (W, Ta, Ti, Mx)C solid solution with an average particle size of 95-105nm.
3. The method for preparing a metal ceramic forming tool according to claim 2, characterized in that: The Mx is Nb or Mo.
4. The method for preparing a metal ceramic forming tool according to claim 2, characterized in that: In the powder premixing, first weigh 170 parts of 200nm face-centered cubic cobalt powder, take 330 parts of quaternary solid solution powder (W, Ta, Ti, Mx)C solid solution, 15 parts of dispersant, weigh 500 parts of 300nm Ti (C0.7, N0.3) powder, mix with all the previous powders, put into a vacuum ball mill, add WC-Co alloy balls at a ball-to-material ratio of 1:5, add 250-350ml of alcohol per 1kg of the mixture, add 2%-4% paraffin, and then perform high-speed ball milling with cold water cooling in the ball mill body for 72h; after unloading the slurry after vacuum ball milling, spray drying is performed to obtain a metal ceramic powder with uniform particle size and good fluidity.
5. The method for preparing a metal ceramic forming tool according to claim 4, characterized in that: The dispersant is prepared by mixing CeO2 and VC in a mass ratio of 3:1, and the average particle size is 200nm.
6. The method for preparing a metal ceramic forming tool according to claim 1, characterized in that: During the pressing process, the obtained metal ceramic powder is loaded into a mold and pressed using a bidirectional press. Bidirectional pressurization is applied for 15 seconds. A secondary pressurization process is used with a pressing force of 260 MPa. After molding, the pressed green body is trimmed and the appearance quality is inspected.
7. The method for preparing a metal ceramic forming tool according to claim 1, characterized in that: During the negative pressure vacuum sintering process, an integrated sintering method is adopted, and the heating rate is: 0.2-2℃ / min for 20-600℃, 3-8℃ / min for 600-1200℃, and 4-7℃ / min for 1200-final firing temperature; the final firing temperature is kept for 1-2h, and the temperature is lowered by filling with inert gas at a cooling rate of 10-20℃ / min.
8. A metal ceramic forming tool, characterized in that: The metal ceramic forming tool is prepared by the preparation method of the metal ceramic forming tool as described in claim 1; the metal ceramic forming tool is prepared by configuring the metal ceramic powder with the following mass parts of raw material powder, pressing it into a compact and then sintering it under negative pressure; the metal ceramic material is: TiCN: 45-60 parts, average particle size 0.8-1.0μm; Co powder 4-12 parts, Ni powder 4-12 parts; quaternary solid solution powder 8 parts-15 parts, ultrafine carbide or nitride 0.1-2 parts.
9. The metal ceramic forming tool according to claim 8, characterized in that: The ultrafine carbides are VC and / or Cr3C2 with a size less than 100 nm.
10. The metal ceramic forming tool according to claim 8, characterized in that: The nitride is TiN with a thickness less than 100 nm.
Citation Information
Patent Citations
Wood cutting tool material of Ti(CN) cermet and preparation method thereof
CN102433482A
Superfine metalloceramics material and preparation method thereof
CN105734382A
Ti (C, N)-based metal ceramic with mixed crystal structure and preparation method thereof
CN109576545A
Wear-resistance anti-corrosion Ti(C,N)-based metal ceramic and preparation method thereof
CN111004954A
Preparation method of graphene reinforced and toughened titanium-based metal ceramic
CN115584409A
Cited By
Preparation method and application of high-cost-performance alloy
CN119457057A