Alloy powder material for thermal barrier coating bonding layer and preparation method of alloy powder material
Fe, Cr, Al, B, and W alloy powder materials are prepared through mechanical alloying to form a high-entropy alloy bonding layer, which solves the problem of instability of existing thermal barrier coatings at high temperatures and significantly improves the performance of thermal barrier coatings. The bonding strength and corrosion resistance of the coating extend the service life of the coating.
Patent Information
- Application Number
- CN202410738673.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-01
AI Technical Summary
The existing thermal barrier coating bonding layer is unstable in high-temperature environments, resulting in a decrease in the bonding strength between the ceramic layer and the substrate, peeling failure, and reduced thermal barrier coating system life.
Fe, Cr, Al, B, and W alloy powder materials are prepared through mechanical alloying. The atomic ratio and particle size are specified. After ball milling, high-entropy alloy powder is formed to form a stable bonding layer and improve high-temperature corrosion resistance.
It achieves the stability and corrosion resistance of alloy powder at high temperatures, significantly improves the bonding strength and life of the thermal barrier coating, and extends the service life of the coating.
Smart Images

Figure CN118726862A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal spraying, and in particular to an alloy powder material for a bonding layer of a thermal barrier coating and a preparation method thereof. Background Art
[0002] With the development of low-speed engines and the application of new fuels, the operating temperature of hot end components is getting higher and higher, which is greater than 1200℃. Therefore, thermal barrier coatings (such as ceramic thermal barrier coatings) are used as protective coatings for hot end components of gas turbines, aircraft engines and hypersonic aircraft to provide heat insulation and cooling, which can greatly improve the service life and service temperature of gas turbines. However, due to the weak bonding strength between the thermal barrier coating and the metal substrate (less than 10MPa), the thermal barrier coating is prone to peeling and failure during service. Therefore, a bonding layer must be set between the thermal barrier coating and the metal substrate to improve the bonding strength between the two (reaching 20-30MPa).
[0003] As an essential component of the thermal barrier coating system, the bonding layer not only affects the anti-stripping properties of the thermal barrier coating, but also plays the role of anti-oxidation, anti-corrosion and regulating the thermal expansion coefficient. The dense metal bonding layer made of NiCrAlY alloy material, which is widely used in the bonding layer of thermal barrier coatings, is shown in patent documents CN117568732A, CN117702044A, and CN117488230A. However, under a continuous high temperature environment, the bonding layer prepared by this type of material will gradually oxidize to generate high-temperature oxides such as Al2O3 and CrO, among which Al2O3 plays a certain strengthening role in the bonding between the substrate and the ceramic layer, while high-temperature oxides such as CrO are unstable at high temperatures, resulting in a decrease in the bonding strength between the ceramic layer and the substrate, which in turn causes the ceramic layer to gradually peel off, thereby reducing the life of the thermal barrier coating system.
[0004] In view of the defects of the traditional NiCrAlY bonding layer, the current research focuses on inhibiting the generation of spinel phase through active element modification, slowing down the growth rate of thermal barrier coating TGO, thereby improving the high temperature service life of thermal barrier coating. There are also studies that use the high temperature stability of high entropy alloys and the high temperature resistant oxides with bonding properties formed at high temperatures to improve the high temperature resistance of the bonding layer. Summary of the invention
[0005] The purpose of the present invention is to provide an alloy powder material for a bonding layer of a thermal barrier coating and a preparation method thereof. The alloy powder material is proportioned according to the alloy composition design principle and is made by a mechanical alloying method. It has high phase stability and excellent corrosion resistance in a high temperature environment.
[0006] In order to achieve the above object, the technical solution of the present invention is:
[0007] The alloy powder material for a bonding layer of a thermal barrier coating of the present invention is characterized in that it is prepared by a mechanical alloying method using Fe powder, Cr powder, Al powder, B powder and W powder, wherein the atomic ratio of the Fe powder, Cr powder, Al powder, B powder and W powder is (20-26): (24-28): 26: (10-15): 11, and the particle size of the alloy powder is ≤48 μm.
[0008] The method for preparing an alloy powder material for a bonding layer of a thermal barrier coating according to the present invention is characterized in that it comprises the following steps:
[0009] (1) Fe powder, Cr powder, Al powder, B powder, and W powder are weighed and mixed according to a specified atomic ratio, and the mixed powder is placed in a ball mill;
[0010] (2) introducing protective gas into the ball milling tank and ball milling at a specified speed;
[0011] (3) After the ball mill is cooled, the powder is separated through a 300-mesh sieve to obtain the alloy powder material for the bonding layer of the thermal barrier coating, which is stored in a vacuum storage tank for later use.
[0012] Preferably, the ball milling jar is a silicon nitride spherical ink jar equipped with zirconium oxide ball milling balls.
[0013] Preferably, the ball-to-material weight ratio during the ball milling process is (15-20):1; the ball milling speed is 400-600 r / min, and the ball milling time is 40-60 h.
[0014] Preferably, the protective gas is argon.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] The invention adopts a mechanical alloying method, and the preparation process is simple and easy to operate; the obtained alloy powder for the bonding layer of the thermal barrier coating has a small particle size, relatively uniform particles, excellent adhesion, and good environmental performance; because the alloy powder contains B and W elements, it can maintain a stable state when the use temperature is as high as 1500°C or even higher, thereby improving the heat resistance of the alloy bonding layer of the thermal barrier coating, ensuring excellent corrosion resistance at high temperatures, and providing support for extending the life of the thermal barrier coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is the SEM image of the alloy powder material for the bonding layer of the thermal barrier coating in Example 1.
[0018] Figure 2 This is the XRD spectrum of the alloy powder material for the bonding layer of the thermal barrier coating in Examples 1 to 3. DETAILED DESCRIPTION
[0019] Those skilled in the art should recognize that the present embodiment is only used to illustrate the present invention, and is not used to limit the present invention. Any changes or modifications to the embodiment within the scope of the present invention are within the scope of the claims of the present invention.
[0020] Example 1
[0021] The alloy powder material for thermal barrier coating is prepared by mechanical alloying method using Fe powder, Cr powder, Al powder, B powder and W powder as raw materials. The specific steps are as follows:
[0022] (1) Fe powder, Cr powder, Al powder, B powder, and W powder were weighed according to an atomic ratio of 22:28:26:13:11, with a total mass of 200 g; the weighed mixed powder was placed in a silicon nitride ball mill, with a weight ratio of 1:15 to zirconia ball milling balls;
[0023] (2) The protective gas argon was introduced into the ball mill and the mill was milled at a speed of 400 r / min for 60 h;
[0024] (3) After the ball mill body is cooled, the powder and the ball mill are taken out together, and the two are sieved and separated with a 300-mesh sieve to obtain the alloy powder material for the bonding layer of the thermal barrier coating, which is stored in a vacuum storage tank for later use.
[0025] Example 2
[0026] The alloy powder material for thermal barrier coating is prepared by mechanical alloying method using Fe powder, Cr powder, Al powder, B powder and W powder as raw materials. The specific steps are as follows:
[0027] (1) Fe powder, Cr powder, Al powder, B powder, and W powder were weighed according to an atomic ratio of 26:24:26:13:11, with a total mass of 200 g; the weighed mixed powder was placed in a silicon nitride ball mill, with a weight ratio of 1:18 to zirconia ball milling balls;
[0028] (2) introducing protective gas argon into the tank and ball milling at a speed of 500 r / min for 50 h;
[0029] (3) After the ball mill body is cooled, the powder and the ball mill are taken out together, and the two are sieved and separated with a 300-mesh sieve to obtain the alloy powder material for the bonding layer of the thermal barrier coating, which is stored in a vacuum storage tank for later use.
[0030] Example 3
[0031] The alloy powder material for thermal barrier coating is prepared by mechanical alloying method using Fe powder, Cr powder, Al powder, B powder and W powder as raw materials. The specific steps are as follows:
[0032] (1) Fe powder, Cr powder, Al powder, B powder, and W powder were weighed according to an atomic ratio of 24:27:26:12:11, with a total mass of 200 g; the weighed mixed powder was placed in a silicon nitride ball mill, with a weight ratio of 1:20 to the zirconia ball mill;
[0033] (2) introducing protective gas argon into the tank and ball milling at a speed of 600 r / min for 40 h;
[0034] (3) After the ball mill body is cooled, the powder and the ball mill are taken out together, and the two are sieved and separated with a 300-mesh sieve to obtain the alloy powder material for the bonding layer of the thermal barrier coating, which is stored in a vacuum storage tank for later use.
[0035] Test experiment example
[0036] The valence electron numbers of the alloy powder materials for the bonding layer of the thermal barrier coating of Examples 1 to 3 are calculated, as shown in Table 1. As can be seen from Table 1, the valence electron numbers of Examples 1 to 3 are all <6.9, indicating that the alloy powders for the thermal barrier coating of Examples 1 to 3 are all high entropy alloys that can form a BCC (body-centered cubic) solid solution phase.
[0037] Table 1 Valence electron numbers of alloy powders of Examples 1 to 3
[0038]
[0039] The crystal structure and microscopic morphology of the prepared alloy powder for thermal barrier coating were analyzed by SEM and XRD. After the alloy powder for thermal barrier coating prepared in Examples 1 to 3 was processed into coatings, high temperature oxidation tests, corrosion resistance and bonding strength tests were performed on them.
[0040] Figure 1 This is a SEM image of the alloy powder material for the bonding layer of the thermal barrier coating of Example 1. The SEM image can intuitively analyze the surface microstructure of the alloy powder material for the bonding layer of the thermal barrier coating of Example 1. It can be found that the alloy powder particles of Example 1 are well dispersed, the observed particle size is relatively uniform, and the average particle size is about 5 μm.
[0041] XRD analysis was performed on the alloy powder materials for the bonding layer of the thermal barrier coating of Examples 1 to 3. Figure 2 From the XRD results, it can be seen that there is no obvious sharp diffraction peak in the range of 30° to 100°, indicating the formation of amorphous state. The characteristic peaks of the samples of Examples 1 to 3 appearing near 45° are in the shape of steamed buns, which are typical amorphous substances.
[0042] The alloy powder for the bonding layer of the thermal barrier coating of Examples 1 to 3 was made into a coating by laser cladding, and the coating sample was placed in a box-type resistance furnace for a high-temperature oxidation test: oxidation at 1500°C for 10 hours, and the sample was weighed after cooling in the furnace; 10 hours was a cycle, and the cumulative high-temperature oxidation time was 100 hours. According to the principle of oxidation kinetics, the average oxidation rate K+ of the coating sample was calculated, and the test results are shown in Table 2.
[0043] Table 2 Antioxidation performance test results of alloy powder coatings of Examples 1 to 3
[0044] Alloy coating name <![CDATA[K + ]]> Antioxidant performance evaluation Example 1 0.09 Complete antioxidant Example 2 0.08 Complete antioxidant Example 3 0.09 Complete antioxidant Prior art bonding layer NiCoCrAlY 1.5 Secondary Antioxidant
[0045] It can be seen from the results in the above table that the average oxidation resistance rate of the coating samples of Examples 1 to 3 is all less than 0.1. Compared with the bonding layer of the prior art (commercially available products, such as NiCoCrAlY of Qinghe Feipu Alloy Materials Co., Ltd.), the oxidation resistance level of Examples 1 to 3 is high, indicating that the cladding coating prepared from the alloy powder for thermal barrier coating of the present invention has better heat resistance.
[0046] The alloy powders for the bonding layer of the thermal barrier coatings of Examples 1 to 3 were prepared into coatings by laser cladding. The coating samples were immersed in a simulated seawater (3.5% NaCl) solution to test their corrosion resistance. The coating samples were used as working electrodes. The working area of the samples was 1 cm 2 The saturated calomel electrode (SCE) was used as the reference electrode, the platinum electrode was used as the auxiliary electrode, and the scanning speed was 2 mV / s. The impedance (EIS) diagram and electrochemical polarization curve were measured on the electrochemical workstation. The self-corrosion potential (E coor ) and self-corrosion current density (I coor ), the test results are shown in Table 3.
[0047] Table 3 Self-corrosion potential and self-corrosion current density of alloy powder coatings of Examples 1 to 3
[0048] Alloy coating name <![CDATA[E coor / (V,vsSCE)]]> <![CDATA[I coor / (μA·cm -2 )]]> Example 1 -0.426 0.2385 Example 2 -0.438 0.2461 Example 3 -0.423 0.2298 Prior art bonding layer NiCoCrAlY -0.608 5.8731
[0049] It can be seen from the results in the above table that the self-corrosion potential and self-corrosion current density of the coating samples of Examples 1 to 3 are comparable. Compared with the bonding layer of the prior art, the self-corrosion potential of Examples 1 to 3 is high and the self-corrosion current density is small, indicating that the cladding coatings prepared from the alloy powder for the bonding layer of the thermal barrier coating of the present invention have a lower corrosion reaction driving force and a significantly lower tendency to corrosion.
[0050] Referring to the standard HB 5476-1991 "Test method for bonding strength of thermal spray coatings", the substrate material is selected as 15CrMo alloy structural steel; the bonding strength test is carried out on the coating samples of Examples 1 to 3, and the test results are shown in Table 4.
[0051] Table 4 Bonding strength of alloy powder coatings of Examples 1 to 3
[0052] Alloy coating name Bonding strength / MPa Example 1 86 Example 2 90 Example 3 88 Prior art bonding layer NiCoCrAlY 60
[0053] It can be seen from Table 4 that the bonding strength between the cladding coating prepared by the alloy powder for the bonding layer of the thermal barrier coating of the present invention and the substrate material 15CrMo alloy structural steel is higher than that of the bonding layer of the prior art, and the adhesion is more excellent.
Claims
1. An alloy powder material for a thermal barrier coating bonding layer, characterized in that: The invention is prepared by a mechanical alloying method using Fe powder, Cr powder, Al powder, B powder and W powder, wherein the atomic ratio of the Fe powder, Cr powder, Al powder, B powder and W powder is (20-26): (24-28): 26: (10-15): 11, and the particle size of the powder is ≤48 μm.
2. The method for preparing the alloy powder material for the bonding layer of the thermal barrier coating according to claim 1, characterized in that: The following steps are involved: (1) Fe powder, Cr powder, Al powder, B powder, and W powder were weighed and mixed according to the specified atomic ratio, and the mixed powder was placed in a ball mill; (2) introducing protective gas into the ball milling tank and ball milling at a specified speed; (3) After the ball mill is cooled, the powder is separated through a 300-mesh sieve to obtain the alloy powder material for the bonding layer of the thermal barrier coating.
3. The method for preparing the alloy powder material for the bonding layer of the thermal barrier coating according to claim 2, characterized in that: The ball milling jar is a silicon nitride spherical ink jar equipped with zirconium oxide ball milling balls.
4. The method for preparing the alloy powder material for the bonding layer of the thermal barrier coating according to claim 3, wherein: The ball-to-material weight ratio during the ball milling process is (15-20):1; the ball milling speed is 400-600 r / min; and the ball milling time is 40-60 h.
5. The method for preparing the alloy powder material for the bonding layer of a thermal barrier coating according to claim 2, characterized in that: The protective gas is argon.
Citation Information
Patent Citations
Thermal barrier coating with high-temperature gradient structure and preparation method of thermal barrier coating
CN117488230A
High-bonding-strength ceramic thermal barrier coating on surface of aluminum alloy and preparation method of high-bonding-strength ceramic thermal barrier coating
CN117568732A
High-bonding-strength ceramic thermal barrier coating on surface of nickel-based alloy and preparation method of high-bonding-strength ceramic thermal barrier coating
CN117702044A
Cited By
Thermal barrier coating with nano-composite double-layer ceramic structure and preparation method of thermal barrier coating
CN119491184A