An intrinsically hydrophilic and oleophobic nanofiber membrane and its preparation method and application
By electrospinning under ultraviolet light, the problem of low separation efficiency and short service life of emulsified oil-containing wastewater is solved, and the oil-water separation effect with high efficiency and long life is achieved.
Patent Information
- Application Number
- CN202411205406.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The prior art is difficult to efficiently separate and emulsify oil-containing wastewater, especially due to the adsorption and polymerization of oil droplets on the surface of the film or holes, resulting in membrane blockage, degradation of separation performance and short service life.
By electrospinning the mixture of functional monomers, photoinitiators and polymers under ultraviolet light, nanocellulose films with intrinsic hydrophilic and oleophobic properties are prepared, avoiding subsequent modification or coating treatment , simplifies the preparation process.
It achieves efficient oil-water separation efficiency, long service life, suitable for large-scale production, and the separation efficiency can reach 99.9%.
Smart Images

Figure CN118727272B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of nanocellulose membranes, and in particular to an intrinsically hydrophilic and oleophobic nanofiber membrane and a preparation method and application thereof. Background Art
[0002] Water pollution has always been one of the major problems facing the world today. Among them, a large amount of oily wastewater generated in daily life, industrial production and oil extraction processes seriously threatens human health and the ecological environment. Over the years, many studies have been devoted to the separation of oily wastewater, especially emulsified oily wastewater. However, due to the small size of oil droplets, high stability and complex separation process, efficient separation of emulsified oily wastewater is still challenging. With the development of bionic interfaces, the design of the wettability of membrane material interfaces has been achieved through the synergistic effect of surface chemical composition and morphology. At present, the special wetting materials commonly used for oil-water separation are mainly superhydrophobic-superoleophilic and superhydrophilic-superoleophilic membrane materials. However, due to the inherent superoleophilicity of the membrane, oil droplets are easily adsorbed, aggregated and adhered on the membrane surface or in the membrane pores during the separation of emulsified oily wastewater, causing blockage of the membrane surface and pores, resulting in decreased separation performance and shortened membrane life. The surface of an ideal emulsion separation membrane material should be able to repel oil stains and spontaneously remove oil stains under the action of water to avoid oil adhesion problems during use.
[0003] In recent years, researchers have successfully prepared hydrophilic-oleophobic surfaces by designing heterogeneous chemical surfaces composed of oleophobic components and hydrophilic components. This surface not only has selective wettability to oil and water, but also has oil repellency in the air. At the same time, it can achieve spontaneous underwater oil removal, and has good application prospects in the field of oil-water separation. However, since the heterogeneous chemical structure and component distribution of hydrophilic-oleophobic materials are difficult to control, and the introduction of too many hydrophilic components will inevitably increase the surface energy of the material, which inevitably makes it difficult to achieve hydrophilicity and oleophobicity at the same time, the preparation of hydrophilic-oleophobic porous membrane materials is relatively challenging.
[0004] At present, superhydrophilic-superoleophobic oil-water separation porous membrane materials are mainly obtained by superhydrophilic-superoleophobic modification of substrates, and the preparation methods mainly include chemical grafting and coating. Among them, the chemical grafting method has the disadvantages of complex preparation process and long time consumption. The surface coating of the material prepared by the coating method lacks effective bonding with the substrate, and the surface fastness of the material is poor. As an oil-water separation membrane, during use or cleaning, the superhydrophilic-superoleophobic component is easy to detach from the substrate surface, resulting in low oil-water separation efficiency and short service life.
[0005] Therefore, at this stage, there is an urgent need for a nanocellulose membrane with hydrophilic and oleophobic properties that has a simple preparation method, a rapid preparation process, a long service life, and high oil-water separation efficiency. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide an intrinsically hydrophilic and oleophobic nanofiber membrane and a preparation method and application thereof; the present invention electrospins an electrospinning mixture containing specific functional monomers and polymers under ultraviolet light in a one-step process to obtain a nanocellulose membrane with hydrophilic and oleophobic properties, without the need for further modification or post-treatment such as coating to obtain a separation membrane with hydrophilic and oleophobic functions; the preparation process is simple, the chemical reaction is rapid, and it is suitable for mass production and preparation, and the prepared nanocellulose membrane has high separation efficiency for oil-water mixtures.
[0007] In order to solve the above technical problems, the first aspect of the present invention is to provide a method for preparing an intrinsically hydrophilic and oleophobic nanofiber membrane, which specifically comprises the following steps:
[0008] S1. In a light-proof environment, a functional monomer, a photoinitiator and a polymer are mixed in an organic solvent to obtain an electrospinning mixture;
[0009] The functional monomers include a hydrophilic monomer, an oleophobic monomer and a cross-linking agent;
[0010] The cross-linking agent is a cross-linking agent containing carbon-carbon double bonds and / or a cross-linking agent containing thiol groups;
[0011] The cross-linking agent containing carbon-carbon double bonds contains at least two carbon-carbon double bonds, and the cross-linking agent containing thiol groups contains at least two thiol groups;
[0012] When the cross-linking agent includes a cross-linking agent containing a carbon-carbon double bond, the hydrophilic monomer includes a hydrophilic monomer containing a thiol group, and the oleophobic monomer includes a fluoroalkyl oleophobic monomer containing a thiol group; when the cross-linking agent includes a cross-linking agent containing a thiol group, the hydrophilic monomer includes a hydrophilic monomer containing a carbon-carbon double bond, and the oleophobic monomer includes a fluoroalkyl oleophobic monomer containing a carbon-carbon double bond;
[0013] S2, setting electrospinning process parameters, spinning the electrospinning mixture prepared in step S1 under ultraviolet light to obtain the intrinsically hydrophilic and oleophobic nanofiber membrane.
[0014] Furthermore, in step S1, the hydrophilic monomer containing a thiol group is selected from compounds of the following general structural formula:
[0015] ;
[0016] Wherein, R is one of hydroxyl, carboxyl, amide, amino or aldehyde; t is any integer from 1 to 9;
[0017] The sulfhydryl-containing fluoroalkyl oleophobic monomer is selected from the following compounds of the general structural formula:
[0018] ;
[0019] Wherein, m is any integer from 1 to 5, and n is any integer from 3 to 9;
[0020] The cross-linking agent containing carbon-carbon double bonds is selected from one or more of polyethylene glycol diacrylate, N-carboxyethyl acrylamide, 3-(trimethoxysilyl)propyl-2-methyl-2-acrylate, pentaerythritol triallyl ether, triallyl isocyanurate, pentaerythritol tetraacrylate, polydipentaerythritol pentaacrylate, vinyl cage-type polysilsesquioxane and acrylate-based cage-type polysilsesquioxane (abbreviated as POSS acrylate);
[0021] When the functional monomer includes a hydrophilic monomer containing a thiol group, a fluoroalkyl oleophobic monomer containing a thiol group, and a cross-linking agent containing a carbon-carbon double bond, the molar ratio of the hydrophilic monomer containing a thiol group, the fluoroalkyl oleophobic monomer containing a thiol group, and the cross-linking agent containing a carbon-carbon double bond in the functional monomer is 1.5-30:1:0.35-4; for example, 30:1:4, 20:1:3 and 1.5:1:0.35, etc., including but not limited to the molar ratios listed above.
[0022] Functional monomers are small molecules and other oligomers that are not spinnable. The present invention combines polymer electrospinning with the rapid cross-linking reaction between functional monomers to achieve the spinning of small molecules. Under the action of ultraviolet light and photoinitiator, the thiol group in the functional monomer will produce thiol free radicals to form an initiation stage. The formed free radicals can attack the double bond of olefins to form a new free radical intermediate. This free radical intermediate can further react with the thiol group on the hydrophilic or oleophobic group, and then cross-link in the electrospinning process to achieve efficient click chemistry reaction.
[0023] Further, in step S1, the hydrophilic monomer containing a carbon-carbon double bond is selected from one or more of acrylic acid, methacrylic acid, acrylamide and methacrylamide;
[0024] The fluoroalkyl oleophobic monomer containing a carbon-carbon double bond is selected from the following compounds of the general structural formula:
[0025] , wherein R is hydrogen or methyl, p is any integer from 1 to 5, and q is any integer from 3 to 9;
[0026] The cross-linking agent containing a thiol group is selected from one or more of bis(3-mercaptopropionic acid)ethylene glycol, trimethylolpropane tris(3-mercaptopropionate) and pentaerythritol tetrathioglycolate;
[0027] When the functional monomer includes a hydrophilic monomer containing a carbon-carbon double bond, a fluoroalkyl oleophobic monomer containing a carbon-carbon double bond, and a cross-linking agent containing a thiol group, the molar ratio of the hydrophilic monomer containing a carbon-carbon double bond, the fluoroalkyl oleophobic monomer containing a carbon-carbon double bond, and the cross-linking agent containing a thiol group in the functional monomer is 5-30:1:0.5-3; for example, 20:1:2, 15:1:1.5, 5:1:0.5, 30:1:3, etc., including but not limited to the molar ratios listed above.
[0028] The present invention controls the wettability of the final nanocellulose membrane by adjusting the ratio of the hydrophilic monomer and the oleophobic monomer in the functional monomer to match the application of the nanocellulose membrane in different scenarios. Too much cross-linking agent in the functional monomer will produce redundancy and affect the performance of the synthesized nanocellulose membrane, while too little cross-linking agent will cause the chemical reaction between the hydrophilic monomer and the hydrophobic monomer to be not rapid enough during the electrospinning process, resulting in poor performance of the nanocellulose membrane after cross-linking. Therefore, preferably, the molar ratio of the hydrophilic monomer containing a carbon-carbon double bond, the fluoroalkyl oleophobic monomer containing a carbon-carbon double bond, and the cross-linking agent containing a thiol group in the functional monomer is set to 1.5-30:1:0.35-4.
[0029] Furthermore, in step S1, the polymer is selected from one or more of collagen, cellulose acetate, polyethylene oxide, polyethylene oxide, polyvinylidene fluoride, polyacrylonitrile, polylactic acid, polyimide and polyvinyl alcohol. During electrospinning, the polymer will be spun into nanofibers, and the functional monomer will quickly undergo a click chemical reaction on the nanofibers to form a nanocellulose film.
[0030] Further, in step S1, the mass ratio of the photoinitiator to the polymer and the functional monomer in the electrospinning mixture is 0.1-3.5:1:10-105. Too little proportion of polymer in the electrospinning mixture will lead to a decrease in the viscoelasticity of the overall electrospinning mixture, resulting in the droplets of the mixture breaking at the moment of ejection from the end of the needle tip during the electrospinning process, and the functional monomer has no time to complete cross-linking polymerization. On the other hand, if the proportion of polymer in the electrospinning mixture is too much, the functional monomer component in the prepared electrospinning membrane will be reduced, thereby affecting the hydrophilic and lipophilic properties of the nanocellulose membrane. Therefore, the present invention needs to control the amount of polymer within a certain range, such as 3.03:1:100.6, 0.89:1:100.9, 2.95:1:98, 3:1:100.3, 2.98:1:99.77, 0.3:1:100, 3:1:100, etc., including but not limited to the above-mentioned proportions.
[0031] Further, in step S1, the solid content of the electrospinning mixture is 10-80wt%; for example, 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, 60wt%, 70wt% and 80wt%, etc., including but not limited to the solid contents listed above; preferably 15-70wt%.
[0032] Furthermore, in step S1, the organic solvent is selected from one or more of acetone, ethyl acetate, ethanol, tetrahydrofuran, N,N'-dimethylformamide and toluene. The organic solvent selected in the present invention is to ensure that the functional monomer, photoinitiator and polymer can be dissolved therein, and there is no strict restriction on the type of organic solvent.
[0033] Furthermore, in step S2, the electrospinning process parameters are: spinning voltage 8-35 kV, spinning distance 5-20 cm, spinning speed 0.5-3 mL / h, and needle diameter 0.2-3.5 mm.
[0034] Furthermore, in step S2, the wavelength of the ultraviolet light is 200-500 nm, and the irradiation intensity of the ultraviolet light is 20-150 W / cm 2 .
[0035] The second aspect of the present invention is to provide a nanocellulose membrane, wherein the nanocellulose membrane is prepared by the above-mentioned preparation method.
[0036] The third aspect of the present invention is to provide application of the nanocellulose membrane described in the second aspect in the field of oil-water separation.
[0037] Beneficial effects of the present invention:
[0038] 1. The present invention provides a method for preparing a nanocellulose film, which is simple to operate, quick to react, low in cost, and suitable for mass production; the prepared nanocellulose film has a long service life (the functional monomer and the polymer are integrated, avoiding the membrane separation problem caused by the modification or coating of the post-treatment process), and has a high efficiency for oil-water separation. An ultraviolet light source is used to irradiate the electrospinning mixture, initiating the polymerization of the functional monomer to form a nanocellulose film; in the process of electrospinning, the polymer can be used as a substrate for click chemistry reaction on the one hand; on the other hand, a certain viscosity can be provided for the electrospinning mixture to prevent the droplets from breaking instantly during the electrospinning process. Under the action of high voltage electricity and ultraviolet light, the electrospinning mixture is ejected from the end of the needle tip, and in the process of reaching the collecting device, the fast and efficient click chemistry reaction between the sulfhydryl group and the olefin allows each group containing the sulfhydryl group and the double bond to be rapidly cross-linked and polymerized, and stretched to form nanofibers, forming a nanofiber film with intrinsic superhydrophilic-superoleophobic properties.
[0039] 2. The present invention obtains a nanocellulose membrane with a porous structure by preparing an electrospinning mixture through a one-step mixing method. The nanocellulose membrane is formed by electrospinning a polymer. The functional monomers undergo a click chemical reaction under ultraviolet light and are coated on the polymer-spun fibers, forming a nanocellulose membrane with a clear fiber interface.
[0040] 3. The nanocellulose membrane prepared by the present invention has excellent oil-water separation efficiency, which can be as high as 99.9%. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 is a scanning electron microscope image (SEM) of the nanocellulose membrane prepared in Example 1 of the present invention;
[0042] Figure 2 The contact angle test of the nanocellulose membrane prepared in Example 1 of the present invention to water;
[0043] Figure 3 This is the contact angle test of the nanocellulose membrane prepared in Example 1 of the present invention on diesel;
[0044] Figure 4 The nanocellulose membrane prepared in Example 1 of the present invention is changed before and after separation of oil-in-water (diesel) emulsion;
[0045] Figure 5 The nanocellulose membrane prepared in Example 1 of the present invention is changed before and after separation of water-in-oil (diesel) emulsion;
[0046] Figure 6 is a scanning electron microscope image (SEM) of the nanocellulose film prepared in Comparative Example 2 of the present invention;
[0047] Figure 7 This is the contact angle test of the nanocellulose membrane prepared in Comparative Example 2 of the present invention to water;
[0048] Figure 8 This is the contact angle test of the nanocellulose membrane prepared in Comparative Example 2 of the present invention on diesel;
[0049] Fig. 9 is a scanning electron microscope image (SEM) of the nanocellulose film prepared in Comparative Example 3 of the present invention;
[0050] Fig.10 This is the contact angle test of the nanocellulose membrane prepared in Comparative Example 3 of the present invention to water;
[0051] Fig.11 This is a contact angle test of the nanocellulose membrane prepared in Comparative Example 3 of the present invention on diesel. DETAILED DESCRIPTION
[0052] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0053] The test methods of various indicators in the embodiment are as follows:
[0054] Contact angle testing method: Use a contact angle meter to drop 6 microliters of water droplets and diesel droplets on the fiber membrane surface, and observe the final angle of the water droplets on the fiber membrane surface. If the final angle is 0°, record the time required for the water droplet to reach 0°, which is the time for the water droplet and oil droplet to be completely wetted.
[0055] Separation efficiency test method: The test instrument is a trace moisture tester (Zibo Zifen Instrument Co., Ltd.); 100 mL of the filtrate before filtration and the filtrate after filtration were taken, and the water content was measured to be C0 and C1 respectively. Finally, according to the formula , the separation efficiency is calculated. Example 1
[0056] This embodiment relates to a method for preparing a nanocellulose film, which specifically comprises the following steps:
[0057] (1) Under dark conditions, methacrylic acid, a hydrophilic component containing double bonds, perfluorohexylethyl methacrylate, an oleophobic component containing double bonds, pentaerythritol tetrathioglycolate, a crosslinking agent containing thiol groups, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and cellulose acetate, a photoinitiator, were added to an acetone solution and stirred at room temperature for 20 min to obtain a uniformly mixed electrospinning mixture. The molar ratio of methacrylic acid, perfluorohexylethyl methacrylate, and pentaerythritol tetrathioglycolate in the functional monomer was 30:2:3; the mass ratio of the photoinitiator, cellulose acetate, and the functional monomer in the electrospinning mixture was 0.89:1:100.9; and the concentration of the electrospinning mixture was 40wt%.
[0058] (2) The electrospinning mixture is subjected to electrospinning. During the electrospinning process, the jet is illuminated by an ultraviolet light source to initiate polymerization of the functional monomers, thereby preparing a nanocellulose membrane. The electrospinning voltage is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, the needle diameter is 1 mm, the wavelength of the ultraviolet light source is 365 nm, and the irradiation intensity is 70 W / cm 2 .
[0059] like Figure 1 The electron microscope image of the prepared nanocellulose membrane is shown, and the contact angle test is performed on it. Figure 2 As shown in the figure, the contact angle of water is 0°, and the time for the water drop to spread completely is 1 s; the contact angle of diesel is 152° ( Figure 3 ), showing superhydrophilic-superoleophobic properties.
[0060] The prepared nanocellulose membrane was placed in water-in-oil (diesel) emulsion and oil (diesel)-in-water emulsion for separation efficiency test. The preparation method of water-in-oil is as follows: 1 g Span 80, 500 g water and 10 g diesel are ultrasonically cleaned in an ultrasonic cleaner for 24 hours to form a stable emulsion, and the prepared emulsion remains stable for at least 48 hours. The preparation method of oil-in-water is as follows: 1 g Span 80, 10 g water and 500 g diesel are ultrasonically cleaned in an ultrasonic cleaner for 24 hours to form a stable emulsion, and the prepared emulsion remains stable for at least 48 hours. The test results are as follows Figure 4 and 5 As shown, whether it is water-in-oil or oil-in-water emulsion, the nanocellulose membrane can separate water and oil, and the separation efficiency can reach 99.9%. Example 2
[0061] This embodiment relates to a method for preparing a nanocellulose film, which specifically comprises the following steps:
[0062] (1) Under dark conditions, methacrylic acid, a hydrophilic component containing double bonds, perfluorohexylethyl methacrylate, an oleophobic component containing double bonds, pentaerythritol tetrathioglycolate, a crosslinking agent containing thiol groups, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and cellulose acetate, a photoinitiator, were added to an acetone solution and stirred at room temperature for 20 min to obtain a uniformly mixed electrospinning mixture. The molar ratio of methacrylic acid, perfluorohexylethyl methacrylate, and pentaerythritol tetrathioglycolate in the functional monomer was 20:1:2; the mass ratio of the photoinitiator, cellulose acetate, and the functional monomer in the electrospinning mixture was 3.03:1:100.6; and the concentration of the electrospinning mixture was 40wt%.
[0063] (2) The electrospinning mixture is subjected to electrospinning. During the electrospinning process, the jet is illuminated by an ultraviolet light source to initiate polymerization of the functional monomers, thereby preparing a nanocellulose membrane. The electrospinning voltage is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, the needle diameter is 1 mm, the wavelength of the ultraviolet light source is 365 nm, and the irradiation intensity is 70 W / cm 2 .
[0064] The results showed that the contact angle of the prepared nanocellulose membrane to water was 0°, the time required for the water droplet to spread completely was 1 s, and the contact angle to diesel was 122°, showing super hydrophilic-oleophobic properties. Example 3
[0065] This embodiment relates to a method for preparing a nanocellulose film, which specifically comprises the following steps:
[0066] (1) Under dark conditions, methacrylic acid, a hydrophilic component containing double bonds, perfluorohexylethyl methacrylate, an oleophobic component containing double bonds, pentaerythritol tetrathioglycolate, a crosslinking agent containing thiol groups, photoinitiators 2-hydroxy-2-methyl-1-phenyl-1-propanone and cellulose acetate were added to an acetone solution and stirred at room temperature for 20 min to obtain a uniformly mixed electrospinning mixture. The molar ratio of methacrylic acid, perfluorohexylethyl methacrylate and pentaerythritol tetrathioglycolate in the functional monomer was 5:1:0.5; the mass ratio of the photoinitiator, cellulose acetate and the functional monomer in the electrospinning mixture was 2.95:1:98; and the concentration of the electrospinning mixture was 40wt%.
[0067] (2) The electrospinning mixture is subjected to electrospinning. During the electrospinning process, the jet is illuminated by an ultraviolet light source to induce polymerization of the functional monomers, thereby preparing a nanocellulose membrane. The electrospinning voltage is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, the needle diameter is 1 mm, the wavelength of the ultraviolet light source is 365 nm, and the irradiation intensity is 70 W / cm 2 .
[0068] The results showed that the contact angle of the prepared nanocellulose membrane to water was 0°, the time required for the water droplet to spread completely was 192 s, and the contact angle to diesel was 159°, showing superhydrophilic-superoleophilic properties. Example 4
[0069] This embodiment relates to a method for preparing a nanocellulose film, which specifically comprises the following steps:
[0070] (1) Under dark conditions, methacrylic acid, a hydrophilic component containing double bonds, perfluorohexylethyl methacrylate, an oleophobic component containing double bonds, pentaerythritol tetrathioglycolate, a crosslinking agent containing thiol groups, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and cellulose acetate, a photoinitiator, were added to an acetone solution and stirred at room temperature for 20 min to obtain a uniformly mixed electrospinning mixture. The molar ratio of methacrylic acid, perfluorohexylethyl methacrylate, and pentaerythritol tetrathioglycolate in the functional monomer was 15:1:1.5; the mass ratio of the photoinitiator, cellulose acetate, and functional monomer was 0.89:1:100.9; and the concentration of the electrospinning mixture was 15wt%.
[0071] (2) The electrospinning mixture is subjected to electrospinning. During the electrospinning process, the jet is illuminated by an ultraviolet light source to induce polymerization of the functional monomers, thereby preparing a nanocellulose membrane. The electrospinning voltage is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, the needle diameter is 1 mm, the wavelength of the ultraviolet light source is 365 nm, and the irradiation intensity is 70 W / cm 2 .
[0072] The results showed that the contact angle of the prepared nanocellulose membrane was tested. The contact angle of water was 0°, the time required for the water droplet to spread completely was 3 s, and the contact angle of diesel was 147°, showing super hydrophilic-oleophobic properties. Example 5
[0073] This embodiment relates to a method for preparing a nanocellulose film, which specifically comprises the following steps:
[0074] (1) Under dark conditions, a hydrophilic component containing double bonds, methacrylic acid, a double-bond oleophobic component containing double bonds, a crosslinking agent containing thiol groups, pentaerythritol tetrathioglycolate, a photoinitiator, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and cellulose acetate were added to an acetone solution and stirred at room temperature for 20 min to obtain a uniformly mixed electrospinning mixture. The molar ratio of methacrylic acid, perfluorohexylethyl methacrylate, and pentaerythritol tetrathioglycolate in the functional monomer is 15:1:1.5; the mass ratio of the photoinitiator, cellulose acetate, and the functional monomer in the electrospinning mixture is 0.89:1:100.9; and the concentration of the electrospinning mixture is 70wt%.
[0075] (2) The electrospinning mixture is subjected to electrospinning. During the electrospinning process, the jet is illuminated by an ultraviolet light source to induce polymerization of the functional monomers, thereby preparing a nanocellulose membrane. The electrospinning voltage is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, the needle diameter is 1 mm, the wavelength of the ultraviolet light source is 365 nm, and the irradiation intensity is 70 W / cm 2 .
[0076] The results showed that the contact angle of the prepared nanocellulose membrane was 0° for water, the time required for the water droplet to spread completely was 2 s, and the contact angle of diesel was 117°, showing super hydrophilic-oleophobic properties. Example 6
[0077] This embodiment relates to a method for preparing a nanocellulose film, which specifically comprises the following steps:
[0078] (1) Under dark conditions, methacrylic acid, a hydrophilic component containing double bonds, perfluorohexylethyl methacrylate, an oleophobic component containing double bonds, pentaerythritol tetrathioglycolate, a crosslinking agent containing thiol groups, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and cellulose acetate, a photoinitiator, were added to an acetone solution and stirred at room temperature for 20 min to obtain a uniformly mixed electrospinning mixture. The molar ratio of methacrylic acid, perfluorohexylethyl methacrylate, and pentaerythritol tetrathioglycolate in the functional monomer was 30:1:3; the mass ratio of the photoinitiator, cellulose acetate, and the functional monomer in the electrospinning mixture was 3:1:100.3; and the concentration of the electrospinning mixture was 40wt%.
[0079] (2) The electrospinning mixture is subjected to electrospinning. During the electrospinning process, the jet is illuminated by an ultraviolet light source to induce polymerization of the functional monomers, thereby preparing a nanocellulose membrane. The electrospinning voltage is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, the needle diameter is 1 mm, the wavelength of the ultraviolet light source is 365 nm, and the irradiation intensity is 70 W / cm 2 .
[0080] The results showed that the contact angle of the prepared nanocellulose membrane was 0° for water, the time required for the water droplet to spread completely was 9 s, and the contact angle of diesel was 143°, which showed super hydrophilicity and super oleophobicity. Example 7
[0081] This embodiment relates to a method for preparing a nanofiber membrane, which specifically comprises the following steps:
[0082] (1) In a dark environment, a hydrophilic component containing thioglycolic acid, a thioglycolic acid oleophobic component containing thioglycolic acid, a crosslinking agent containing double bonds, a photoinitiator 2-hydroxy-2-methyl-1-phenyl-1-propanone and cellulose acetate are added to an acetone solution and stirred at room temperature for 20 min to obtain a uniformly mixed electrospinning mixture. Among them, the molar ratio of thioglycolic acid, 1H,1H,2H,2H-perfluorooctane thiol and POSS acrylate in the functional monomer is 30:1:4; the mass ratio of the photoinitiator, cellulose acetate and the functional monomer in the electrospinning mixture is 2.98:1:99.77; and the concentration of the electrospinning mixture is 40wt%.
[0083] (2) The electrospinning mixture is subjected to electrospinning. During the electrospinning process, the jet is illuminated by an ultraviolet light source to induce polymerization of the functional monomers, thereby preparing a nanocellulose membrane. The electrospinning voltage is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, the needle diameter is 1 mm, the wavelength of the ultraviolet light source is 365 nm, and the irradiation intensity is 70 W / cm 2 .
[0084] The results showed that the contact angle of the prepared nanocellulose membrane was 0° for water, the time required for the water droplet to spread completely was 3 s, and the contact angle of diesel was 127°, showing super hydrophilic-oleophobic properties. Example 8
[0085] This embodiment relates to a method for preparing a nanofiber membrane, which specifically comprises the following steps:
[0086] (1) In a dark environment, a hydrophilic component containing thioglycolic acid, a thioglycolic acid oleophobic component containing thioglycolic acid, a crosslinking agent containing double bonds, a photoinitiator 2-hydroxy-2-methyl-1-phenyl-1-propanone and cellulose acetate are added to an acetone solution of cellulose, and stirred at room temperature for 2 h to obtain a uniformly mixed electrospinning mixture. The molar ratio of thioglycolic acid monomer, 1H,1H,2H,2H-perfluorooctane thiol and POSS acrylate in the functional monomer is 20:1:3; the mass ratio of the photoinitiator, cellulose acetate and the functional monomer in the electrospinning mixture is 0.3:1:10; and the concentration of the electrospinning mixture is 40wt%.
[0087] (2) The electrospinning mixture is subjected to electrospinning. During the electrospinning process, the jet is illuminated by an ultraviolet light source to induce polymerization of the functional monomers, thereby preparing a nanocellulose membrane. The electrospinning voltage is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, the needle diameter is 1 mm, the wavelength of the ultraviolet light source is 365 nm, and the irradiation intensity is 70 W / cm 2 .
[0088] The results showed that the contact angle of the prepared nanocellulose membrane was 0° for water, the time required for the water droplet to spread completely was 7 s, and the contact angle of diesel was 151°, showing superhydrophilic-superoleophobic properties. Example 9
[0089] This embodiment relates to a method for preparing a nanofiber membrane, which specifically comprises the following steps:
[0090] (1) In a dark environment, a hydrophilic component containing thioglycolic acid, a thioglycolic acid oleophobic component containing thioglycolic acid, a crosslinking agent containing double bonds, a pentaerythritol tetrathioglycolate containing thioglycolic acid, a photoinitiator 2-hydroxy-2-methyl-1-phenyl-1-propanone and cellulose acetate are added to an acetone solution and stirred at room temperature for 2 h to obtain a uniformly mixed electrospinning mixture. The molar ratio of thioglycolic acid monomer, 1H,1H,2H,2H-perfluorooctane thiol and POSS acrylate in the functional monomer is 1.5:1:0.35; the mass ratio of the photoinitiator, cellulose acetate and the functional monomer in the electrospinning mixture is 3:1:100; and the concentration of the electrospinning mixture is 40wt%.
[0091] (2) The electrospinning mixture is subjected to electrospinning. During the electrospinning process, the jet is illuminated by an ultraviolet light source to induce polymerization of the functional monomers, thereby preparing a nanocellulose membrane. The electrospinning voltage is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, the needle diameter is 1 mm, the wavelength of the ultraviolet light source is 365 nm, and the irradiation intensity is 70 W / cm 2 .
[0092] The results showed that the contact angle of the prepared nanocellulose membrane was 0° for water, the time required for the water droplet to spread completely was 258 s, and the contact angle of diesel was 153°, showing superhydrophilic-superoleophobic properties. Comparative Example 1
[0093] This comparative example relates to a method for preparing a nanocellulose membrane. The difference between this comparative example and Example 1 is that only cellulose acetate in the electrospinning mixture is electrospun, and specifically comprises the following steps:
[0094] Cellulose acetate was added to an acetone solution and stirred at room temperature for 2 h to obtain a uniformly mixed 17 wt% cellulose acetate mixture. The mixture was electrospun to prepare a nanocellulose membrane. The electrospinning voltage was 25 kV, the spinning distance was 15 cm, the spinning speed was 1 mL / h, and the needle diameter was 1 mm.
[0095] The results showed that the contact angle of the prepared nanocellulose membrane was 148° for water and 0° for diesel. The time required for diesel to spread completely was 1 s, showing hydrophobic-superoleophilic properties. Comparative Example 2
[0096] This comparative example relates to a method for preparing a nanofiber membrane. The difference between this comparative example and Example 1 is that there is no ultraviolet light irradiation in step (2). Specifically, the following steps are included:
[0097] (1) Under dark conditions, methacrylic acid, a hydrophilic component containing double bonds, perfluorohexylethyl methacrylate, an oleophobic component containing double bonds, pentaerythritol tetrathioglycolate, a crosslinking agent containing thiol groups, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and cellulose acetate, a photoinitiator, were added to an acetone solution and stirred at room temperature for 20 min to obtain a uniformly mixed electrospinning mixture. The molar ratio of methacrylic acid, perfluorohexylethyl methacrylate, and pentaerythritol tetrathioglycolate in the functional monomer was 15:1:1.5; the mass ratio of the photoinitiator, cellulose acetate, and the functional monomer in the electrospinning mixture was 0.89:1:100.9; and the concentration of the electrospinning mixture was 40wt%.
[0098] (2) The electrospinning mixture is subjected to electrospinning; wherein the electrospinning voltage is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, the diameter of the needle is 1 mm, and no ultraviolet light source is irradiated during the electrospinning process, thereby preparing a nanocellulose membrane.
[0099] The results show that Figure 6 The fiber interface of the prepared nanocellulose membrane is not obvious and there is adhesion between the pores, which indicates that the lack of light during the electrospinning process will cause the functional monomers in the electrospinning mixture to adhere to the surface of the electrospun fibers; Figure 7 The contact angle of the nanocellulose membrane to water is 63° and the contact angle to diesel is 0° ( Figure 8 ), showing hydrophilic-superlipophilic properties. Comparative Example 3
[0100] This comparative example relates to a method for preparing a nanofiber membrane. The difference between this comparative example and Example 1 is that in step (2), an electrospinning process is first performed, and then an ultraviolet light irradiation step is performed; specifically, the following steps are included:
[0101] (1) Under dark conditions, methacrylic acid, a hydrophilic component containing double bonds, perfluorohexylethyl methacrylate, an oleophobic component containing double bonds, pentaerythritol tetrathioglycolate, a crosslinking agent containing thiol groups, photoinitiators 2-hydroxy-2-methyl-1-phenyl-1-propanone and cellulose acetate were added to an acetone solution and stirred at room temperature for 20 min to obtain a uniformly mixed electrospinning mixture. The molar ratio of methacrylic acid, perfluorohexylethyl methacrylate and pentaerythritol tetrathioglycolate in the functional monomer was 15:1:1.5; the mass ratio of the photoinitiator, cellulose acetate and the functional monomer in the electrospinning mixture was 0.89:1:100.9; and the concentration of the electrospinning mixture was 40wt%.
[0102] (2) The electrospinning mixture is electrospun, and no ultraviolet light source is used to illuminate the ejected jet during the electrospinning process. After electrospinning, it is placed under an ultraviolet light source for full irradiation to obtain a nanocellulose membrane. The voltage of the electrospinning is 25 kV, the spinning distance is 15 cm, the spinning speed is 1 mL / h, and the diameter of the needle is 1 mm; the wavelength of the ultraviolet light source is 365 nm, and the irradiation intensity is 70 W / cm 2 .
[0103] The results show that Fig. 9 The adhesion between the fibers of the prepared nanocellulose membrane is more serious, and the contact angle of the prepared nanocellulose membrane to water is 140° ( Fig.10 ), the contact angle of diesel is 102º( Fig.11 ), showing hydrophobic-oleophobic properties.
[0104] The contact angles of water and oil of the nanocellulose membranes prepared in the above examples and comparative examples were tested. The results are shown in Table 1.
[0105] Table 1
[0106]
[0107] As shown in Table 1, the nanocellulose film prepared by using cellulose acetate alone in Comparative Example 1 shows hydrophobic super-oleophilic performance.Comparative Example 2 is to spin the electrospinning mixture to obtain a nanocellulose film without ultraviolet light, showing hydrophilic-super-oleophilic performance, indicating that click chemistry reaction can not occur between functional monomers without ultraviolet light irradiation, thereby showing hydrophilic-oleophilic performance.Comparative Example 3 first electrospins the electrospinning mixture, and then irradiates the product of its spinning with ultraviolet light (ultraviolet light irradiation time is sufficient), and it is found that a hydrophilic and oleophobic nanocellulose film can not be prepared.Examples 1-9 are nanocellulose films obtained by irradiating ultraviolet light simultaneously in the process of electrospinning preparation of electrospinning mixture, and their nanocellulose films all show intrinsic hydrophilic and oleophobic performance, indicating that applying ultraviolet light irradiation simultaneously in the process of electrospinning is a key factor in preparing hydrophilic and oleophobic nanocellulose films.
[0108] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A method for preparing an intrinsically hydrophilic and oleophobic nanofiber membrane, characterized in that: The following steps are involved: S1. In a light-proof environment, a functional monomer, a photoinitiator and a polymer are mixed in an organic solvent to obtain an electrospinning mixture; The functional monomers include a hydrophilic monomer, an oleophobic monomer and a cross-linking agent; The cross-linking agent is a cross-linking agent containing carbon-carbon double bonds and / or a cross-linking agent containing thiol groups; The cross-linking agent containing carbon-carbon double bonds contains at least two carbon-carbon double bonds, and the cross-linking agent containing thiol groups contains at least two thiol groups; When the cross-linking agent includes a cross-linking agent containing a carbon-carbon double bond, the hydrophilic monomer includes a hydrophilic monomer containing a thiol group, and the oleophobic monomer includes a fluoroalkyl oleophobic monomer containing a thiol group; when the cross-linking agent includes a cross-linking agent containing a thiol group, the hydrophilic monomer includes a hydrophilic monomer containing a carbon-carbon double bond, and the oleophobic monomer includes a fluoroalkyl oleophobic monomer containing a carbon-carbon double bond; S2, setting electrospinning process parameters, spinning the electrospinning mixture prepared in step S1 under ultraviolet light to obtain the intrinsically hydrophilic and oleophobic nanofiber membrane.
2. The preparation method according to claim 1, characterized in that In step S1, the hydrophilic monomer containing a thiol group is selected from compounds of the following general structural formula: ; Wherein, R is one of hydroxyl, carboxyl, amide, amino or aldehyde; t is any integer from 1 to 9; The sulfhydryl-containing fluoroalkyl oleophobic monomer is selected from the following compounds of the general structural formula: ; Wherein, m is any integer from 1 to 5, and n is any integer from 3 to 9; The cross-linking agent containing carbon-carbon double bonds is selected from one or more of polyethylene glycol diacrylate, N-carboxyethyl acrylamide, 3-(trimethoxysilyl)propyl-2-methyl-2-acrylate, pentaerythritol triallyl ether, triallyl isocyanurate, pentaerythritol tetraacrylate, polydipentaerythritol pentaacrylate, vinyl cage-type polysilsesquioxane and acrylate cage-type polysilsesquioxane; When the functional monomers include a hydrophilic monomer containing a thiol group, a fluoroalkyl oleophobic monomer containing a thiol group, and a cross-linking agent containing a carbon-carbon double bond, the molar ratio of the hydrophilic monomer containing a thiol group, the fluoroalkyl oleophobic monomer containing a thiol group, and the cross-linking agent containing a carbon-carbon double bond in the functional monomers is 1.5-30:1:0.35-4.
3. The preparation method according to claim 1, characterized in that: In step S1, The hydrophilic monomer containing a carbon-carbon double bond is selected from one or more of acrylic acid, methacrylic acid, acrylamide, and methacrylamide; The fluoroalkyl oleophobic monomer containing a carbon-carbon double bond is selected from the following compounds of the general structural formula: , wherein R is hydrogen or methyl, p is any integer from 1 to 5, and q is any integer from 3 to 9; The cross-linking agent containing a thiol group is selected from one or more of bis(3-mercaptopropionic acid)ethylene glycol, trimethylolpropane tris(3-mercaptopropionate) and pentaerythritol tetrathioglycolate; When the functional monomers include a hydrophilic monomer containing a carbon-carbon double bond, a fluoroalkyl oleophobic monomer containing a carbon-carbon double bond, and a cross-linking agent containing a thiol group, the molar ratio of the hydrophilic monomer containing a carbon-carbon double bond, the fluoroalkyl oleophobic monomer containing a carbon-carbon double bond, and the cross-linking agent containing a thiol group in the functional monomers is 5-30:1:0.5-3.
4. The preparation method according to claim 1, characterized in that: In step S1, the polymer is selected from one or more of collagen, cellulose acetate, polyethylene oxide, polyethylene oxide, polyvinylidene fluoride, polyacrylonitrile, polylactic acid, polyimide and polyvinyl alcohol.
5. The preparation method according to claim 1, characterized in that: In step S1, the mass ratio of the photoinitiator to the polymer and the functional monomer in the electrospinning mixture is 0.1-3.5:1:10-105.
6. The preparation method according to claim 1, characterized in that: In step S1, the solid content of the electrospinning mixture is 10-80 wt%.
7. The preparation method according to claim 1, characterized in that: In step S2, the electrospinning process parameters are: spinning voltage 8-35 kV, spinning distance 5-20 cm, spinning speed 0.5-3 mL / h, and needle diameter 0.2-3.5 mm.
8. The preparation method according to claim 1, characterized in that: In step S2, the wavelength of the ultraviolet light is 200-500nm; the irradiation intensity of the ultraviolet light is 20-150 W / cm 2 .
9. A nanocellulose film, characterized in that The nanocellulose membrane is prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the nanocellulose membrane as claimed in claim 9 in the field of oil-water separation.