Neodymium-doped silicate broadband near-infrared emission laser crystal and preparation method and application thereof
The neodymium-doped silicate material Y2Mg3(SiO4)3 is used to form a broadband near-infrared emitting laser crystal, which solves the quality and size limitations of the existing Nd3+-doped laser crystal during the growth process and achieves efficient light-to-light conversion efficiency. , has broad application prospects.
Patent Information
- Application Number
- CN202410861279.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to obtain high-quality, large-sized single crystals during the growth process of existing Nd3+-doped laser crystals, and the high symmetry of YAG brings a narrow spectral width, limiting its application in ultrafast laser output. In particular, there are high requirements on the linewidth and temperature dependence of the pump light source.
The neodymium-doped silicate material Y2Mg3(SiO4)3 is used as the laser crystal, and trivalent neodymium ions are added by replacing the Y lattice site to form ~1μm broadband near-infrared emission. Combined with the melt method for crystal growth, a multi-layer inert laser crystal is prepared. Sequential laser crystal.
It has achieved a peak height and full width of 31.62nm at 808nm, which is a good match for commercial GaAlAs semiconductor lasers, improves light-to-light conversion efficiency, and has important application prospects in the fields of medical treatment, transmission communications, and military defense.
Smart Images

Figure CN118727147A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of laser crystal gain materials, and in particular to a neodymium-doped silicate broadband near-infrared emitting laser crystal and a preparation method and application thereof. Background Art
[0002] At present, among the ultrafast laser crystals that can realize LD-pumped all-solid-state femtosecond laser output, Nd 3+ The doped laser crystal has rich energy levels and can achieve near-infrared laser output, which has attracted widespread attention. The specific reasons are as follows: (1) Nd 3+ The ions have an ideal four-level system and can achieve near-infrared luminescence at ~0.93μm, 1.08μm, and 1.35μm, corresponding to Nd 3+ Ionic 4 F 3 / 2 → 4 I 9 / 2 , 4 F 3 / 2 → 4 I 11 / 2 , 4 F 3 / 2 → 4 I 13 / 2 (2) The energy difference between the ground state and the excited state is about 2000cm -1 , has a lower laser threshold. (3) Nd 3+ The absorption peak at 808nm matches well with the emission wavelength of commercial GaAlAs semiconductor lasers and has high conversion efficiency. 3+ Doped laser crystal materials have been widely studied and applied, such as Nd:YAG for medium-average power lasers and Nd:YVO4 for low-power, miniaturized lasers. 3+ Doped laser crystals have been industrialized. However, the high symmetry of YAG leads to a narrow spectral width, which places high demands on the line width and temperature dependence of the pump light source. It is well known that a wider emission spectrum bandwidth is conducive to the realization of ultrashort pulses. However, due to the volatilization of raw material components during the growth process of YVO4 crystals, it is difficult to grow high-quality, large-sized single crystals. Therefore, it is necessary to further explore new femtosecond laser crystals with excellent comprehensive performance.
[0003] As one of the earliest studied laser crystal matrix materials, silicate materials with garnet structure are often used as matrix materials for solid laser gain media. They have a wide spectral coverage, high quantum efficiency, good luminescence performance, and abundant raw materials (especially SiO2). They are not easy to deliquesce, and have good chemical stability and thermal stability. With the continuous deepening of the exploration of silicate materials, the research on their luminescence properties has gradually developed from orthosilicates composed of a single cation to silicate materials with multiple cations and multiple disordered structures. The multiple disordered structures in Y2Mg3(SiO4)3(YMS) crystals give them a lower symmetry, which is conducive to the Starks energy level splitting of doped ions, enriching and broadening the spectrum, and is also conducive to lifting the parity ban and realizing polarized laser output. However, there is still a blank in the research on the luminescence performance of rare earth ion doped YMS single crystals at home and abroad. Therefore, in order to explore new laser gain medium materials with excellent performance, it is of great significance to study neodymium ion doped near-infrared laser crystal YMS. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a neodymium-doped silicate broadband near-infrared emission laser crystal and its preparation method and application. The trivalent neodymium ions in the laser crystal provided by the present invention are activated ions, replacing the lattice site of Y to form a broadband near-infrared emission of ~1μm. Figure 2 The absorption coefficient shown indicates that the peak height full width of the crystal at 808 nm reaches 31.62 nm, which means that it can be well matched with the emission wavelength of commercial GaAlAs semiconductor lasers to obtain higher light-to-light conversion efficiency.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a neodymium-doped silicate broadband near-infrared emitting laser crystal, the chemical formula of which is Nd x Y 2-x Mg3(SiO4)3, x is 0.001~0.03.
[0007] The present invention provides a method for preparing the laser crystal according to the above technical solution, comprising the following steps:
[0008] 1) Nd2O3, Y2O3, MgO and SiO2 are used as raw materials, and the ingredients are prepared and mixed according to the following chemical formula to obtain a mixed material;
[0009] 0.5xNd2O3+3MgO+0.5(2-x)Y2O3+3SiO2→Nd x Y 2-x Mg3(SiO4)3, x is 0.001 to 0.03;
[0010] 2) pressing and calcining the mixed material obtained in step 1) to obtain a calcined material;
[0011] 3) The calcined material obtained in step 2) is subjected to crystal growth by a melt method to obtain a laser crystal.
[0012] Preferably, the calcination conditions in step 2) include: a temperature of 1250 to 1400° C. and a time of 15 to 20 hours.
[0013] Preferably, the calcination temperature is 1300-1350° C. and the calcination time is 16 hours.
[0014] Preferably, the step 2) further comprises, after calcination, grinding, screening and pressing the calcined material, and then calcining to obtain a calcined material.
[0015] Preferably, the grinding conditions include: grinding in an agate mortar for 20 to 60 minutes;
[0016] The screening conditions include: using a standard sorting sieve with a particle size of 20 to 200 meshes to screen the ground powder, and pressing the sieve-down material.
[0017] Preferably, the melt method in step 3) comprises any one of a Czochralski method, a laser base heating method, a guided mold method, a pyrolysis method and a heat exchange method.
[0018] The present invention also provides the application of the laser crystal described in the above technical solution in one or more of spectroscopy, communication sensing, medical treatment and military defense.
[0019] Beneficial effects of the present invention:
[0020] The laser crystal provided by the present invention uses Y2Mg3(SiO4)3 with multiple disorders as the matrix and trivalent neodymium ions as the activation ions to replace the lattice site of Y to form a broadband near-infrared emission of ~1μm, which has important application prospects in the fields of medical treatment, transmission communication, military defense, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the embodiments are briefly introduced below.
[0022] Figure 1 Nd 3+ Ion energy level diagram;
[0023] Figure 2 is the absorption spectrum of Nd:YMS at 300-900nm, Nd 3+ After absorbing the incident energy, the ions change from the ground state to 4 I 9 / 2Excited to a higher energy level, there are seven absorption peaks in the range of 300-900nm as shown in the figure. 4 I 9 / 2 → 4 F 5 / 2 + 2 H 9 / 2 The transformed 790-810nm band has a more obvious absorption peak, which is consistent with the emission wavelength of 808nm of commercial AlGaAs semiconductor lasers, and the peak height full width of the crystal at 808nm reaches 31.62nm. It is well known that a wider absorption peak is conducive to improving pump efficiency and better matching the laser diode pump source. DETAILED DESCRIPTION
[0024] The present invention provides a neodymium-doped silicate broadband near-infrared emitting laser crystal, the chemical formula of which is Nd x Y 2-x Mg3(SiO4)3, x is 0.001~0.03.
[0025] The present invention provides a method for preparing the laser crystal according to the above technical solution, comprising the following steps:
[0026] 1) Nd2O3, Y2O3, MgO and SiO2 are used as raw materials, and the ingredients are prepared and mixed according to the following chemical formula to obtain a mixed material;
[0027] 0.5xNd2O3+3MgO+0.5(2-x)Y2O3+3SiO2→Nd x Y 2-x Mg3(SiO4)3, x is 0.001 to 0.03;
[0028] 2) pressing and calcining the mixed material obtained in step 1) to obtain a calcined material;
[0029] 3) The calcined material obtained in step 2) is subjected to crystal growth by a melt method to obtain a laser crystal.
[0030] The present invention uses Nd2O3, Y2O3, MgO and SiO2 as raw materials, and mixes them according to the following chemical formula to obtain a mixed material: 0.5xNd2O3+3MgO+0.5(2-x)Y2O3+3SiO2→Nd x Y 2-xMg3(SiO4)3, x is 0.001-0.03. In the present invention, the purity of the raw materials is 99.999%. In the present invention, the mixing conditions preferably include: putting the weighed raw material powder into a centrifuge tube that has been cleaned in advance, and then placing the centrifuge tube containing the raw material into a sealed box, or directly loading the raw material into the sealed box. Then fix the sealed box on the mixer, and the mixer moves alternately clockwise and counterclockwise for 24 hours to ensure uniform mixing.
[0031] The present invention presses and calcines the obtained mixed material to obtain a calcined material. In the present invention, the pressing conditions preferably include: first, the raw material is placed in a mold and pressed to make the raw material into a block. A hydraulic press can be used for initial pressing, then it is sealed, and further pressed with an isostatic press. In the present invention, the calcining conditions preferably include: a temperature of 1250 to 1400°C and a time of 15 to 20 hours. In the present invention, the calcining conditions also preferably include: a temperature of 1300 to 1350°C and a time of 16 hours. In the present invention, the calcining process also preferably includes: grinding, screening and pressing the calcined material, and then calcining to obtain a calcined material. After two calcinations, a sintered raw material with high mechanical strength and good density can be obtained. In the present invention, the grinding conditions preferably include: grinding in an agate mortar for 20 to 60 minutes. In the present invention, the screening conditions preferably include: using a standard sorting sieve with a particle size of 20 to 200 meshes to screen the ground powder, and pressing the material under the sieve.
[0032] The present invention uses a melt method to grow crystals from the obtained calcined material to obtain a laser crystal. In the present invention, the melt method preferably includes: any one of a Czochralski method, a laser base heating method, a guided mold method, a kypermeation method, and a heat exchange method. The present invention has no special limitation on the melt method, and those skilled in the art can use conventional methods.
[0033] The present invention also provides the application of the laser crystal described in the above technical solution in one or more of spectroscopy, communication sensing, medical treatment and military defense.
[0034] In order to further illustrate the present invention, the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0035] Example 1
[0036] Calculate the required mass of each raw material according to the chemical equation and weigh them accurately: 0.1595 g Nd2O3 (purity 99.999%), 2.2933 g MgO (purity 99.999%), 4.2721 g Y2O3 (purity 99.999%) and 3.4187 g SiO2 (purity 99.999%).
[0037] 0.5xNd2O3+3MgO+0.5(2-x)Y2O3+3SiO2→Nd x Y 2-x Mg3(SiO4)3, x is 0.001.
[0038] Then place the centrifuge tube containing the raw materials into a sealed box, and then fix the sealed box on the mixer. The mixer rotates clockwise and counterclockwise alternately for 24 hours to ensure uniform mixing. Use an acrylic mold with a hydraulic press to press the mixed sample into a cake shape, then put it into a muffle furnace and sinter it in an air atmosphere. The sintering temperature is 1250℃ and the sintering time is 20 hours to obtain the first sintered polycrystalline material. Then put it into an agate mortar and grind it thoroughly. Then use a standard sorting sieve to screen the ground powder (use a standard sorting sieve with a particle size of 200 mesh to screen the ground powder. The powder that does not pass the screening will be poured back into the agate mortar for further grinding and then screened). Then use a funnel and a glass rod to load these polycrystalline powders into a balloon with a diameter of 6mm. During this period, use a glass rod to initially compact it evenly, and finally seal the balloon. Then use a press to press the balloon filled with polycrystalline powder under high pressure, and sinter it again at 1250℃ for 20 hours to obtain the material rod required for growth.
[0039] The obtained material rod is polished to a diameter of 1.8 mm, and then the seed crystal (pure Y2Mg3(SiO4)3 crystal, seed crystal oriented to
[100] ) and the material rod are respectively fixed to the seed crystal pulling rod and the material rod feeding rod in the laser heating pedestal furnace, aligning them to the center of the laser beam circle and keeping them in the same vertical line. Close the furnace door, adjust the air pressure in the furnace, turn on the water cooler and CO2 laser, adjust the power to raise the temperature above the melting point to melt the material rod into a hemispherical shape. Then seed the crystal, set the appropriate pulling speed and material rod feeding speed, and start growing. When the growth process is over, the crystal is pulled out and cooled to room temperature at an annealing rate of 0.005W / h, and then the crystal Nd is taken out. 0.001 Y 1.999 Mg3(SiO4)3.
[0040] The absorption spectrum of the crystal in the wavelength range of 300-910 nm was recorded using a UV-visible-near infrared spectrophotometer (UV-3150) with a resolution of 1 nm. Figure 2 The absorption coefficient shown in Figure 2 shows that the peak height full width of the crystal at 808 nm reaches 31.62 nm, which means that it can be well matched with the emission wavelength of commercial GaAlAs semiconductor lasers to obtain higher light-to-light conversion efficiency.
[0041] Example 2
[0042] Calculate the required mass of each raw material according to the chemical equation and weigh them accurately: 0.0574 g Nd2O3 (purity 99.999%), 2.7490 g MgO (purity 99.999%), 5.0954 g Y2O3 (purity 99.999%) and 4.0981 g SiO2 (purity 99.999%).
[0043] 0.5xNd2O3+3MgO+0.5(2-x)Y2O3+3SiO2→Nd x Y 2-x Mg3(SiO4)3, x is 0.015.
[0044] Then place the centrifuge tube containing the raw materials into a sealed box, and then fix the sealed box on the mixer. The mixer rotates clockwise and counterclockwise alternately for 24 hours to ensure uniform mixing. Use an acrylic mold with a hydraulic press to press the mixed sample into a cake shape, then put it into a muffle furnace and sinter it in an air atmosphere. The sintering temperature is 1400℃ and the sintering time is 16 hours to obtain the first sintered polycrystalline material. Then put it into an agate mortar and grind it thoroughly. Then use a standard sorting sieve to screen the ground powder (use a standard sorting sieve with a particle size of 200 mesh to screen the ground powder. The powder that does not pass the screening will be poured back into the agate mortar for further grinding and then screened). Then use a funnel and a glass rod to load these polycrystalline powders into a balloon with a diameter of 7mm. During this period, use a glass rod to initially compact it evenly, and finally seal the balloon. Then use a press to press the balloon filled with polycrystalline powder under high pressure, and sinter it again at 1400℃ for 16 hours to obtain the material rod required for growth.
[0045] The obtained material rod is polished to a diameter of 1.9 mm, and then the seed crystal (pure Y2Mg3(SiO4)3 crystal, seed crystal oriented to
[100] ) and the material rod are respectively fixed to the seed crystal pulling rod and the material rod feeding rod in the laser heating pedestal furnace, aligning them to the center of the laser beam circle and keeping them in the same vertical line. Close the furnace door, adjust the air pressure in the furnace, turn on the water cooler and CO2 laser, adjust the power to raise the temperature above the melting point to melt the material rod into a hemispherical shape. Then seed the crystal, set the appropriate pulling speed and material rod feeding speed, and start growing. When the growth process is over, the crystal is pulled out and cooled to room temperature at an annealing rate of 0.10W / h, and then the crystal Nd is taken out. 0.015 Y 1.985 Mg3(SiO4)3.
[0046] Example 3
[0047] Calculate the required mass of each raw material according to the chemical equation and weigh them accurately: 0.0478 g Nd2O3 (purity 99.999%), 2.2909 g MgO (purity 99.999%), 4.2462 g Y2O3 (purity 99.999%) and 3.4151 g SiO2 (purity 99.999%).
[0048] 0.5xNd2O3+3MgO+0.5(2-x)Y2O3+3SiO2→Nd x Y 2-x Mg3(SiO4)3, x is 0.03.
[0049] Then place the centrifuge tube containing the raw materials into a sealed box, and then fix the sealed box on the mixer. The mixer rotates clockwise and counterclockwise alternately for 24 hours to ensure uniform mixing. Use an acrylic mold with a hydraulic press to press the mixed sample into a cake shape, then put it into a muffle furnace and sinter it in an air atmosphere. The sintering temperature is 1350℃ and the sintering time is 16 hours to obtain the first sintered polycrystalline material. Then put it into an agate mortar and grind it thoroughly. Then use a standard sorting sieve to screen the ground powder (use a standard sorting sieve with a particle size of 200 mesh to screen the ground powder. The powder that does not pass the screening will be poured back into the agate mortar for further grinding and then screened). Then use a funnel and a glass rod to load these polycrystalline powders into a balloon with a diameter of 6mm. During this period, use a glass rod to initially compact it evenly, and finally seal the balloon. Then use a press to press the balloon filled with polycrystalline powder under high pressure, and sinter it again at 1350℃ for 10 hours to obtain the material rod required for growth.
[0050] The obtained material rod is polished to a diameter of 1.7mm, and then the seed crystal (pure Y2Mg3(SiO4)3 crystal, seed crystal oriented to
[100] ) and the material rod are respectively fixed to the seed crystal pulling rod and the material rod feeding rod in the laser heating pedestal furnace, aligning them to the center of the laser beam circle and keeping them in the same vertical line. Close the furnace door, adjust the air pressure in the furnace, turn on the water cooler and CO2 laser, adjust the power to raise the temperature above the melting point to melt the material rod into a hemispherical shape. Then seed the crystal, set the appropriate pulling speed and material rod feeding speed, and start growing. When the growth process is over, the crystal is pulled out and cooled to room temperature at an annealing rate of 0.10W / h, and then the crystal Nd is taken out. 0.03 Y 1.97 Mg3(SiO4)3.
[0051] Example 4
[0052] Calculate the required mass of each raw material of Nd2O3 (purity of 99.999%), MgO (purity of 99.999%), Y2O3 (purity of 99.999%), and SiO2 (purity of 99.999%) according to the chemical equation and weigh them accurately.
[0053] 0.5xNd2O3+3MgO+0.5(2-x)Y2O3+3SiO2→Nd x Y 2-x Mg3(SiO4)3, x is 0.03.
[0054] Then put the prepared raw materials into a mixer to mix them evenly, and press the mixed sample into blocks and place them in a crucible. Then place the sample in a muffle furnace for calcination. The sintering temperature is 1300°C and the sintering time is 15 hours to obtain a sintered material. The obtained sintered material is placed in a pulling furnace, heated to 50°C above the melting point, completely melted, and kept at a constant temperature for 5 hours, and then the temperature is slowly lowered to the crystallization point for crystal growth. The pulling speed is 1.5mm / h and the rotation speed is 15rpm. When the growth process is over, the crystal is pulled out of the melt and cooled to room temperature at an annealing rate of 10°C / h, and then the crystal Nd is taken out. x Y 2-x Mg3(SiO4)3(x=0.03).
[0055] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A neodymium-doped silicate broadband near-infrared emitting laser crystal, characterized in that: The chemical formula of the laser crystal is Nd x Y 2-x Mg3(SiO4)3, x is 0.001~0.
03.
2. A method for preparing the laser crystal according to claim 1, characterized in that: The following steps are involved: 1) Nd2O3, Y2O3, MgO and SiO2 are used as raw materials, and the ingredients are prepared and mixed according to the following chemical formula to obtain a mixed material; 0.5xNd2O3+3MgO+0.5(2-x)Y2O3+3SiO2→Nd x Y 2-x Mg3(SiO4)3, x is 0.001 to 0.03; 2) pressing and calcining the mixed material obtained in step 1) to obtain a calcined material; 3) The calcined material obtained in step 2) is subjected to crystal growth by a melt method to obtain a laser crystal.
3. The preparation method according to claim 2, characterized in that: The calcination conditions in step 2) include: a temperature of 1250 to 1400° C. and a time of 15 to 20 hours.
4. The preparation method according to claim 3, characterized in that: The calcination temperature is 1300-1350° C. and the calcination time is 16 hours.
5. The preparation method according to claim 2, characterized in that: The step 2) further comprises, after calcination, grinding, screening and pressing the calcined material, and then calcining to obtain a calcined material.
6. The preparation method according to claim 5, characterized in that: The grinding conditions include: grinding in an agate mortar for 20 to 60 minutes; The screening conditions include: using a standard sorting sieve with a particle size of 20 to 200 meshes to screen the ground powder, and pressing the sieve-down material.
7. The preparation method according to claim 2, characterized in that: The melt method in step 3) includes any one of a Czochralski method, a laser base heating method, a guided mold method, a pyrolysis method and a heat exchange method.
8. Application of the laser crystal of claim 1 in one or more of spectroscopy, communication sensing, medical treatment and military defense.