Magnesium alloy metallographic corrosive agent and preparation method and application thereof

By using a metallographic corrosive agent composed of nitric acid, acetic acid, anhydrous ethanol and deionized water, combined with electrochemical polishing technology, the difficulty in obtaining high-quality metallographic photos of non-rare earth magnesium alloys and deformed magnesium alloys in the existing technology is solved. problem, achieving the effect of preparing high-quality metallographic photos in a variety of magnesium alloys.

CN118726979APending Publication Date: 2024-10-01INSTITUTE OF MATERIALS & INTELLIGENT MANUFACTURING JIANGXI ACADEMY OF SCIENCES

Patent Information

Application Number
CN202410971453.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to obtain high-quality metallographic photos of non-rare earth magnesium alloys and deformed magnesium alloys with existing metallographic corrosive agents, which limits the application scope of magnesium alloys.

Method used

Use a metallographic etchant composed of nitric acid, acetic acid, absolute ethanol and deionized water. The volume ratio is 2%-5% nitric acid, 20%-30% acetic acid, 15%-30% absolute ethanol and 45%. %-60% deionized water, stir evenly and then use it on magnesium alloy samples, combined with electrochemical polishing technology to prepare high-quality metallographic photos.

Benefits of technology

This corrosive can produce high-quality metallographic photos in rare earth magnesium alloys, non-rare earth magnesium alloys, cast magnesium alloys and deformed magnesium alloys, expands the scope of use, and significantly improves the metallographic microscope observation effect of magnesium alloys. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726979A_ABST
    Figure CN118726979A_ABST
Patent Text Reader

Abstract

The invention discloses a magnesium alloy metallographic corrosive and a preparation method and application thereof, and belongs to the technical field of metallographic corrosion. The metallographic corrosive is composed of nitric acid, acetic acid, ethyl alcohol and deionized water, wherein the volume ratio of the nitric acid is 2%-5%, the volume ratio of the acetic acid is 20%-30%, the volume ratio of the ethyl alcohol is 15%-30%, and the volume ratio of the deionized water is 45%-60%. The metallographic corrosive can be used for different-state magnesium alloys such as rare earth magnesium alloys, non-rare earth magnesium alloys, as-cast magnesium alloys and deformed magnesium alloys, and high-quality metallographs are prepared, so that the relationship between the grain size and the mechanical property of a material is analyzed conveniently. Compared with the prior art, the method is suitable for more types of magnesium alloys, the application range is wider, and the success rate is higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallographic corrosion, and in particular relates to a magnesium alloy metallographic corrosive agent and a use method thereof. Background Art

[0002] Magnesium alloys have the characteristics of low density, high specific strength and specific stiffness, excellent damping and shock absorption performance and electromagnetic shielding performance. They are ideal lightweight materials in the fields of transportation. The low mechanical strength of magnesium alloys seriously hinders their widespread application. Grain refinement can effectively improve the strength of magnesium alloys. Therefore, it is necessary to observe the microstructure such as the grain size of magnesium alloys during the preparation and processing of magnesium alloys to analyze the influence of microstructure evolution on the mechanical properties of magnesium alloys. Metallographic microscope technology is simple to operate. Compared with scanning electron microscopes, metallographic microscopes have a significant advantage of low price and are one of the most widely used means in material research and inspection. Magnesium alloys are chemically active and are easily oxidized or corroded during mechanical grinding and corrosion, making it difficult to present high-quality metallographic structures. Previously, the metallographic etchants commonly used for magnesium alloys were a mixture of picric acid, glacial acetic acid, anhydrous ethanol and deionized water. Picric acid is difficult to be widely used. Patents with application numbers 202110363054.4 and 202210037722.9 disclose a rare earth magnesium alloy metallographic etchant and its application. However, it is difficult to obtain high-quality metallographic photographs in non-rare earth magnesium alloys and deformed magnesium alloys using the etchant. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the present invention provides a magnesium alloy phase etchant and a method for using the same. The metallographic etchant of the present invention can be used for magnesium alloys in different states such as rare earth magnesium alloys and non-rare earth magnesium alloys, cast magnesium alloys and deformed magnesium alloys to prepare high-quality metallographic photographs.

[0004] The present invention is achieved through the following technical solutions.

[0005] The magnesium alloy metallographic etching agent of the present invention comprises components: nitric acid, acetic acid, ethanol and deionized water, wherein the volume ratio of nitric acid is 2%-5%, the volume ratio of acetic acid is 20%-30%, the volume ratio of anhydrous ethanol is 15%-30%, and the volume ratio of deionized water is 45%-60%.

[0006] A method for preparing a magnesium alloy metallographic etching agent comprises the following steps.

[0007] (1) Take each solvent according to the volume ratio: 2%-5% nitric acid, 20%-30% acetic acid, 15%-30% anhydrous ethanol, and 45%-60% deionized water.

[0008] (2) First, mix anhydrous ethanol and deionized water, then add acetic acid to the mixed solution, and then add nitric acid to the mixed solution.

[0009] (3) Stir the mixed solution evenly with a glass rod to obtain a magnesium alloy metallographic etching agent.

[0010] The invention discloses an application of a magnesium alloy metallographic etching agent in the preparation of a magnesium alloy sample, comprising the following steps: slowly dripping the etching agent onto one side of the magnesium alloy sample to be corroded, washing the corroded surface of the sample with clean water every 10-15 seconds, then washing the corroded surface with alcohol, drying with hot air, and then observing the metallographic structure of the magnesium alloy through a metallographic microscope.

[0011] Furthermore, the application of the magnesium alloy metallographic etching agent in the preparation of magnesium alloy samples includes the following steps: first, coarse grinding is performed in running water using metallographic sandpaper with a particle size of 800 mesh, then fine grinding is performed using sandpapers with a particle size of 1200 mesh, 2000 mesh and 3000 mesh in sequence, and finally polishing is performed using an electrochemical polishing power supply, perchloric acid and alcohol polishing agent.

[0012] The volume ratio of perchloric acid to alcohol in the polishing agent is 4%-10%: 96%-90%, the electrolytic polishing temperature is -100°C-20°C, the polishing time is 60 seconds-150 seconds, and the polishing voltage is 20 V. After electrolytic polishing, rinse the polished surface with alcohol and blow dry with hot air.

[0013] Compared with the prior art, the beneficial effect of the present invention is that the metallographic etching agent of the present invention can be used for a variety of magnesium alloys, including rare earth magnesium alloys and non-rare earth magnesium alloys, cast magnesium alloys and deformed magnesium alloys and other magnesium alloys in different states, and has a wider range of use. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a photo of the microstructure after corrosion obtained in Example 1.

[0015] Figure 2 This is a photo of the microstructure after corrosion obtained in Example 2.

[0016] Figure 3 This is a photo of the microstructure after corrosion obtained in Example 3.

[0017] Figure 4 This is a photo of the microstructure after corrosion obtained in Example 1.

[0018] Figure 5 This is a photo of the microstructure after corrosion obtained in Example 2.

[0019] Figure 6 This is a photo of the microstructure after corrosion obtained in Example 3. DETAILED DESCRIPTION

[0020] The present invention will be further illustrated by the following examples. Example 1

[0021] A magnesium alloy metallographic etchant and a method for using the same include measuring each solvent according to volume ratio: 2% nitric acid, 20% acetic acid, 25% anhydrous ethanol, and 55% deionized water, mixing anhydrous ethanol and deionized water, then adding acetic acid to the mixed solution, and then adding nitric acid to the mixed solution. Finally, stirring the mixed solution evenly with a glass rod to obtain a magnesium alloy metallographic etchant. A small sample of AZ31 magnesium alloy rolled plate annealed at 400 degrees Celsius for 2 hours is cut by a wire cutting machine, with the size of 5 mm in thickness, 10 mm in length, and 8 mm in width. First, a metallographic sandpaper with a particle size of 800 mesh is used to coarsely grind the sample in running water, and then 1200 mesh, 2000 mesh, and 3000 mesh sandpaper are used in sequence for fine grinding, and finally, an electrochemical polishing power supply and a perchloric acid and alcohol polishing agent are used for polishing. The volume ratio of perchloric acid to alcohol in the polishing agent is 4%%: 96%, the electrolytic polishing temperature is about -80°C, the polishing time is 120 seconds, and the polishing voltage is 20V. After electrolytic polishing, rinse the polished surface with alcohol and blow dry with hot air. Slowly drip the corrosive agent onto one side of the magnesium alloy sample to be corroded, rinse the corroded surface of the sample with clean water every 10-15 seconds, then rinse the corroded surface with alcohol, blow dry with hot air, and then observe the metallographic structure of the magnesium alloy through a metallographic microscope. The obtained metallographic photo is as follows: Figure 1 As shown in Figure 1, the grain boundaries of the magnesium alloy are clearly observed. Example 2

[0022] A magnesium alloy metallographic etchant and a method for using the same include measuring each solvent according to the volume ratio: 2% nitric acid, 20% acetic acid, 25% anhydrous ethanol, and 55% deionized water, mixing anhydrous ethanol and deionized water, then adding acetic acid to the mixed solution, and then adding nitric acid to the mixed solution. Finally, stirring the mixed solution evenly with a glass rod to obtain a magnesium alloy metallographic etchant. A magnesium alloy sample with surface ultrasonic rolling is cut by a wire cutting machine, and the size is: thickness 4mm, length 10mm, width 6mm. First, a metallographic sandpaper with a particle size of 800 mesh is used to coarsely grind the sample in running water, and then 1200 mesh, 2000 mesh and 3000 mesh sandpaper are used in sequence for fine grinding, and finally, an electrochemical polishing power supply and a perchloric acid and alcohol polishing agent are used for polishing. The volume ratio of perchloric acid to alcohol in the polishing agent is 4%%: 96%, the electrolytic polishing temperature is about -80°C, the polishing time is 120 seconds, and the polishing voltage is 20V. After electrolytic polishing, the polished surface is rinsed with alcohol and dried with hot air. Slowly drip the corrosive agent onto one side of the magnesium alloy sample to be corroded, rinse the corroded surface of the sample with clean water every 10-15 seconds, then rinse the corroded surface with alcohol, blow dry with hot air, and then observe the metallographic structure of the magnesium alloy through a metallographic microscope. The obtained metallographic photo is as follows Figure 2In this figure, the grain boundaries and twin boundaries are clearly observed. Example 3

[0023] A magnesium alloy metallographic etchant and a method for using the same include measuring each solvent according to volume ratio: 2% nitric acid, 20% acetic acid, 25% anhydrous ethanol, and 55% deionized water, mixing the anhydrous ethanol and deionized water, then adding acetic acid to the mixed solution, and then adding nitric acid to the mixed solution. Finally, stirring the mixed solution evenly with a glass rod to obtain a magnesium alloy metallographic etchant. A small sample of a Mg-0.35at.%Y extruded rod annealed at 500 degrees Celsius for 2 hours is cut with a wire cutting machine, the size of which is: 3mm in thickness, 16mm in diameter, and 8mm in width. First, the sample is coarsely ground in running water with metallographic sandpaper with a particle size of 800 mesh, then finely ground with sandpapers of 1200 mesh, 2000 mesh, and 3000 mesh in sequence, and finally polished with an electrochemical polishing power supply, perchloric acid, and an alcohol polishing agent. The volume ratio of perchloric acid and alcohol in the polishing agent is 4%%: 96%, the electrolytic polishing temperature is about -80°C, the polishing time is 120 seconds, and the polishing voltage is 20V. After electrolytic polishing, rinse the polished surface with alcohol and blow dry with hot air. Slowly drip the corrosive agent onto one side of the magnesium alloy sample to be corroded, rinse the corroded surface of the sample with clean water every 10-15 seconds, then rinse the corroded surface with alcohol, blow dry with hot air, and then observe the metallographic structure of the magnesium alloy through a metallographic microscope. The obtained metallographic photograph is as follows: Figure 1 As shown in Figure 1, the grain boundaries of the magnesium alloy are clearly observed.

[0024] Comparative example 1.

[0025] In order to compare the effects of the present invention with the existing magnesium alloy metallographic preparation methods, the magnesium alloy metallographic prepared by the method given in the patent (a magnesium alloy metallographic etchant, application number: 201510476698.9) in comparative example 1.

[0026] Take 2 parts of nitric acid with a mass percentage concentration of 68%, 3 parts of acetic acid with a mass percentage concentration of 98%, and 100 parts of ethanol; the amount of oxalic acid is 12g of oxalic acid per 100mL of ethanol. A small sample of Mg-0.35at.%Y extruded rod annealed at 500 degrees Celsius for 2 hours was cut using a wire cutting machine, with the size of 3mm thickness, 16mm diameter, and 8mm width. First, a metallographic sandpaper with a particle size of 800 mesh was used to coarsely grind the sample in running water, and then 1200 mesh, 2000 mesh, and 3000 mesh sandpaper were used for fine grinding in sequence, and finally, an electrochemical polishing power supply and perchloric acid and alcohol polishing agent were used for polishing. The volume ratio of perchloric acid to alcohol in the polishing agent is 4%: 96%, the electrolytic polishing temperature is about -80°C, the polishing time is 120 seconds, and the polishing voltage is 20V. After electrolytic polishing, the polished surface is rinsed with alcohol and blown dry with hot air. Slowly drip the corrosive agent onto one side of the magnesium alloy sample to be corroded, rinse the corroded surface of the sample with clean water every 10-15 seconds, then rinse the corroded surface with alcohol, blow dry with hot air, and then observe the metallographic structure of the magnesium alloy through a metallographic microscope. The obtained metallographic photo is as follows Figure 4 As shown. There are a lot of black spots and the corrosion effect is poor.

[0027] Comparative example 2.

[0028] In order to compare the effects of the present invention with the existing magnesium alloy metallographic preparation methods, the magnesium alloy metallographic prepared by the method provided in the patent (a rare earth magnesium alloy metallographic etchant and a method for preparing a metallographic sample thereof, application number: 202210037722.9) in comparative example 2.

[0029] Take 1 part of nitric acid, 1 part of glacial acetic acid, and 98 parts of deionized water; each 100ml of the mixed solvent formed by nitric acid, glacial acetic acid and deionized water contains 1g of oxalic acid. A small sample of AZ31 magnesium alloy rolled plate annealed at 400 degrees Celsius for 2 hours was cut using a wire cutting machine, with the size of 5mm thickness, 10mm length, and 8mm width. First, a metallographic sandpaper with a particle size of 800 mesh was used to coarsely grind the sample in running water, and then 1200 mesh, 2000 mesh and 3000 mesh sandpaper were used for fine grinding in sequence, and finally, an electrochemical polishing power supply and perchloric acid and alcohol polishing agent were used for polishing. The volume ratio of perchloric acid to alcohol in the polishing agent is 4%: 96%, the electrolytic polishing temperature is about -80°C, the polishing time is 120 seconds, and the polishing voltage is 20V. After electrolytic polishing, the polished surface is rinsed with alcohol and blown dry with hot air. Slowly drip the corrosive agent onto one side of the magnesium alloy sample to be corroded, rinse the corroded surface of the sample with clean water every 10-15 seconds, then rinse the corroded surface with alcohol, blow dry with hot air, and then observe the metallographic structure of the magnesium alloy through a metallographic microscope. The obtained metallographic photo is as follows Figure 5 It is difficult to observe the cleaned grain boundaries in this figure.

[0030] Comparative example 3.

[0031] In order to compare the effects of the present invention with the existing magnesium alloy metallographic preparation methods, the magnesium alloy metallographic prepared by the method provided in the patent (A rare earth magnesium alloy metallographic etchant and its application, application number: 202110363054.4) in Example 3 is used.

[0032] Take 3.5g potassium chloride, 9g boric acid, 20ml glycerol, 60ml anhydrous ethanol, and 20ml distilled water. A small sample of AZ31 magnesium alloy rolled plate annealed at 400 degrees Celsius for 2 hours was cut using a wire cutting machine, with the size of 5mm thickness, 10mm length, and 8mm width. First, a metallographic sandpaper with a particle size of 800 mesh was used to coarsely grind the sample in running water, and then 1200 mesh, 2000 mesh, and 3000 mesh sandpaper were used for fine grinding in sequence, and finally, an electrochemical polishing power supply and perchloric acid and alcohol polishing agent were used for polishing. The volume ratio of perchloric acid to alcohol in the polishing agent is 4%: 96%, the electrolytic polishing temperature is about -80°C, the polishing time is 120 seconds, and the polishing voltage is 20V. After electrolytic polishing, the polished surface is rinsed with alcohol and dried with hot air. Slowly drip the corrosive agent onto one side of the magnesium alloy sample to be corroded, rinse the corroded surface of the sample with clean water every 10-15 seconds, then rinse the corroded surface with alcohol, blow dry with hot air, and then observe the metallographic structure of the magnesium alloy through a metallographic microscope. The obtained metallographic photo is as follows Figure 6 It is difficult to observe the cleaned grain boundaries in this figure.

Claims

1. A magnesium alloy metallographic etchant, characterized in that The components include: nitric acid, acetic acid, ethanol and deionized water, wherein the volume ratio of nitric acid is 2%-5%, the volume ratio of acetic acid is 20%-30%, the volume ratio of anhydrous ethanol is 15%-30%, and the volume ratio of deionized water is 45%-60%.

2. The method for preparing a magnesium alloy metallographic etchant according to claim 1, characterized in that The following steps are involved: (1) Take each solvent according to the volume ratio: 2%-5% nitric acid, 20%-30% acetic acid, 15%-30% anhydrous ethanol, and 45%-60% deionized water; (2) firstly mix anhydrous ethanol and deionized water, then add acetic acid to the mixed solution, and then add nitric acid to the mixed solution; (3) Stir the mixed solution evenly with a glass rod to obtain a magnesium alloy metallographic etching agent.

3. The use of a magnesium alloy metallographic etching agent according to claim 1 in the preparation of magnesium alloy samples, characterized in that The following steps are involved: Slowly drip the corrosive agent onto one side of the magnesium alloy sample to be corroded, rinse the corroded surface of the sample with clean water every 10-15 seconds, then rinse the corroded surface with alcohol, blow dry with hot air, and then observe the metallographic structure of the magnesium alloy through a metallographic microscope.

4. The use of a magnesium alloy metallographic etching agent in the preparation of magnesium alloy samples according to claim 3, characterized in that The following steps are involved: First, the metallographic sandpaper with a particle size of 800 mesh is used for coarse grinding in running water, and then the sandpaper with a particle size of 1200 mesh, 2000 mesh and 3000 mesh is used for fine grinding in sequence, and finally the electrochemical polishing power supply, perchloric acid and alcohol polishing agent are used for polishing; The volume ratio of perchloric acid to alcohol in the polishing agent is 4%-10%: 96%-90%, the electrolytic polishing temperature is -100°C-20°C, the polishing time is 60 seconds-150 seconds, and the polishing voltage is 20V; after electrolytic polishing, the polished surface is rinsed with alcohol and blown dry with hot air.

Citation Information

Patent Citations

  • Film forming treatment agent for composite chemical conversion film for magnesium alloy, and film forming process

    US20180363145A1

Cited By

  • Corrosion method of super invar alloy

    CN121163995A

  • A method of corrosion of a superinvar alloy