Heat treatment process for eliminating residual stress of copper alloy thin strip
Through the heat treatment process of online solid solution treatment, hot rolling blanking, cold rolling and intermediate annealing, the annealing process of the copper alloy thin strip is optimized, the problems of residual stress and etching performance of the copper alloy strip are solved, and the residual stress and etching performance of the copper alloy strip are significantly reduced. stress and improve etching performance.
Patent Information
- Application Number
- CN202410925066.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology is difficult to effectively reduce the residual stress while weighing the strength and conductivity of the copper alloy strip, and the etching performance is poor, leading to problems such as warping.
The heat treatment process of online solid solution treatment, hot rolling blanking, cold rolling and intermediate annealing, annealing and other steps is used to control the thickness and annealing temperature of the copper alloy thin strip. The residual stress is reduced by optimizing the heat treatment process to prepare a copper alloy with excellent performance. thin strip.
It significantly reduces the residual stress of the copper alloy thin strip, improves its texture strength and etching performance, provides excellent raw materials for subsequent high-precision etching of the copper alloy lead frame, and ensures the overall performance of the alloy.
Smart Images

Figure CN118726871A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat treatment, and particularly relates to a heat treatment process for eliminating residual stress of a copper alloy thin strip. Background Art
[0002] The integrated circuit industry is a focal point of current and future global technological competition. Currently, copper alloy lead frames serve as the chip carriers for integrated circuits, the channel through which chips communicate with the outside world, and are a crucial foundational material in the semiconductor industry. The copper alloy strip used for lead frames is primarily produced using chemical etching. While etching, as a stress-free process, enables the production of high-density, high-pin count lead frames, this method places more stringent demands on the copper alloy strip's internal stress, warpage, surface quality, and etching performance. Uneven stress release during etching can cause warping in rolled copper alloy strip, seriously impacting the subsequent use of the product. Therefore, as product performance requirements continue to increase, the question of how to effectively reduce residual stress and improve etching performance while balancing the strength and conductivity of copper alloy strip has become a key research topic.
[0003] Rolling and annealing are key processes in the manufacturing of copper alloy strip for lead frames. Annealing effectively reduces residual stresses generated during rolling and improves the alloy's fatigue performance and ductility. Low-temperature stress relief annealing adjusts the metal's texture and composition, altering the microstructure within the grains and causing dislocation rearrangement, thereby effectively reducing residual stress. High and uneven residual stresses in copper alloy strip for etched lead frames can easily lead to strip warping and workpiece failure. Therefore, selecting the appropriate annealing temperature and holding time to achieve the desired stress relief results is challenging.
[0004] It is well known that residual stress causes strain in the atomic structure, thereby changing the work function that determines the surface properties of the material, which in turn affects the mechanical properties and corrosion resistance of the material. Studies have shown that residual compressive stress inhibits the occurrence of intergranular corrosion in alloys, thereby improving corrosion resistance. On the other hand, the change in grain orientation during annealing affects the stability and corrosion resistance of grain boundaries. For FCC metals, the corrosion rates of grains with different orientations are also different. The (100) crystal plane has the fastest corrosion rate, followed by the (111) crystal plane. The corrosion rates of the (110) crystal plane and the (331) crystal plane are almost the same. In addition, grain size, grain boundary type, the proportion of low ΣCSL grain boundaries in the grain boundary structure, and the connectivity of the random high-angle grain boundary network have an important influence on corrosion performance. Summary of the Invention
[0005] The main purpose of the present invention is to overcome the shortcomings of the existing technology and solve the technical problem of balancing the strength and electrical conductivity of copper alloy strips while effectively reducing their residual stress and improving their etching performance. The present invention provides a heat treatment process for eliminating the residual stress of copper alloy strips. By optimizing the pre-etching heat treatment process, a copper alloy strip with excellent performance is prepared, providing a reference for breakthroughs in the manufacturing technology of copper alloy strips for high-precision etching lead frames required by integrated circuits and the development of the industry, and continuously improving the precision forming quality of copper alloy strips.
[0006] The present invention is achieved through the following technical solution: A heat treatment process for eliminating residual stress in a copper alloy thin strip comprises the following steps: S1. Online solution treatment: The copper alloy ingot is placed in a heating furnace and heated at a solution temperature of 900°C to 1000°C for 1h to 2h. During the online solution treatment, an inert gas is continuously introduced into the heating furnace to prevent oxidation of the copper alloy ingot. S2, hot rolling: hot rolling the copper alloy ingot after the online solution treatment in step S1 to produce a copper alloy slab with a thickness of 15 mm to 17 mm; S3, cold rolling and intermediate annealing: The copper alloy slab prepared in step S2 is cold rolled, with 15 to 20 cold rolling passes. When the copper alloy slab is cold rolled to a thickness of 1.6 mm to 2 mm, 0.8 mm to 1 mm, and 0.35 mm to 0.4 mm, intermediate annealing is repeated three times, each at a temperature of 450° C. to 550° C. and a holding time of less than 1 hour, to obtain a copper alloy strip having a thickness of 0.18 mm to 0.22 mm. Repeating intermediate annealing multiple times when the copper alloy slab is cold rolled to a specific thickness can reduce the hardness of the alloy, facilitating further cold rolling of the copper alloy slab in the next pass. S4, annealing: The copper alloy strip prepared in step S3 is reheated in the furnace for annealing at a heating rate of 5°C / min to 7°C / min, an annealing temperature of 380°C to 420°C, and a holding time of 1 min to 60 min. After annealing, the copper alloy strip is cooled in the furnace to room temperature to obtain a finished copper alloy strip with residual stress eliminated, which is then used as a raw material for the subsequent copper alloy lead frame etching process.
[0007] Furthermore, in step S2, the time interval between taking out the copper alloy ingot after the online solution treatment and sending it to the hot rolling cogging station does not exceed 30 seconds.
[0008] The beneficial effects of the present invention are: The present invention controls the strength of the internal structure of the alloy ribbon through a heat treatment process, thereby achieving the purpose of significantly reducing the residual stress. After testing, the residual stress value of the Cu-2.13Fe-0.026P (wt%) alloy ribbon is reduced to 23.1MPa after annealing. At this time, the texture strength of the alloy is the lowest, and its main texture Brass (011) <211> 、S(123) <634> 、Copper(112) <111> and Cube(001) <100> The texture strength value of the copper alloy strip is similar. Under the premise of ensuring good comprehensive properties such as strength, conductivity and etching performance of the copper alloy strip, the present invention greatly reduces the residual stress of the alloy, providing excellent raw material preparation for the subsequent copper alloy lead frame etching process. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 It is a process flow chart of the present invention; Figure 2 Polarization curves of the copper alloy strips prepared in Examples 1 to 5 and Comparative Example 1 in etching solution. DETAILED DESCRIPTION
[0010] The present invention will be described in further detail below with reference to the accompanying drawings and examples.
[0011] The copper alloy ingots in the following embodiments are all made of Cu-2.13Fe-0.026P (wt%) alloy. Example 1
[0012] like Figure 1 A heat treatment process for eliminating residual stress in a copper alloy thin strip is shown, comprising the following steps: S1. Online solution treatment: The copper alloy ingot is placed in a heating furnace and heated at a solution temperature of 1000°C for 1 hour. During the online solution treatment, an inert gas is continuously introduced into the heating furnace. S2. Hot rolling: The copper alloy ingot after the online solution treatment in step S1 is subjected to hot rolling. The time interval between taking out the copper alloy ingot after the online solution treatment and feeding it into the hot rolling station is no more than 30 seconds, and a copper alloy slab is produced. The thickness of the copper alloy slab is 16.5 mm. S3, cold rolling and intermediate annealing: The copper alloy slab prepared in step S2 is cold rolled in 16 passes. When the copper alloy slab is cold rolled to a thickness of 1.8 mm, 0.9 mm, and 0.37 mm, intermediate annealing is repeated three times, each at a temperature of 500° C. and a holding time of 30 min, to obtain a copper alloy strip having a thickness of 0.203 mm. S4, annealing: The copper alloy strip prepared in step S3 is reheated in the furnace for annealing at a heating rate of 7°C / min, an annealing temperature of 400°C, and a holding time of 1 minute. After annealing, the copper alloy strip is cooled in the furnace to room temperature to obtain a copper alloy strip product with residual stress eliminated. The residual stress is -118.7 MPa. Electron backscattered diffraction (EBSD) is used for detection, and the main texture is Brass (011). <211> 、S(123) <634> 、Copper(112) <111> and Cube(001) <100> The texture strength values are shown in Table 1. Example 2
[0013] like Figure 1 A heat treatment process for eliminating residual stress in a copper alloy thin strip is shown, comprising the following steps: S1. Online solution treatment: The copper alloy ingot is placed in a heating furnace and heated at a solution temperature of 1000°C for 1 hour. During the online solution treatment, an inert gas is continuously introduced into the heating furnace. S2. Hot rolling: The copper alloy ingot after the online solution treatment in step S1 is subjected to hot rolling. The time interval between taking out the copper alloy ingot after the online solution treatment and feeding it into the hot rolling station is no more than 30 seconds, and a copper alloy slab is produced. The thickness of the copper alloy slab is 16.5 mm. S3, cold rolling and intermediate annealing: The copper alloy slab prepared in step S2 is cold rolled in 16 passes. When the copper alloy slab is cold rolled to a thickness of 1.8 mm, 0.9 mm, and 0.37 mm, intermediate annealing is repeated three times, each at a temperature of 500° C. and a holding time of 30 min, to obtain a copper alloy strip having a thickness of 0.203 mm. S4, annealing: The copper alloy strip prepared in step S3 is reheated in the furnace for annealing at a heating rate of 7°C / min, an annealing temperature of 400°C, and a holding time of 5 min. After annealing, the copper alloy strip is cooled in the furnace to room temperature to obtain a copper alloy strip product with residual stress eliminated. The residual stress is -98.7 MPa. EBSD is used for detection, and the main texture Brass (011) is <211> 、S(123) <634> 、Copper(112) <111> and Cube(001) <100> The texture strength values are shown in Table 1. Example 3
[0014] like Figure 1 A heat treatment process for eliminating residual stress in a copper alloy thin strip is shown, comprising the following steps: S1. Online solution treatment: The copper alloy ingot is placed in a heating furnace and heated at a solution temperature of 1000°C for 1 hour. During the online solution treatment, an inert gas is continuously introduced into the heating furnace. S2. Hot rolling: The copper alloy ingot after the online solution treatment in step S1 is subjected to hot rolling. The time interval between taking out the copper alloy ingot after the online solution treatment and feeding it into the hot rolling station is no more than 30 seconds, and a copper alloy slab is produced. The thickness of the copper alloy slab is 16.5 mm. S3, cold rolling and intermediate annealing: The copper alloy slab prepared in step S2 is cold rolled in 16 passes. When the copper alloy slab is cold rolled to a thickness of 1.8 mm, 0.9 mm, and 0.37 mm, intermediate annealing is repeated three times, each at a temperature of 500° C. and a holding time of 30 min, to obtain a copper alloy strip having a thickness of 0.203 mm. S4, annealing: The copper alloy strip prepared in step S3 is reheated in the furnace for annealing at a heating rate of 7°C / min, an annealing temperature of 400°C, and a holding time of 10 min. After annealing, the copper alloy strip is cooled in the furnace to room temperature to obtain a copper alloy strip product with residual stress eliminated. The residual stress is -23.1 MPa. EBSD is used for detection, and the main texture Brass (011) is <211> 、S(123) <634> 、Copper(112) <111> and Cube(001) <100> The texture strength values are shown in Table 1. Example 4
[0015] like Figure 1 A heat treatment process for eliminating residual stress in a copper alloy thin strip is shown, comprising the following steps: S1. Online solution treatment: The copper alloy ingot is placed in a heating furnace and heated at a solution temperature of 1000°C for 1 hour. During the online solution treatment, an inert gas is continuously introduced into the heating furnace. S2. Hot rolling: The copper alloy ingot after the online solution treatment in step S1 is subjected to hot rolling. The time interval between taking out the copper alloy ingot after the online solution treatment and feeding it into the hot rolling station is no more than 30 seconds, and a copper alloy slab is produced. The thickness of the copper alloy slab is 16.5 mm. S3, cold rolling and intermediate annealing: The copper alloy slab prepared in step S2 is cold rolled in 16 passes. When the copper alloy slab is cold rolled to a thickness of 1.8 mm, 0.9 mm, and 0.37 mm, intermediate annealing is repeated three times, each at a temperature of 500° C. and a holding time of 30 min, to obtain a copper alloy strip having a thickness of 0.203 mm. S4, annealing: The copper alloy strip prepared in step S3 is reheated in the furnace for annealing at a heating rate of 7°C / min, an annealing temperature of 400°C, and a holding time of 30 min. After annealing, the copper alloy strip is cooled to room temperature in the furnace to obtain a copper alloy strip product with residual stress eliminated. The residual stress is 72.7 MPa. EBSD is used for detection, and the main texture Brass (011) is <211> 、S(123) <634> 、Copper(112) <111> and Cube(001) <100> The texture strength values are shown in Table 1. Example 5
[0016] like Figure 1 A heat treatment process for eliminating residual stress in a copper alloy thin strip is shown, comprising the following steps: S1. Online solution treatment: The copper alloy ingot is placed in a heating furnace and heated at a solution temperature of 1000°C for 1 hour. During the online solution treatment, an inert gas is continuously introduced into the heating furnace. S2. Hot rolling: The copper alloy ingot after the online solution treatment in step S1 is subjected to hot rolling. The time interval between taking out the copper alloy ingot after the online solution treatment and feeding it into the hot rolling station is no more than 30 seconds, and a copper alloy slab is produced. The thickness of the copper alloy slab is 16.5 mm. S3, cold rolling and intermediate annealing: The copper alloy slab prepared in step S2 is cold rolled in 16 passes. When the copper alloy slab is cold rolled to a thickness of 1.8 mm, 0.9 mm, and 0.37 mm, intermediate annealing is repeated three times, each at a temperature of 500° C. and a holding time of 30 min, to obtain a copper alloy strip having a thickness of 0.203 mm. S4, annealing: The copper alloy strip prepared in step S3 is reheated in the furnace for annealing at a heating rate of 7°C / min, an annealing temperature of 400°C, and a holding time of 60 min. After annealing, the copper alloy strip is cooled to room temperature in the furnace to obtain a copper alloy strip product with residual stress eliminated. The residual stress is -78.2 MPa. EBSD is used for detection, and the main texture Brass (011) is <211> 、S(123) <634> 、Copper(112) <111> and Cube(001) <100> The texture strength values are shown in Table 1. Comparative Example 1
[0017] A heat treatment process for eliminating residual stress in a copper alloy strip comprises the following steps: S1. Online solution treatment: The copper alloy ingot is placed in a heating furnace and heated at a solution temperature of 1000°C for 1 hour. During the online solution treatment, an inert gas is continuously introduced into the heating furnace. S2. Hot rolling: The copper alloy ingot after the online solution treatment in step S1 is subjected to hot rolling. The time interval between taking out the copper alloy ingot after the online solution treatment and feeding it into the hot rolling station is no more than 30 seconds, and a copper alloy slab is produced. The thickness of the copper alloy slab is 16.5 mm. S3, cold rolling and intermediate annealing: The copper alloy slab prepared in step S2 is cold rolled, with 16 cold rolling passes. When the copper alloy slab is cold rolled to a thickness of 1.8 mm, 0.9 mm, and 0.37 mm, intermediate annealing is repeated three times, each at a temperature of 500° C. and a holding time of 30 min, to obtain a copper alloy thin strip having a thickness of 0.203 mm. The copper alloy thin strip product with residual stress eliminated is obtained, and its residual stress is -144.9 MPa. EBSD is used for detection, and its main texture Brass (011) is obtained. <211> 、S(123) <634> 、Copper(112) <111> and Cube(001) <100> The texture strength values are shown in Table 1.
[0018] The texture strength values of the main textures of Examples 1-5 and Comparative Example 1 are shown in Table 1, and the hardness, conductivity, residual stress and electrochemical corrosion results of Examples 1-5 and Comparative Example 1 are shown in Table 2.
[0019]
[0020]
[0021] It can be seen from Table 1 that when the holding time of the annealing process in step S4 in Example 3 is controlled at 10 min, compared with the other examples, the maximum texture strength of the copper alloy thin strip product with residual stress eliminated obtained in Example 3 is the lowest, and the texture strength values of the main textures are close.
[0022] According to common knowledge, if the residual stress of the copper alloy strip is unevenly released, it is very easy to warp in the subsequent etching process. Therefore, it is necessary to reduce the residual stress of the alloy strip through a reasonable heat treatment process while ensuring the comprehensive performance of the alloy strip (a certain hardness, high electrical conductivity, and fast etching rate to reduce side corrosion and improve corrosion efficiency). It can be seen from Table 2 that when the holding time of the annealing process in step S4 of Example 3 is controlled at 10 minutes, compared with the other examples, the copper alloy strip product with residual stress eliminated obtained in Example 3 has a better comprehensive performance of hardness, electrical conductivity and etching performance, and significantly reduces the residual stress of the alloy. Figure 2 It can also be seen from the self-corrosion current density of the copper alloy thin strip products with residual stress eliminated prepared in various embodiments that the copper alloy thin strip product with residual stress eliminated prepared in Example 3 has higher etching performance.
[0023] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in the present invention should be included in the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection of the claims.
Claims
1. A heat treatment process for eliminating residual stress in a copper alloy strip, characterized in that: The following steps are involved: S1. Online solution treatment: The copper alloy ingot is placed in a heating furnace for heating. The solution temperature is 900°C to 1000°C and the holding time is 1h to 2h. During the online solution treatment, an inert gas is continuously introduced into the heating furnace. S2, hot rolling: hot rolling the copper alloy ingot after the online solution treatment in step S1 to obtain a copper alloy slab, the thickness of the copper alloy slab is 15 mm to 17 mm; S3, cold rolling and intermediate annealing: the copper alloy slab prepared in step S2 is cold rolled, the cold rolling passes are 15-20 passes, when the copper alloy slab is cold rolled to a thickness of 1.6 mm-2 mm, 0.8 mm-1 mm and 0.35 mm-0.4 mm, the intermediate annealing is repeated three times, each intermediate annealing temperature is 450° C.-550° C., the holding time is within 1 hour, and the copper alloy thin strip is obtained, and the thickness of the copper alloy thin strip is 0.18 mm-0.22 mm; S4, annealing: the copper alloy strip prepared in step S3 is reheated in the furnace for annealing, the heating rate is 5°C / min-7°C / min, the annealing temperature is 380°C-420°C, and the holding time is 1min-60min. After annealing, the copper alloy strip is cooled in the furnace to room temperature to obtain a copper alloy strip product with residual stress eliminated.
2. A heat treatment process for eliminating residual stress in a copper alloy thin strip according to claim 1, characterized in that: In the step S2, the time interval between taking out the copper alloy ingot after the online solution treatment and sending it to the hot rolling blanking station is no more than 30 seconds.