Functional filler / sodium alginate composite fiber and preparation method thereof

By mixing functional fillers with sodium alginate aqueous solution and adding cross-linking agent dropwise, sodium alginate composite fibers are prepared, which solves the problems of single fiber and high cost in the existing technology, and realizes the introduction of silk core and diverse structures in the fiber. It is suitable for large-scale production and expands the functional applications of seaweed fiber.

CN118727196APending Publication Date: 2024-10-01NANKAI UNIV

Patent Information

Application Number
CN202410832905.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing preparation method of sodium alginate fiber has problems of simplicity and high cost. It is impossible to introduce silk core material into the fiber and prepare a complex 'skin-core' structure, which limits its functional expansion.

Method used

By mixing the functional filler with the sodium alginate aqueous solution, dripping a cross-linking agent on the surface, pulling it into filaments, and drying it, the functional filler/sodium alginate composite fiber is obtained, which achieves the introduction of silk core and structural diversity in the fiber.

Benefits of technology

This method simplifies the preparation process, reduces costs, is suitable for large-scale production, breaks through the limitations of single fiber components and structures, and expands the functions and applications of seaweed fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727196A_ABST
    Figure CN118727196A_ABST
Patent Text Reader

Abstract

The invention provides a functional filler / sodium alginate composite fiber and a preparation method thereof. The composite fiber is composed of a functional filler and a sodium alginate polymer, the preparation method comprises the following steps: firstly, dispersing the functional filler into a sodium alginate aqueous solution, dropwise adding a cross-linking agent aqueous solution on the surface, and then pulling into filaments, or embedding different filament cores into a functional filler / sodium alginate mixed solution, dropwise adding a cross-linking agent aqueous solution on the surface, pulling the filament cores and the solution together into filaments, and drying to obtain the functional filler / sodium alginate composite fiber. Through rapid interface crosslinking of the composite medium sodium alginate, preparation of the functional filler / sodium alginate composite fiber can be realized, and coating of the functional filler / sodium alginate on various silk cores can be further realized. The polymer matrix sodium alginate disclosed by the invention is wide in source, green and environment-friendly, and the preparation method is rapid, simple and universal, is suitable for various functional fillers / and various filament cores, is low in production cost, is suitable for continuous preparation, and is expected to be produced and used on a large scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a functional filler / sodium alginate composite fiber and a preparation method thereof. Background Art

[0002] As a new type of green biomass material, sodium alginate has the advantages of being non-toxic, biocompatible, widely available, and biodegradable. Sodium alginate fibers prepared from sodium alginate have great application potential in terms of moisture absorption, antibacterial, and radiation protection.

[0003] At present, the preparation methods of sodium alginate fiber mainly include wet spinning, electrostatic spinning, microfluidic spinning, etc. Wet spinning is to extrude the sodium alginate spinning solution first, prepare it into gel fiber through a coagulation bath, and then obtain the fiber by drying. This method has simple flow, low cost, and is easy to scale up production. It is one of the most common methods for preparing sodium alginate fiber. In addition to preparing pure sodium alginate fiber, the convenience of wet spinning can be further extended to the preparation of sodium alginate composite fiber. Prior art (such as the invention patent of publication number CN105926084A) combines rare earth ions into sodium alginate fiber by wet spinning to prepare functional fibers with catalytic properties. However, a large amount of coagulation bath solution is required during the wet spinning operation, and the fiber properties are greatly affected by the process. As emerging fiber preparation technologies, electrostatic spinning and microfluidic spinning are expensive and not suitable for large-scale production. In addition, existing wet spinning, electrospinning, microfluidic spinning and other technologies are limited to the production of sodium alginate fibers with a single homogeneous structure. It is impossible to introduce core materials into the fibers to prepare more complex "skin-core" structures, which limits their functional expansion. Summary of the invention

[0004] The purpose of the present invention is to overcome the singleness of the above sodium alginate fibers and the limitations of their preparation methods, and to provide a functional filler / sodium alginate composite fiber and its preparation method. The fiber is simple to prepare, universal, has low equipment requirements, and saves materials. The type and proportion of fillers in the fiber are flexible and adjustable, and a silk core can be introduced to form a "skin-core" structure, which greatly expands the functional application of sodium alginate fibers.

[0005] In order to solve the above technical problems, the technical solution of the present invention is as follows:

[0006] A functional filler / sodium alginate composite fiber and a preparation method thereof, characterized by comprising the following steps:

[0007] Step 1: Add a certain amount of functional filler to a sodium alginate aqueous solution of a certain concentration, mix by stirring, and obtain a uniform functional filler / sodium alginate mixed aqueous solution.

[0008] Step 2: In step 1, a certain concentration of cross-linking agent aqueous solution is added dropwise to the surface of the functional filler / sodium alginate mixed aqueous solution.

[0009] Step 3: pulling the mixed solution to which the cross-linking agent is added in step 2 into filaments.

[0010] Step 4: Drying the wet silk fibers obtained in step 3.

[0011] Furthermore, the concentration of sodium alginate in step 1 is 0.01% to 20%, preferably 0.1% to 5%, and more preferably 1% to 2.5%.

[0012] Furthermore, the ratio of the functional filler to sodium alginate in step 1 is adjusted within the range of 0:1 to 1:0.01.

[0013] Furthermore, the functional filler in step one is one or a mixture of two or more of a metal filler, a polymer filler, an inorganic non-metal filler, an MOFs filler, and a composite filler.

[0014] Furthermore, the cross-linking agent in step 2 is one or a mixture of two or more of calcium chloride, magnesium chloride, zinc chloride, aluminum chloride, calcium nitrate, magnesium nitrate, aluminum nitrate, zinc nitrate, and calcium sulfate, and the concentration is 0.01% to 20%, preferably 0.1% to 5%, and further preferably 1% to 2.5%.

[0015] Furthermore, the fiber core can be embedded in the functional filler / sodium alginate mixed aqueous solution before the crosslinking agent is added in step 2. Furthermore, the fiber core can be one or a mixture of two or more of metal fiber, polymer fiber, composite fiber, and carbon fiber.

[0016] Furthermore, in step three, if a fiber core is added in step two, the fiber core is pulled together with the solution.

[0017] Furthermore, the wet silk fiber drying method in step 4 is one or more of natural drying, oven drying, and freeze drying.

[0018] The beneficial effects of the present invention are:

[0019] Compared with the existing sodium alginate fiber preparation technology, the preparation method of the present invention is simpler, more universal, low-cost, and suitable for large-scale production: compared with the most common wet spinning method that requires the use of a large amount of coagulation bath, the preparation method of the present invention fully utilizes the materials by dripping a cross-linking agent on the surface, thus simplifying the preparation process. In addition, compared with electrospinning, microfluidic spinning and other technologies, this method is simpler and has low requirements for production equipment.

[0020] The functional filler / sodium alginate composite fiber of the present invention breaks through the limitation of single fiber component and structure prepared by traditional spinning technology. It provides an efficient and universal technology for introducing multiple functional fillers into fibers. The technology can also combine functional fibers with core materials to form a unique "skin-core" structure, further broadening the functions and applications of seaweed fibers. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The schematic diagram of the functional filler / sodium alginate composite fiber and the preparation method thereof is shown in the figure: 1. cross-linking agent; 2. functional filler; 3. sodium alginate; 4. fiber core.

[0022] Figure 2 This is a photo of the MOF-303 / sodium alginate (nickel-chromium metal wire core) composite fiber prepared in the present invention.

[0023] Figure 3 These are photos of MOF-303 / sodium alginate (wire-free core (a) and nickel-chromium metal wire core (b)) composite fibers prepared in the present invention.

[0024] Figure 4 The water absorption performance of the MOF-303 / sodium alginate (without silk core) composite fiber prepared by the present invention.

[0025] Figure 5 This is an infrared image of the electrically heated MOF-303 / sodium alginate (nickel-chromium metal wire core) composite fiber prepared in the present invention. DETAILED DESCRIPTION

[0026] The technical scheme of the present invention is described in detail below in conjunction with specific embodiments. The purpose of the examples listed is to explain the present invention and there is no limiting effect on the scope of the present invention. The raw materials and chemicals mentioned in each embodiment are commercially available products or prepared by publicly available methods.

[0027] Attached Figure 1 A schematic diagram of the functional filler / sodium alginate composite fiber and its preparation method of the present invention is given. The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0028] Embodiment 1:

[0029] (1) Add 1 g of MOF-303 to 25 ml of water and disperse thoroughly under ultrasonication for 20 min. Add 25 g of 2% sodium alginate solution and stir for 20 min to mix evenly to obtain a MOF-303 / sodium alginate solution.

[0030] (2) Add 2% calcium chloride aqueous solution dropwise on the surface of the above solution.

[0031] (3) The mixed solution to which calcium chloride has been dropped is pulled into filaments using tweezers.

[0032] (4) The wet silk fibers obtained above are naturally dried to obtain white fibers.

[0033] Embodiment 2:

[0034] (1) Add 1 g of MOF-303 to 18 ml of water and disperse thoroughly under ultrasonication for 20 min. Add 12.5 g of 2% sodium alginate solution and stir for 20 min to mix well to obtain a MOF-303 / sodium alginate solution.

[0035] (2) Add 2% calcium chloride aqueous solution dropwise on the surface of the above solution.

[0036] (3) The mixed solution to which calcium chloride has been dropped is pulled into filaments using tweezers.

[0037] (4) The wet silk fibers obtained above are naturally dried to obtain white fibers.

[0038] Embodiment 3:

[0039] (1) Add 1 g of MOF-303 to 18 ml of water and disperse thoroughly under ultrasonication for 20 min. Add 6 g of 2% sodium alginate solution and stir for 20 min to mix well to obtain a MOF-303 / sodium alginate solution.

[0040] (2) Add 2% calcium chloride aqueous solution dropwise on the surface of the above solution.

[0041] (3) The mixed solution to which calcium chloride has been dropped is pulled into filaments using tweezers.

[0042] (4) The wet silk fiber obtained above is naturally dried to obtain white fiber ( Figure 2 , with a diameter of about 300 μm ( Figure 3 a).

[0043] (5) The above white fiber is applied to the field of atmospheric water collection. The water adsorption performance under different humidity is as follows: Figure 4 shown.

[0044] Embodiment 4:

[0045] (1) Add 1 g of MOF-303 to 18 ml of water and disperse thoroughly under ultrasonication for 20 min. Add 6 g of 2% sodium alginate solution and stir for 20 min to mix well to obtain a MOF-303 / sodium alginate solution.

[0046] (2) A nickel-chromium wire with a diameter of 80 μm was placed inside the above solution, and a 2% calcium chloride aqueous solution was dripped onto the surface of the solution.

[0047] (3) The mixed solution to which calcium chloride has been dropped is pulled together with the nickel-chromium wire using tweezers to form a wire.

[0048] (4) The wet silk fibers obtained above were naturally dried to obtain white fibers containing a nickel-chromium metal wire core with a diameter of about 300 μm ( Figure 3 b).

[0049] (5) The white fiber containing the nickel-chromium metal wire core is electrically heated, and the heating effect is as follows: Figure 5 As shown, it can be used in the field of atmospheric water collection and air humidity control.

[0050] The above embodiments are only some embodiments of the present invention, not all embodiments, and the scope of the present invention shall be defined by the scope of protection required by the claims. Under the enlightenment of the present invention, any specific modification and transformation made by those skilled in the art based on the present invention shall be within the scope of protection required by the present invention.

Claims

1. A functional filler / sodium alginate composite fiber, characterized in that: The composite fiber consists of a functional filler and a sodium alginate polymer matrix, wherein the ratio of the functional filler to the sodium alginate is 0:1 to 1:0.

01.

2. The functional filler / sodium alginate composite fiber according to claim 1, characterized in that: The functional filler is one or more of a metal filler, a polymer filler, an inorganic non-metal filler, a metal-organic hybrid (MOFs) filler, and a composite filler.

3. The functional filler / sodium alginate composite fiber according to claim 1, characterized in that: A silk core is added or not added to the functional filler / sodium alginate composite fiber.

4. The functional filler / sodium alginate composite fiber according to claim 3, characterized in that: The wire core is one or more of metal fiber wire, polymer fiber wire, composite fiber wire and carbon fiber wire.

5. The method for preparing the functional filler / sodium alginate composite fiber according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) preparing a mixed aqueous solution of functional filler and sodium alginate; (2) adding a crosslinking agent to the surface of the functional filler / sodium alginate mixed solution in step (1); (3) pulling the mixed solution to which the crosslinking agent is added in step (2) into filaments; (4) Drying the wet silk fibers obtained in step (3).

6. The method for preparing the functional filler / sodium alginate composite fiber according to claim 5, characterized in that: In step (1), the concentration of sodium alginate is 0.01% to 20%, the ratio of functional filler to sodium alginate is 0:1 to 1:0.01, and the mixture is mixed by stirring for more than 1 minute.

7. The method for preparing the functional filler / sodium alginate composite fiber according to claim 5, characterized in that: In step (2), a silk core may or may not be added before the cross-linking agent is added, and the length of the added silk core below the solution interface is greater than 1 mm.

8. The method for preparing the functional filler / sodium alginate composite fiber according to claim 5, characterized in that: The cross-linking agent in step (2) is selected from one or more of calcium chloride, magnesium chloride, zinc chloride, aluminum chloride, calcium nitrate, magnesium nitrate, aluminum nitrate, zinc nitrate, and calcium sulfate, and the concentration is 0.01% to 20%.

9. The method for preparing the functional filler / sodium alginate composite fiber according to claim 5, characterized in that: The pulling angle in step (3) is 30-90° with the solution surface.

10. The method for preparing the functional filler / sodium alginate composite fiber according to claim 5, characterized in that: In step (3), the mixed solution to which the cross-linking agent is added is pulled together with the silk core into silk.

Citation Information

Patent Citations

  • Sodium alginate fiber catalytic material carrying rare earth ions and preparing method of sodium alginate fiber catalytic material

    CN105926084A

Cited By

  • Novel gas phase confinement method for batch preparation of alginate hydrogel fibers

    CN119663479A

  • A method for batch production of alginate hydrogel fibers by a novel gas-phase confinement method

    CN119663479B