Low-hydrogen embrittlement cadmium plating method for spring parts
Through the low hydrogen embrittlement cadmium plating method, including pre-plating treatment, ultrasonic degreasing, anodic electrolytic degreasing and weak corrosion treatment, the problem of hydrogen embrittlement fracture of spring parts after cadmium plating has been solved, and the hydrogen content has been reduced and improved. Surface protection ensures the safety performance and durability of the material.
Patent Information
- Application Number
- CN202410899869.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
AI Technical Summary
Spring parts are prone to hydrogen absorption during the cadmium plating process, leading to hydrogen embrittlement and fracture, affecting safety performance. Especially in marine environments, corrosion resistance is poor. Commonly used cadmium plating processes have hydrogen absorption effects, which are difficult to effectively solve.
Adopt low hydrogen embrittlement cadmium plating method, including pre-plating treatment, ultrasonic degreasing, anodic electrolytic degreasing, weak corrosion treatment, electroplating cadmium, hydrogen removal, passivation and aging. Strictly control the electroplating cadmium time and hydrogen content. Through multiple Secondary water washing and blow-drying operations, combined with bending tests before and after plating, to ensure that the hydrogen content is within a safe range.
It effectively reduces the hydrogen content of spring parts during the cadmium plating process, avoids hydrogen embrittlement fracture, improves the safety performance and surface protection of the material, and extends the service life of the parts.
Smart Images

Figure CN118727073A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chromium plating of spring parts, and in particular relates to a method for low-hydrogen embrittlement cadmium plating of spring parts. Background Art
[0002] The materials of spring parts are usually 50CrVA, 65Mn, 70Mn, etc., and their strength is about 1000MPa. They are high-strength steel parts, sensitive to hydrogen embrittlement, and prone to hydrogen embrittlement fracture. However, the corrosion resistance of this material is poor. When used in a marine environment, the surface is very easy to rust, resulting in a decrease in material performance. In order to improve the surface protection, the design requires electroplating a layer of metal cadmium protective layer on the surface of the parts to improve the corrosion resistance of the surface of the parts. In the actual production process, since the commonly used cadmium plating process methods will produce hydrogen absorption in the degreasing, strong corrosion, and cadmium plating steps, it is easy to cause spring parts to absorb more hydrogen during the cadmium plating process. Since spring parts are high-strength steel parts, they are extremely sensitive to hydrogen embrittlement. There have been many cases of spring parts being cadmium-plated and hydrogen embrittled during use, causing extremely serious accidents.
[0003] In order to improve the surface protection of spring parts during use in the marine environment, a metal cadmium protective layer must be electroplated on the surface. However, the current cadmium plating process is likely to lead to increased material inhalation. To solve this problem, it is necessary to design a low hydrogen embrittlement cadmium plating process method to reduce the hydrogen content of spring materials during the cadmium plating process, thereby avoiding hydrogen embrittlement and fracture of spring parts after cadmium plating, so as to improve the safety performance of the material.
[0004] By searching domestic and foreign patent literature and paper databases, and conducting patent inquiries, three related patents were found, namely: 1. Patent number: CN108164031A, patent name: A method for treating potassium chloride cyanide-free cadmium plating wastewater. This patent mainly involves a method for treating cyanide-free cadmium plating wastewater, and does not involve a low-hydrogen embrittlement cadmium plating process. 2. Patent number: CN103898493A, patent name: A brush-coated cadmium passivation solution and its preparation and passivation method. This patent mainly involves a brush-coated cadmium passivation solution and its preparation and passivation method, and does not involve a low-hydrogen embrittlement cadmium plating process. 3. Patent number: CN201510861878.9, patent name: A method for electro-cadmium plating with a high-thickness cadmium coating. This patent mainly involves an electro-cadmium plating method with a high-thickness cadmium coating, and does not involve a low-hydrogen embrittlement cadmium plating process. Summary of the invention
[0005] The invention provides a method for low hydrogen embrittlement cadmium plating of spring parts, which solves the problem of hydrogen embrittlement fracture of spring parts after cadmium plating.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for low hydrogen embrittlement cadmium plating of spring parts, comprising:
[0008] Spring parts are treated before plating and then ultrasonically degreased after treatment;
[0009] Eliminate stress on degreased parts, then perform bending tests and anodic electrolytic degreasing;
[0010] Wash the parts twice after degreasing, and then perform water film inspection after washing. Perform weak corrosion treatment on the parts that pass the water film inspection, and then perform dust removal after weak corrosion treatment;
[0011] The parts after dust removal are subjected to cadmium electroplating, third water washing, drying, hydrogen removal, activation, fourth water washing, passivation, aging, fifth water washing and drying.
[0012] The parts after the blow-drying operation are subjected to a post-plating bending test, and the parts that pass the test are subjected to a performance test, and the parts that pass the performance test are put into storage.
[0013] Preferably, the pre-plating treatment of the spring parts is specifically to grind the surface of the spring parts to be smooth and free of black spots.
[0014] Preferably, the ultrasonic degreasing time is 10-30 min.
[0015] Preferably, the temperature for eliminating stress of the degreased parts is 200±10° C., and the stress elimination time is ≥2 hours.
[0016] Preferably, the anode electrolytic degreasing temperature is 60-80°C and the time is 5-10 minutes.
[0017] Preferably, two water washings are performed sequentially, the first water washing temperature is 60-90°C, the water washing time is 0.5-2 min, and the second water washing is a water washing at room temperature for 0.5-2 min.
[0018] Preferably, a part that passes the water film inspection is one that maintains a continuous thin water film for at least 10 seconds.
[0019] Preferably, the weak corrosion treatment time is 0.5-2 minutes, and the dust removal time is 2-5 minutes.
[0020] Preferably, the third water washing, the fourth water washing and the fifth water washing are all washed at room temperature for 0.5-2 min.
[0021] Preferably, the dehydrogenation operation is carried out within 4 hours of drying the parts, the dehydrogenation temperature is 200±10°C, the dehydrogenation time is at least 8 hours, the activation time is 5-10 seconds, the passivation time is 3-5 seconds, and the aging time is 4-6 seconds.
[0022] Compared with the prior art, the present invention has the following beneficial effects: the present invention provides a method for low hydrogen embrittlement cadmium plating of spring parts. In order to reduce the hydrogen content of spring parts in the cadmium electroplating process, the present invention has two methods for electrolytic degreasing, namely, anodic degreasing and cathodic degreasing. Since there is a risk of hydrogen absorption in the parts when only the cathode is degreased, the spring parts are not allowed to undergo cathode degreasing, and anodic degreasing is required. In order to avoid a large increase in hydrogen content in spring parts during the strong corrosion process, weak corrosion and dust removal steps are designed to replace the strong corrosion steps of the conventional cadmium electroplating process. In the cadmium plating step, the cadmium plating time determines the amount of hydrogen absorption. In order to avoid an excessively long cadmium electroplating time, which results in an increase in hydrogen absorption, the cadmium electroplating time is required to be strictly controlled during the cadmium electroplating process. The power is turned off every two minutes to measure the thickness. If the thickness does not meet the requirements, the power is turned on to continue the cadmium electroplating until the thickness meets the requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The present invention is a flow chart of a method for low hydrogen embrittlement cadmium plating of spring parts. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0025] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0027] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0028] In addition, if the term "horizontal" appears, it does not mean that the component must be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0029] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.
[0031] like Figure 1 The present invention provides a method for low hydrogen embrittlement cadmium plating of spring parts, comprising:
[0032] S101 performs pre-plating treatment on spring parts and ultrasonic degreasing after treatment;
[0033] The specific pre-plating treatment for spring parts is to grind the surface of spring parts to be smooth and free of black spots. Special pre-plating inspection and ultrasonic degreasing are added for spring parts. It is required that for spring parts, the surface should be smooth and free of black spots before processing. Minor black spots can be removed by polishing with a scouring pad. At the same time, for spring parts, it is necessary to increase the degreasing in the ultrasonic degreasing tank for 10 to 30 minutes.
[0034] S102 eliminates stress on degreased parts, then conducts bending tests and anodic electrolytic degreasing;
[0035] The temperature for eliminating stress of parts after degreasing is 200±10℃, and the stress elimination time is ≥2 hours. The temperature of anodic electrolytic degreasing is 60-80℃, and the time is 5-10min.
[0036] S103 washes the parts after degreasing twice, performs water film inspection after washing, performs weak corrosion treatment on the parts that pass the water film inspection, and performs dust removal treatment after the weak corrosion treatment;
[0037] The first washing is carried out at a temperature of 60-90°C for 0.5-2 minutes, and the second washing is carried out at room temperature for 0.5-2 minutes. The parts that pass the water film inspection are those that maintain a continuous thin water film for at least 10 seconds, the weak corrosion treatment time is 0.5-2 minutes, and the dust removal time is 2 to 5 minutes.
[0038] S104 performs cadmium electroplating, a third water washing, drying, dehydrogenation, activation, a fourth water washing, passivation, aging, a fifth water washing and drying on the parts after the dust removal treatment;
[0039] S105 performs a post-plating bending test on the parts after the blow-drying operation, performs a performance test on the parts that pass the test, and puts the parts that pass the performance test into storage.
[0040] The third, fourth and fifth washings were all performed at room temperature for 0.5-2 min.
[0041] The dehydrogenation operation is carried out within 4 hours of drying the parts. The dehydrogenation temperature is 200±10℃, the dehydrogenation time is at least 8h, the activation time is 5-10s, the passivation time is 3-5s, and the aging time is 4-6s.
[0042] The overall process is divided into the following steps:
[0043] 1 Acceptance before plating → 2 Ultrasonic degreasing → 3 Stress relief → 4 Bending test before plating → 5 Anodic electrolytic degreasing → 6 Hot water washing → 7 Cold water washing → 8 Water film inspection → 9 Weak corrosion → 10 Dust removal → 11 Cold water washing → 12 Cadmium electroplating → 13 Cold water washing → 14 Blow dry → 15 Hydrogen removal → 16 Activation → 17 Cold water washing → 18 Passivation → 19 Aging → 20 Cold water washing → 21 Blow dry → 22 Bending test after plating → 23 Inspection → 24 Warehousing
[0044] 1. Acceptance before plating: For spring parts, the surface should be smooth and free of black spots. Minor black spots can be removed by polishing with a scouring pad.
[0045] 2 Ultrasonic degreasing: For spring parts, it is necessary to add 10 to 30 minutes of degreasing in the ultrasonic degreasing tank.
[0046] 3 Stress relief: temperature 200±10℃, time ≥2 hours.
[0047] 4 Bending test before plating: For spring parts, a bending test before plating is required. Three hydrogen embrittlement specimens from the same material batch are used for the bending test before plating. The test is qualified if there is no brittle fracture of the substrate at the bending part during the bending test. The hydrogen content of the spring before cadmium plating is controlled through the bending test.
[0048] 5 Anodic electrolytic degreasing: For spring parts, cathodic degreasing is strictly prohibited. Anodic degreasing must be used at 60-80°C and the anodic electrolytic degreasing time is 5-10 minutes.
[0049] 6. Hot water washing: at 60-90℃, wash for 0.5-2min.
[0050] 7 Cold water wash: Wash with water at room temperature for 0.5 to 2 minutes.
[0051] 8 Water film inspection: Check the oil removal quality. A continuous thin water film should be maintained for at least 10 seconds to be qualified.
[0052] 9 Weak corrosion: In order to prevent spring parts from absorbing too much hydrogen in the strong corrosion tank, weak corrosion is used instead of strong corrosion for the activated surface state of spring parts, and it is required to be in the weak corrosion solution for 0.5 to 2 minutes.
[0053] 10 De-dusting: For spring parts, de-dusting should be performed at room temperature for 2 to 5 minutes after weak corrosion.
[0054] 11 Cold water wash: Wash with water at room temperature for 0.5 to 2 minutes.
[0055] 12 Cadmium electroplating: For spring parts, in order to avoid long cadmium plating time, which will lead to increased hydrogen absorption, the cadmium plating time must be strictly controlled during the cadmium plating process. It is required to cut off the power and measure the thickness every two minutes. If the thickness does not meet the requirements, the power will be turned on to continue cadmium plating until the thickness meets the requirements.
[0056] 13 Cold water wash: Wash with water at room temperature for 0.5 to 2 minutes.
[0057] 14 Blow dry: Blow dry with compressed air.
[0058] 15 Dehydrogenation: For spring parts, dehydrogenation should be carried out as soon as possible within 4 hours after cadmium plating. It is required to dehydrogenate for at least 8 hours at 200±10℃.
[0059] 16 Activation: Activate for 5 to 10 seconds at room temperature.
[0060] 17 Cold water wash: Wash with water at room temperature for 0.5 to 2 minutes.
[0061] 18. Passivation: Activate for 3 to 5 seconds at room temperature.
[0062] 19 Aging: Activate for 4 to 6 seconds at room temperature.
[0063] 20 Cold water wash: Wash with water at room temperature for 0.5 to 2 minutes.
[0064] 21 Blow dry: Blow dry with compressed air.
[0065] 22 Bending test after plating: For spring parts, a bending test after plating is required. Three hydrogen embrittlement specimens from the same material batch and parts are electroplated in the same tank and then subjected to a bending test after plating. The test is qualified if there is no brittle fracture of the substrate at the bending part during the bending test. The hydrogen content of springs after cadmium plating is controlled through the bending test.
[0066] 23 Inspection: Inspection of the appearance, thickness, bonding strength, hydrogen embrittlement and other performance of spring parts after cadmium electroplating.
[0067] 24 Warehouse entry: Qualified spring parts and oil seals are packed and warehoused
[0068] The advantages of the present invention are:
[0069] 1. A special low hydrogen embrittlement cadmium plating process suitable for spring parts has been developed to avoid hydrogen embrittlement fracture of spring parts due to a large increase in hydrogen content after using conventional cadmium plating methods.
[0070] 2. In the process of cadmium electroplating, the steps that are prone to hydrogen increase are electrolytic degreasing, strong corrosion, and cadmium plating. Conventional cadmium electroplating methods use mixed anode and cathode degreasing in electrolytic degreasing, use strong corrosion steps, and have no precise control over the cadmium plating time. Spring parts that use conventional cadmium electroplating are prone to a large increase in hydrogen content and hydrogen embrittlement fracture. Compared with the conventional cadmium electroplating method, in order to reduce the hydrogen content of spring parts during the cadmium electroplating process, the present invention has two methods for electrolytic degreasing, namely, anodic degreasing and cathodic degreasing. Since there is a risk of hydrogen absorption in parts when only the cathode is degreased, cathode degreasing is not allowed for spring parts, and anodic degreasing is required. For strong corrosion, in order to avoid a large increase in hydrogen content in spring parts during the strong corrosion process, weak corrosion and dust removal steps are designed to replace the strong corrosion step of the conventional cadmium electroplating process method. For the cadmium plating step, the cadmium plating time determines the amount of hydrogen absorption. In order to avoid an excessively long cadmium plating time, which leads to an increase in hydrogen absorption, the cadmium plating time is required to be strictly controlled during the cadmium plating process, and the power is turned off every two minutes to measure the thickness. If the thickness does not meet the requirements, the power is turned on to continue the cadmium plating until the thickness meets the requirements.
[0071] 3. In order to improve the quality of cadmium electroplating of spring parts, the present invention adds special pre-plating inspection and ultrasonic degreasing for spring parts. It is required that the surface of spring parts should be smooth and free of black spots before processing. Minor black spots can be removed by polishing with a scouring pad. At the same time, spring parts need to be degreased in an ultrasonic degreasing tank for 10 to 30 minutes.
[0072] 4. Compared with the conventional cadmium electroplating method, the present invention adds hydrogen embrittlement test before and after cadmium electroplating of spring parts. The bending test is carried out by using samples of the same batch of materials and the same slot processing process to test the hydrogen embrittlement of spring parts before and after cadmium electroplating. The bending test is qualified if there is no brittle fracture of the matrix at the bending part. The hydrogen content of the spring before and after cadmium electroplating is controlled by the bending test.
[0073] Although the embodiments of the present invention are described above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific embodiments and application fields, and the above-mentioned specific embodiments are only illustrative and instructive, rather than restrictive. Under the guidance of the specification, a person skilled in the art can also make many forms without departing from the scope of protection of the claims of the present invention, all of which belong to the scope of protection of the present invention.
Claims
1. A method for low hydrogen embrittlement cadmium plating of spring parts, characterized in that: include: Spring parts are treated before plating and then ultrasonically degreased after treatment; Eliminate stress on degreased parts, then perform bending tests and anodic electrolytic degreasing; Wash the parts twice after degreasing, and then perform water film inspection after washing. Perform weak corrosion treatment on the parts that pass the water film inspection, and then perform dust removal after weak corrosion treatment; The parts after dust removal are subjected to cadmium electroplating, third water washing, drying, hydrogen removal, activation, fourth water washing, passivation, aging, fifth water washing and drying. The parts after the blow-drying operation are subjected to a post-plating bending test, and the parts that pass the test are subjected to a performance test, and the parts that pass the performance test are put into storage.
2. The method for low hydrogen embrittlement cadmium plating of spring parts according to claim 1, characterized in that: The pre-plating treatment of spring parts is to polish the surface of spring parts to be smooth and free of black spots.
3. The method for low hydrogen embrittlement cadmium plating of spring parts according to claim 1, characterized in that: The ultrasonic degreasing time is 10-30min.
4. The method for low hydrogen embrittlement cadmium plating of spring parts according to claim 1, characterized in that: The temperature for eliminating stress of parts after degreasing is 200±10℃, and the stress elimination time is ≥2 hours.
5. The method for low hydrogen embrittlement cadmium plating of spring parts according to claim 1, characterized in that: The temperature of anode electrolytic degreasing is 60-80℃ and the time is 5-10min.
6. The method for low hydrogen embrittlement cadmium plating of spring parts according to claim 1, characterized in that: The two water washings are carried out in sequence, the first water washing temperature is 60-90°C, the water washing time is 0.5-2min, and the second water washing is carried out at room temperature for 0.5-2min.
7. The method for low hydrogen embrittlement cadmium plating of spring parts according to claim 1, characterized in that: Parts that pass the water film inspection are those that maintain a continuous thin water film for at least 10 seconds.
8. The method for low hydrogen embrittlement cadmium plating of spring parts according to claim 1, characterized in that: The weak corrosion treatment time is 0.5-2 minutes, and the dust removal time is 2 to 5 minutes.
9. The method for low hydrogen embrittlement cadmium plating of spring parts according to claim 1, characterized in that: The third, fourth and fifth washings were all performed at room temperature for 0.5-2 min.
10. The method for low hydrogen embrittlement cadmium plating of spring parts according to claim 1, characterized in that: The dehydrogenation operation is carried out within 4 hours of drying the parts. The dehydrogenation temperature is 200±10℃, the dehydrogenation time is at least 8h, the activation time is 5-10s, the passivation time is 3-5s, and the aging time is 4-6s.