Non-dissolution type antibacterial spun-bonded non-woven fabric as well as preparation process and application thereof

By inserting a cationic antibacterial agent and polypropylene-grafted maleic anhydride into the montmorillonite sheet, combined with a silane coupling agent, a non-leaching antibacterial spunbond non-woven fabric was prepared, which solved the problem of the compatibility between the antibacterial agent and polypropylene and the Dispersion problem, achieving efficient and long-lasting antibacterial performance and improved mechanical strength.

CN118727273AActive Publication Date: 2024-10-01HENAN TUOREN MEDICAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410863589.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-29
Publication Date
2024-10-01
Estimated Expiration
2044-06-29

AI Technical Summary

Technical Problem

The antibacterial agent of existing antibacterial spunbond non-woven fabrics is difficult to be compatible with polypropylene, the blend system has poor dispersion, low production efficiency, and the coating is easy to fall off, resulting in short-lasting antibacterial performance and difficulty in popularization and application.

Method used

Antibacterial modified montmorillonite is used as a carrier, and a cationic antibacterial agent and polypropylene-grafted maleic anhydride are inserted between the montmorillonite sheets through mechanical grinding. Combined with a silane coupling agent, a non-leaching antibacterial agent is prepared through a spunbonding process. Spunbond non-woven fabric ensures the strong combination of antibacterial agent and spunbond non-woven fabric.

Benefits of technology

The antibacterial properties and mechanical strength are improved. The high compatibility between antibacterial modified montmorillonite and polypropylene ensures that the antibacterial agent does not dissolve and fall off, and improves the production efficiency and application promotion potential of spunbond non-woven fabrics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727273A_ABST
    Figure CN118727273A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of non-woven, and relates to a non-dissolution type antibacterial spun-bonded non-woven fabric and a preparation process and application thereof. The non-woven fabric is prepared by using polypropylene, antibacterial modified montmorillonite and a silane coupling agent as main raw materials through a spunbond process, wherein the antibacterial modified montmorillonite is obtained by taking montmorillonite as a carrier and inserting a cationic antibacterial agent, polypropylene grafted maleic anhydride and polypropylene powder between lamellas of the montmorillonite through a mechanical grinding method. The antibacterial property is achieved, the bacteriostasis rate on staphylococcus aureus is larger than 65%, the bacteriostasis rate on escherichia coli is larger than 65%, the bacteriostasis rate on candida albicans is larger than 50%, and the cell survival rate is larger than 92%; the mechanical strength is excellent, the transverse elongation is 95-110%, and the transverse breaking force is 40-47N; the longitudinal elongation is 75-85%, and the longitudinal breaking force is 90-100N. The non-woven fabric is laminated and compounded with a melt-blown non-woven fabric, a breathable film and a lamination layer to prepare an antibacterial spun-bonded melt-blown composite non-woven fabric, an antibacterial laminated non-woven fabric and an antibacterial laminated non-woven fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonwovens, and relates to a spunbonded nonwoven fabric, and in particular to a non-dissolving antibacterial spunbonded nonwoven fabric, and a preparation process and application thereof. Background Art

[0002] The main materials of spunbond nonwovens include polyester and polypropylene, among which polypropylene spunbond nonwovens are the most common in medical and sanitary materials. Polypropylene spunbond nonwovens, also known as polypropylene spunbond nonwovens, are a new generation of environmentally friendly materials with the characteristics of water repellency, breathability, flexibility, non-combustibility, non-toxicity, non-irritation, and rich colors. During the epidemic, ordinary protective products cannot meet the needs of resisting bacteria and viruses, and consumables such as masks and protective clothing may become new sources of infection after use. With the increasing application of spunbond nonwovens, the demand for safe, efficient, long-lasting and non-dissolving antibacterial spunbond nonwovens is also growing sharply.

[0003] The antibacterial spunbond nonwoven fabrics in the prior art have the following problems: 1. Antibacterial agents are difficult to be compatible with polypropylene, and the dispersibility of the blending system is poor; 2. Most of the antibacterial spunbond nonwoven fabrics on the market achieve short-term antibacterial purposes by spraying / immersing antibacterial agent solutions, with low production efficiency and difficulty in ensuring long-term antibacterial effects; 3. Coating antibacterial agents are easy to fall off the surface of nonwoven fabrics and will produce cytotoxicity to normal cells.

[0004] In response to the above problems, Chinese invention patent CN111424432B discloses a non-dissolving long-lasting antibacterial protective non-woven fabric and its preparation method and application. The antibacterial liquid is evenly sprayed on the non-woven fabric or the non-woven fabric is soaked in the antibacterial liquid. After the silicone molecules are polymerized, the binding force between the non-woven fabric fiber and the antibacterial active substance is enhanced. After high-temperature shaping, the antibacterial active substances such as ammonium salts and nano-silver are directionally loaded on the surface of the non-woven fabric to make an antibacterial protective non-woven fabric. This technology achieves antibacterial properties by preparing non-woven fabrics and antibacterial liquids, spraying or soaking in antibacterial liquids, and high-temperature shaping. It can be seen that there are too many processes and resources are consumed. The coating is easy to fall off during use, and the production efficiency is low, which is difficult to promote and apply.

[0005] Chinese invention patent CN111172749A discloses an antibacterial and antiviral non-woven fabric and its preparation method, and a mask containing the same. Inorganic antibacterial agents such as titanium dioxide and nano zinc oxide are prepared into sols with organic antibacterial agents such as chitosan and quaternary ammonium salts, and the second layer of the mask after organic fluorine finishing is immersed in the sol to prepare the antibacterial and antiviral non-woven fabric. The non-woven fabric is compounded with a first fabric layer, an anti-haze filter layer, and a second fabric layer to prepare a mask. Sol immersion is not efficient, and a new fabric layer is added to the original mask structure. The preparation process is complicated, which may affect the air resistance of the original mask, and the production efficiency is not high, making it difficult to mass produce.

[0006] Chinese invention patent CN113968585A discloses a modified nano-montmorillonite, nano-tackifier and its preparation method and application, which introduces long-chain active groups between nano-montmorillonite sheets through intercalation reaction in solution to change the hydrophilicity and hydrophobicity of nano-montmorillonite itself. This patent proves the feasibility of modifying montmorillonite in solution, but the operation is complicated, time-consuming, low in yield, and not easy for industrial production.

[0007] Chinese invention patent CN100519415C discloses a method for preparing flaky exfoliated nano-montmorillonite, which uses a mechanochemical method to prepare nano-montmorillonite, and organically intercalates sodium-based montmorillonite through a mechanochemical method to obtain flaky exfoliated nano-montmorillonite powder. The process is simple and suitable for industrial production, but the method does not specify the application scenario, and related processes need to be developed separately for the actual use of different products.

[0008] Organic modified montmorillonite is one of the hot spots of current research. Surfactant treatment can change the microenvironment of montmorillonite. As one of the surfactants, quaternary ammonium salt can exchange ions with cations in montmorillonite in the solvent, enter between the montmorillonite layers to increase the interlayer spacing of montmorillonite, and improve the performance of montmorillonite. The alkyl chain outside the layer increases the lipophilicity of montmorillonite, enhances the affinity between the montmorillonite layer and the resin molecular chain, reduces the surface energy of montmorillonite, and makes it easier for the resin monomer or molecular chain to be inserted between the montmorillonite layers to form a nanocomposite material. The montmorillonite modified by quaternary ammonium salt intercalation has certain antibacterial properties and can improve the strength of polypropylene, but when it is used together with polypropylene, compatibility needs to be considered. The addition of polypropylene grafted maleic anhydride can improve its compatibility, but the dispersibility of polypropylene grafted maleic anhydride with polypropylene and modified montmorillonite also needs to be considered.

[0009] Modified montmorillonite and polypropylene matrix can be firmly combined in the form of intercalation through the nano effect during melt blending modification. The melt intercalation method only requires mixing polypropylene and montmorillonite, and mixing the two evenly in an extruder to obtain a nanocomposite material. The polymer molecules can be inserted into the interlaminar space of montmorillonite to improve the toughness, thermal stability, anti-aging tensile strength, etc. of the polypropylene material itself. This process does not require too much solvent and is simple to operate. It only requires conventional equipment such as screw extruders and mixers. Organic modification and polypropylene grafting maleic anhydride can improve the compatibility of montmorillonite and polypropylene. At present, the nanocomposite of polypropylene and montmorillonite is mostly concentrated on the enhancement of polypropylene. This firm intercalation method also ensures that the cationic modifier uses montmorillonite as a carrier in polypropylene, but it is not too involved.

[0010] In view of the shortcomings of the existing technology, it is urgently necessary to develop a new type of antibacterial spunbond nonwoven fabric, which can firmly combine the antibacterial unit with the spunbond nonwoven fabric, and has a simple production process and can be continuously mass-produced, which is conducive to promotion and application. Summary of the invention

[0011] Based on this, the purpose of the present invention is to provide a non-dissolving antibacterial spunbond nonwoven fabric and a preparation process thereof to solve the deficiencies in the prior art.

[0012] To achieve the above object, the present invention adopts the following technical solutions: The invention provides a non-dissolving antibacterial spunbonded nonwoven fabric, which is characterized in that the non-dissolving antibacterial spunbonded nonwoven fabric is prepared by a spunbonding process using polypropylene, antibacterial modified montmorillonite and a silane coupling agent as main raw materials; the antibacterial modified montmorillonite is obtained by inserting a cationic antibacterial agent, polypropylene grafted maleic anhydride and polypropylene powder between its sheets by a mechanical grinding method using montmorillonite as a carrier.

[0013] Furthermore, the non-woven fabric has antibacterial properties, with an antibacterial rate of >65% against Staphylococcus aureus, >65% against Escherichia coli, >50% against Candida albicans, and a cell survival rate of >92%; it has excellent mechanical strength, with a lateral elongation of 95-110% and a lateral breaking force of 40-47N; the longitudinal elongation is 75-85% and the longitudinal breaking force is 90-100N.

[0014] The present invention further provides a process for preparing a non-dissolving antibacterial spunbonded nonwoven fabric, which is characterized by comprising the following steps: S1, adding montmorillonite alcohol solution A and cationic antibacterial agent alcohol solution B to a ball mill in proportion, grinding and reacting for a period of time, adding polypropylene powder and polypropylene grafted maleic anhydride in proportion, and continuing grinding, drying and crushing to obtain antibacterial modified montmorillonite; S2, mixing the antibacterial modified montmorillonite, polypropylene powder and silane coupling agent in S1 in proportion, and forming an antibacterial masterbatch after extrusion and cutting by an extruder; S3, the antibacterial masterbatch, polypropylene and color masterbatch described in S2 are mixed in proportion, and then melted, spun, initially pressed and hot rolled to obtain a non-dissolving antibacterial spunbonded nonwoven fabric.

[0015] Furthermore, the ratio of the montmorillonite to the solvent in the montmorillonite alcohol solution A in S1 is 1:5-10, and the amount of montmorillonite added is 3-5 parts; the ratio of the cationic antibacterial agent to the solvent in the antibacterial agent alcohol solution B is 1:3-5, and the amount of cationic antibacterial agent added is 1-6 parts; the amount of polypropylene powder added is 1 part; the amount of polypropylene grafted maleic anhydride added is 1.5-3 parts; wherein the raw material components are measured in parts by weight.

[0016] Furthermore, the montmorillonite in S1 includes sodium montmorillonite with an ion exchange capacity of 100-200 meq / 100g; the cationic antibacterial agent includes any one or more of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, cetylpyridinium bromide, cetylpyridinium chloride, tetradecyldimethylbenzylammonium chloride, and cetyldimethylbenzylammonium chloride; the solvent includes any one or more of anhydrous ethanol and methanol.

[0017] Furthermore, the added proportion of the antibacterial modified montmorillonite, polypropylene powder and silane coupling agent in S2 is 1:0.8-1.2:0.03-0.05; the coupling agent mainly includes any one or two of γ-methacryloxypropyltrimethoxysilane (KH560, CAS No.: 2530-85-0) and γ-glycidyloxypropyltrimethoxysilane (KH570, CAS No.: 2530-83-8); wherein the raw material components are measured in parts by weight; wherein the raw material components are measured in parts by weight.

[0018] Furthermore, the ratio of the antibacterial masterbatch, polypropylene and color masterbatch added in S3 is 1:6-10:0-0.3; wherein the raw material components are measured in parts by weight.

[0019] Furthermore, the mass ratio of large, medium and small agate balls used in the ball mill described in S1 is 10-20:25-40:40-65; the overall ball-to-material ratio is 70-80:20-30, the ball milling speed is 400-500rpm, and after the A and B solutions are mixed, the ball milling time is 1-2h in the forward direction and 1-2h in the reverse direction; after the polypropylene grafted maleic anhydride and polypropylene powder are added, the ball milling time is 1-2h in the reverse direction and 1-2h in the forward direction; after the ball milling, the ball milling is dried for 6-8h at a drying temperature of 80-90°C.

[0020] Furthermore, the antibacterial masterbatch extrusion parameters described in S2 include: stirring at low speed in a high mixing pot for 1 minute; introducing the stirred raw materials into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 140±10°C for zone 1, 145±10°C for zone 2, 155±5°C for zone 3, 180±10°C for zone 4, 195±5°C for zone 5, 200±5°C for zone 6, 205±10°C for zone 7, 205±10°C for zone 8, 205±10°C for zone 9, and 205±10°C for the die head, the feeding speed is 12±2 rpm / min, the main engine speed is 120±15 rpm / min, and the pelletizing speed is 370±20rpm / min.

[0021] Furthermore, the non-dissolving antibacterial spunbond non-woven fabric extrusion parameters described in S3 include: the spunbond process temperatures in zones 1 to 6 are 185±10°C for zone 1, 225±10°C for zone 2, 235±10°C for zone 3, 235±10°C for zone 4, 235±10°C for zone 5, and 235±10°C for zone 6; the cooling, stretching, and blasting related parameters are melt cooling air 6±2°C; monomer 550±50 rpm / min; metering pump 24±1 Hz; suction 1150±100 rpm / min; and web speed 215±15m / min.

[0022] The present invention also provides an application of a non-dissolving antibacterial spunbond non-woven fabric, characterized in that the antibacterial spunbond meltblown composite non-woven fabric, the antibacterial coated non-woven fabric and the antibacterial coated non-woven fabric are prepared by stacking and compounding with a meltblown non-woven fabric, a breathable film and a coating layer.

[0023] The beneficial effects of the present invention are: 1. The preparation process provided by the present invention is to closely intercalate the cationic antibacterial agent in the sodium montmorillonite through a mechanical grinding process, and then add polypropylene powder and polypropylene grafted maleic anhydride. In the ball milling stage, the montmorillonite layer gradually increases, and the polypropylene molecular chains and the polypropylene grafted maleic anhydride molecular chains are mutually entangled inside and outside the montmorillonite layer. The maleic anhydride groups in the layer can form hydrogen bonds with the nitrogen ions in the intercalated quaternary ammonium salt antibacterial agent, and the combination is firm, and the compatibility and interface bonding strength between the montmorillonite and the organic polymer polypropylene are improved.

[0024] 2. In the preparation process provided by the present invention, adding a coupling agent can further promote the mixing of montmorillonite and polypropylene, the polypropylene molecular chain is inserted into the montmorillonite layer, the montmorillonite layer is further enlarged and the compatibility with polypropylene is improved, and an antibacterial montmorillonite-polypropylene nanocomposite material is obtained. The quaternary ammonium salt cations intercalated between the montmorillonite layers are used to form a composite material with montmorillonite and polypropylene, which further improves the firmness of the antibacterial agent and polypropylene while realizing the antibacterial function, and obtains a non-dissolving antibacterial masterbatch, ensuring the safety of downstream products.

[0025] 3. The preparation process provided by the present invention, the montmorillonite antibacterial masterbatch prepared by ball milling combined with melt extrusion process, due to the ball milling dispersion, organic intercalation and other processes, the coupling agent, polypropylene grafted maleic anhydride, and polypropylene promote each other, and the obtained nano-montmorillonite masterbatch has a high compatibility with polypropylene, which can not only show the rigidity of the nano-montmorillonite itself, but also promote the crystallization of non-woven fibers during the melt cooling and stretching process of the non-woven fabric, make the arrangement of the molecular chains more regular, and improve the strength of the non-woven fabric.

[0026] 4. The non-dissolving antibacterial spunbonded non-woven fabric provided by the present invention has an antibacterial rate of >65% against Staphylococcus aureus, an antibacterial rate of >65% against Escherichia coli, an antibacterial rate of >50% against Candida albicans, and a cell survival rate of >92%; it has excellent mechanical strength, with a transverse elongation of 95-110% and a transverse breaking force of 40-47N; a longitudinal elongation of 75-85% and a longitudinal breaking force of 90-100N.

[0027] 5. The antibacterial spunbond non-woven fabric, antibacterial spunbond meltblown composite non-woven fabric, antibacterial coated non-woven fabric and antibacterial film-coated non-woven fabric provided by the present invention can be widely used in medical surgical masks, medical isolation gowns, medical protective clothing, disposable mid-sheets, disposable surgical gowns, disposable nursing pads, disposable diapers, disposable travel clothes and other products. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solution of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Attached Figure 1 Schematic diagram of the intercalation and modification process of antibacterial modified montmorillonite.

[0030] Attached Figure 2 Schematic diagram of the antibacterial masterbatch granulation process.

[0031] Attached Figure 3 XRD patterns of antibacterial modified montmorillonite before and after modification.

[0032] Attached Figure 4 This is the infrared test spectrum of antibacterial modified montmorillonite.

[0033] Attached Figure 5 This is the transverse rupture force and displacement curve of Example 3.

[0034] Attached Figure 6 This is the longitudinal breaking force and displacement curve of Example 3.

[0035] Attached Figure 7 This is the non-dissolution test result of antibacterial spunbond nonwoven fabric. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. The embodiments mentioned are all implemented on the premise of the technical solutions of the present invention, and detailed implementation processes are given, but it should be stated that the protection scope of the present invention is not limited to the following embodiments. Example 1

[0037] Preparation of a non-dissolving antibacterial spunbonded nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 100 parts of sodium montmorillonite (100meq / 100g) and add 500 parts of anhydrous ethanol, and stir continuously to prepare suspension solution A; weigh 57.6 parts of cetylpyridinium bromide (1.5 times the cation exchange capacity) and put it into 200 parts of anhydrous ethanol solvent and stir it with a magnetic stirrer to prepare mixed solution B; put grinding balls into a planetary ball mill, pour in mixed solution A and B, the ratio of grinding balls is large (D14), medium (D10), small (D6) = 10:25:65, and the ball-to-material ratio is 80:20 and sealed; open the ball mill and heat at 500 rpm / min, grind forward for 1h, reverse grind for 2h, then add 50 parts of polypropylene grafted maleic anhydride and 30 parts of polypropylene powder into the ball mill, continue grinding at 500r / min, reverse for 1h, and forward for 2h; filter the mixed slurry taken out from the ball mill and dry it in a vacuum drying oven at 80℃ for 8h to obtain highly compatible antibacterial modified montmorillonite; more than 5kg is prepared cumulatively; (2) Preparation of antibacterial masterbatch: Weigh 20 parts of spunbond polypropylene powder, 1 part of KH570, and 20 parts of the highly compatible antibacterial modified montmorillonite obtained in step (1), and stir them at a low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 139° C. for zone 1, 142° C. for zone 2, 157° C. for zone 3, 177° C. for zone 4, 196° C. for zone 5, 205° C. for zone 6, 209° C. for zone 7, 208° C. for zone 8, 210° C. for zone 9, and 209° C. for the die head, the feed speed is 12.2 rpm / min, the main engine speed is 117 rpm / min, and the pelletizing speed is 359 rpm / min; (3) Preparation of antibacterial spunbond nonwoven fabrics: Add 10 parts of montmorillonite antibacterial masterbatch, 80 parts of spunbond polypropylene pellets, and 1 part of masterbatch to the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drawing, and induced air cloth is formed. The spunbond process temperatures in zones 1 to 6 are 192°C for zone 1, 232°C for zone 2, 244°C for zone 3, 245°C for zone 4, 241°C for zone 5, and 242°C for zone 6. The cooling, drawing, and blast related parameters are melt cooling air 6°C; monomer 570 rpm / min; metering pump 23.2 Hz; suction 1230rpm / min. Web forming speed 219m / min; The finished antibacterial spunbond nonwoven fabrics were tested for appearance, width, weight, stretch and other performances. Example 2

[0038] Preparation of a non-dissolving antibacterial spunbonded nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 100 parts of sodium montmorillonite (200meq / 100g) and add 450 parts of anhydrous methanol, and stir continuously to prepare suspension solution A; weigh 118.8 parts of hexadecylbenzyldimethylammonium chloride (1.5 times the cation exchange capacity) and put it into 400 parts of anhydrous ethanol solvent and stir it with a magnetic stirrer to prepare mixed solution B; put grinding balls into a planetary ball mill, pour in mixed solution A and B, the ratio of grinding balls is large (D14), medium (D10), small (D6) = 15:30:55, and the ball-to-material ratio is 75:25 and sealed; open the ball mill and heat at 450 rpm / min, grind forward for 1.5h, reverse grind for 1h, then add 50 parts of polypropylene grafted maleic anhydride and 20 parts of polypropylene powder into the ball mill, continue grinding at 500r / min, reverse for 1.5h, and forward for 1.5h; filter the mixed slurry taken out from the ball mill and dry it in a vacuum drying oven at 90℃ for 6h to obtain highly compatible antibacterial modified montmorillonite; more than 5kg is prepared cumulatively; (2) Preparation of antibacterial masterbatch: Weigh 20 parts of spunbond polypropylene powder, 0.8 parts of KH570, and 18 parts of the antibacterial modified montmorillonite obtained in step (1), and stir them at a low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 136°C for zone 1, 139°C for zone 2, 156°C for zone 3, 176°C for zone 4, 197°C for zone 5, 200°C for zone 6, 196°C for zone 7, 197°C for zone 8, 198°C for zone 9, and 199°C for die head, the feed speed is 13.2 rpm / min, the main engine speed is 133 rpm / min, and the pelletizing speed is 375 rpm / min; (3) Preparation of antibacterial spunbond nonwoven fabrics: Add 10 parts of montmorillonite antibacterial masterbatch, 90 parts of spunbond polypropylene pellets, and 2 parts of masterbatch into the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drafting, and induced air cloth is formed. The spunbond process temperature in zones 1 to 6 is 185°C in zone 1, 227°C in zone 2, 239°C in zone 3, 241°C in zone 4, 241°C in zone 5, and 243°C in zone 6; the cooling, drafting, and blasting related parameters are melt cooling air 7°C; monomer 550 rpm / min; metering pump 24.1 Hz; suction 1150rpm / min. Web forming speed 201m / min; The finished antibacterial spunbond nonwoven fabrics were tested for appearance, width, weight, stretch and other performances. Example 3

[0039] Preparation of a non-dissolving antibacterial spunbonded nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 100 parts of sodium montmorillonite (200meq / 100g) and add 500 parts of anhydrous ethanol, and stir continuously to prepare suspension solution A; weigh 112.4 parts of cetylpyridinium chloride (2 times the cation exchange capacity) and put it into 500 parts of anhydrous methanol solvent and stir it with a magnetic stirrer for 1 hour to prepare mixed solution B; put grinding balls into a planetary ball mill, pour in mixed solutions A and B, the ratio of grinding balls is large (D14), medium (D10), small (D6) = 10:40:50, and the ball-to-material ratio is 70:30 and sealed; open the ball mill and heat at 500 rpm / min, grind forward for 1h, grind forward for 1h, then add 45 parts of polypropylene grafted maleic anhydride and 20 parts of polypropylene powder into the ball mill, continue grinding at 500r / min, continue grinding at 450r / min, reverse for 1.5h, and forward for 1.5h; the mixed slurry taken out from the ball mill is filtered and placed in a vacuum drying oven at 90℃ for 6h to obtain highly compatible antibacterial modified montmorillonite; more than 5kg is prepared cumulatively; (2) Preparation of antibacterial masterbatch: Weigh 20 parts of spunbond polypropylene powder, 0.6 parts of KH570, and 24 parts of the antibacterial modified montmorillonite obtained in step (1), and stir them at a low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 132°C for zone 1, 136°C for zone 2, 153°C for zone 3, 173°C for zone 4, 194°C for zone 5, 203°C for zone 6, 193°C for zone 7, 194°C for zone 8, 196°C for zone 9, and 198°C for die head, the feed speed is 14 rpm / min, the main engine speed is 116 rpm / min, and the pelletizing speed is 375 rpm / min; (3) Preparation of antibacterial spunbond nonwoven fabrics: Add 10 parts of montmorillonite antibacterial masterbatch, 60 parts of spunbond polypropylene pellets, and 3 parts of masterbatch into the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drawing, and induced air cloth formation, the spunbond process temperature in zones 1 to 6 is 181°C for zone 1, 223°C for zone 2, 235°C for zone 3, 237°C for zone 4, 238°C for zone 5, and 240°C for zone 6. The cooling, drawing, and blast related parameters are melt cooling air 5.5°C; monomer 580 rpm / min; metering pump 23.8 Hz; suction 1130 rpm / min. The web forming speed is 198m / min. The finished antibacterial spunbond nonwoven fabrics were tested for appearance, width, weight, stretch and other performances. Example 4

[0040] Preparation of a non-dissolving antibacterial spunbonded nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 100 parts of sodium montmorillonite (100meq / 100g), add 600 parts of anhydrous ethanol, and stir continuously to prepare suspension solution A; weigh 49.63 parts of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride (1 times the cation exchange amount) and put it into 290 parts of anhydrous ethanol solvent and stir it with a magnetic stirrer to prepare mixed solution B; put grinding balls into a planetary ball mill, pour in mixed solutions A and B, the ratio of grinding balls is large (D14), medium (D10), small (D6) = 20:40:40, and the ball-to-material ratio is 80:20 and sealed; open the ball mill and heat it at 500 rpm / min, grind forward for 1h, grind forward for 2h, then add 50g polypropylene grafted maleic anhydride and 20g polypropylene powder into the ball mill, continue grinding at 500r / min, reverse for 2h, and forward for 1h; the mixed slurry taken out from the ball mill is filtered and dried in a vacuum drying oven at 90℃ for 6h to obtain highly compatible antibacterial modified montmorillonite; more than 7kg is prepared cumulatively; (2) Preparation of antibacterial masterbatch: Weigh 20 parts of spunbond polypropylene powder, 1 part of KH560, and 20 parts of the antibacterial modified montmorillonite obtained in step (1), and stir them at low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 130°C for zone 1, 135°C for zone 2, 150°C for zone 3, 170°C for zone 4, 191°C for zone 5, 195°C for zone 6, 195°C for zone 7, 196°C for zone 8, 196°C for zone 9, and 197°C for die head, the feed speed is 13.8 rpm / min, the main engine speed is 118 rpm / min, and the pelletizing speed is 381 rpm / min; (3) Preparation of antibacterial spunbond nonwoven fabrics: Add 10 parts of montmorillonite antibacterial masterbatch and 60 parts of spunbond polypropylene pellets into the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drawing, and induced air forming, the spunbond process temperature in zones 1 to 6 is 180°C for zone 1, 220°C for zone 2, 230°C for zone 3, 230°C for zone 4, 230°C for zone 5, and 235°C for zone 6. The cooling, drawing, and blast related parameters are melt cooling air 4.2°C; monomer 530 rpm / min; metering pump 23.0 Hz; suction 1120 rpm / min. The web forming speed is 215m / min. The finished antibacterial spunbond nonwoven fabrics were tested for appearance, width, weight, stretch and other performances.

[0041] The temperature range in step (3) can fluctuate by 10°C, and the spunbond nonwoven fabric can be stably prepared. Example 5

[0042] Preparation of a non-dissolving antibacterial spunbonded nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 100 parts of sodium montmorillonite (100meq / 100g) and add 400 parts of anhydrous ethanol, and stir continuously to prepare suspension solution A; weigh 36.8 parts of tetradecyl dimethyl benzyl ammonium chloride (1 times the cation exchange amount) and put it into 120 parts of anhydrous ethanol solvent and stir it with a magnetic stirrer to prepare mixed solution B; put grinding balls in a planetary ball mill, pour in mixed solutions A and B, and the ratio of grinding balls is large (D14), medium (D10), and small (D6) = 1 0:30:60, the ball-to-material ratio is 77:23 and sealed; open the ball mill at 450rpm / min, grind forward for 2h, grind forward for 1h, then add 75 parts of polypropylene grafted maleic anhydride and 25 parts of polypropylene powder into the ball mill, continue to grind at 500r / min, reverse for 1h, and forward for 1h; filter the mixed slurry taken out from the ball mill and dry it in a vacuum drying oven at 80℃ for 8h to obtain highly compatible antibacterial modified montmorillonite; prepare more than 5kg cumulatively; (2) Preparation of antibacterial masterbatch: Weigh 20 parts of spunbond polypropylene powder, 1 part of KH560, and 22 parts of the highly compatible antibacterial modified montmorillonite obtained in step (1), and stir them at a low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 137°C for zone 1, 142°C for zone 2, 158°C for zone 3, 177°C for zone 4, 199°C for zone 5, 203°C for zone 6, 209°C for zone 7, 210°C for zone 8, 210°C for zone 9, and 209°C for die head, the feed speed is 12.1 rpm / min, the main engine speed is 115 rpm / min, and the pelletizing speed is 361 rpm / min; (3) Preparation of antibacterial spunbond nonwoven fabrics: Add 10 parts of montmorillonite antibacterial masterbatch, 60 parts of spunbond polypropylene pellets, and 1.5 parts of masterbatch to the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drafting, and induced air cloth formation, the spunbond process temperature in zones 1 to 6 is 194°C in zone 1, 232°C in zone 2, 240°C in zone 3, 241°C in zone 4, 243°C in zone 5, and 245°C in zone 6. The cooling, drafting, and blasting related parameters are melt cooling air 6°C; monomer 550 rpm / min; metering pump 23.1 Hz; suction 1210 rpm / min. Web forming speed 221m / min; The finished antibacterial spunbond nonwoven fabrics were tested for appearance, width, weight, stretch and other performances. Example 6

[0043] Preparation of a non-dissolving antibacterial spunbonded nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 100 parts of sodium montmorillonite (100meq / 100g), add 450 parts of anhydrous ethanol, and continue stirring to prepare suspension solution A; weigh 29.7 parts of hexadecylbenzyldimethylammonium chloride and 37.22 parts of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride (1.5 times the cation exchange capacity) and put them into 250 parts of anhydrous ethanol solvent and stir them with a magnetic stirrer to prepare mixed solution B; put grinding balls into a planetary ball mill, pour in mixed solutions A and B, the ratio of grinding balls is large (D14), medium (D10), small (D6) = 15:30:60, and the ball-to-material ratio is 74:26 and sealed; open the ball mill and heat at 500 rpm / min, grind forward for 1h, reverse grind for 1.5h, then add 45 parts of polypropylene grafted maleic anhydride and 30 parts of polypropylene powder into the ball mill, continue grinding at 500r / min, reverse for 1h, and forward for 1h; filter the mixed slurry taken out from the ball mill and dry it in a vacuum drying oven at 80℃ for 8h to obtain highly compatible antibacterial modified montmorillonite; more than 5kg is prepared cumulatively; (2) Preparation of antibacterial masterbatch: Weigh 20 parts of spunbond polypropylene powder, 0.9 parts of KH560, and 19 parts of the highly compatible antibacterial modified montmorillonite obtained in step (1), and stir them at a low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 137°C for zone 1, 140°C for zone 2, 155°C for zone 3, 176°C for zone 4, 193°C for zone 5, 201°C for zone 6, 205°C for zone 7, 207°C for zone 8, 209°C for zone 9, and 209°C for die head, the feed speed is 14 rpm / min, the main engine speed is 135 rpm / min, and the pelletizing speed is 356 rpm / min; (3) Preparation of antibacterial spunbond nonwoven fabrics: Add 10 parts of montmorillonite antibacterial masterbatch, 100 parts of spunbond polypropylene pellets, and 3 parts of masterbatch into the corresponding hopper and mix them evenly as the materials are discharged. After melt extrusion, side-blowing cooling, blast drawing, and induced air cloth formation. The spunbond process temperature in zones 1 to 6 is 189°C for zone 1, 228°C for zone 2, 244°C for zone 3, 245°C for zone 4, 241°C for zone 5, and 242°C for zone 6; the cooling, drawing, and blast related parameters are melt cooling air 6°C; monomer 600 rpm / min; metering pump 24 Hz; suction 1250rpm / min. Web forming speed 225m / min; The finished antibacterial spunbond nonwoven fabrics were tested for appearance, width, weight, stretch and other performances. Example 7

[0044] Preparation of a non-dissolving antibacterial spunbonded nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 100 parts of sodium montmorillonite (200meq / 100g), add 500 parts of anhydrous ethanol, and stir continuously to prepare suspension solution A; weigh 42.26 parts of cetylpyridinium chloride and 41.4 parts of tetradecyldimethylbenzyl ammonium chloride (1.5 times the cation exchange capacity), put them into 400ml of anhydrous ethanol solvent, stir with a magnetic stirrer to prepare mixed solution B; put grinding balls into a planetary ball mill, pour in mixed solution A and B, the ratio of grinding balls is large (D14), medium (D10), small (D6) = 12:26:62, and the ball-to-material ratio is 79:21 and sealed; open the ball mill and heat at 500 rpm / min, grind forward for 1h, reverse grind for 2h, then add 50 parts of polypropylene grafted maleic anhydride and 20 parts of polypropylene powder into the ball mill, continue grinding at 500r / min, reverse for 1.5h, and forward for 1.5h; the mixed slurry taken out from the ball mill is filtered and dried in a vacuum drying oven at 90℃ for 6h to obtain highly compatible antibacterial modified montmorillonite; more than 5kg is prepared cumulatively; (2) Preparation of antibacterial masterbatch: Weigh 20 parts of spunbond polypropylene powder, 0.9 parts of KH560, and 18 parts of the antibacterial modified montmorillonite obtained in step (1), and stir them at low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 136°C for zone 1, 139°C for zone 2, 156°C for zone 3, 176°C for zone 4, 197°C for zone 5, 200°C for zone 6, 196°C for zone 7, 197°C for zone 8, 198°C for zone 9, and 199°C for die head, the feed speed is 10 rpm / min, the main engine speed is 115 rpm / min, and the pelletizing speed is 355 rpm / min; (3) Preparation of antibacterial spunbond nonwoven fabrics: Add 10 parts of montmorillonite antibacterial masterbatch, 90 parts of spunbond polypropylene pellets, and 1.5 parts of masterbatch to the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drafting, and induced air cloth formation, the spunbond process temperature in zones 1 to 6 is 185°C for zone 1, 227°C for zone 2, 239°C for zone 3, 241°C for zone 4, 241°C for zone 5, and 243°C for zone 6. The cooling, drafting, and blasting related parameters are melt cooling air 7°C; monomer 550 rpm / min; metering pump 24.1 Hz; suction 1150 rpm / min. Web forming speed 201m / min; The finished antibacterial spunbond nonwoven fabrics were tested for appearance, width, weight, stretch and other performances.

[0045] Comparative Example 1 Preparation of a nonwoven fabric (1) Preparation of spunbond nonwoven fabrics: 39.88 parts of polypropylene and 0.12 parts of masterbatch are added to the corresponding hopper and mixed evenly with the materials. After melt extrusion, side blowing cooling, blast drawing, and induced air cloth is formed. The spunbond process temperature in zones 1 to 6 is 186°C for zone 1, 224°C for zone 2, 235°C for zone 3, 236°C for zone 4, 237°C for zone 5, and 239°C for zone 6; the cooling, drawing, and blast related parameters are melt cooling air 7°C; monomer 600 rpm / min; metering pump 23.1 Hz; suction 950 rpm / min. The web forming speed is 225m / min; (2) Antibacterial modification: The spunbond nonwoven fabric obtained in step (1) was immersed in an aqueous solution containing 1% dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride for 30 min and dried at 80°C.

[0046] The finished non-woven fabrics will be tested for appearance, width, weight, stretch and other performance.

[0047] Comparative Example 2 Preparation of a nonwoven fabric (1) Preparation of modified montmorillonite: Weigh 100 parts of sodium montmorillonite (200meq / 100g) and add 500 parts of anhydrous ethanol, and stir continuously to obtain suspension solution A; put grinding balls in a planetary ball mill, pour in mixed solution A, the ratio of grinding balls is large (D14), medium (D10), small (D6) = 10:25:65, and the ball-to-material ratio is 80:20 and sealed; open the ball mill and grind at 500 rpm / min, forward rotation for 1 hour, then add mixed solution A, 50 parts of polypropylene grafted maleic anhydride, and 20 parts of polypropylene powder into the ball mill, continue to grind at 500r / min, reverse for 1.5 hours, and forward for 1.5 hours; put the mixed slurry taken out of the ball mill in a vacuum drying oven at 90°C and dry for 6 hours to obtain modified montmorillonite; cumulative preparation of more than 5kg; (2) Masterbatch preparation: Weigh 20 parts of spunbond polypropylene powder, 0.9 parts of KH560, and 18 parts of the modified montmorillonite obtained in step (1), and stir them at low speed in a high-speed mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 140°C for zone 1, 143°C for zone 2, 157°C for zone 3, 178°C for zone 4, 198°C for zone 5, 205°C for zone 6, 200°C for zone 7, 199°C for zone 8, 199°C for zone 9, and 200°C for die head, the feed speed is 14 rpm / min, the main engine speed is 122 rpm / min, and the pelletizing speed is 355 rpm / min; (3) Non-woven fabric preparation: 10 parts of montmorillonite masterbatch, 45 parts of spunbond polypropylene pellets, and 1.5 parts of masterbatch are added to the corresponding hopper and mixed evenly with the materials. After melt extrusion, side-blowing cooling, blast drawing, and induced air cloth is formed. The spunbond process temperature in zones 1 to 6 is 191°C for zone 1, 228°C for zone 2, 237°C for zone 3, 239°C for zone 4, 240°C for zone 5, and 243°C for zone 6; the cooling, drawing, and blast related parameters are melt cooling air 7°C; monomer 590 rpm / min; metering pump 24 Hz; suction 1250 rpm / min. Web forming speed 209m / min; The prepared non-woven fabric products are tested for appearance, width, weight, stretch and other performance.

[0048] Comparative Example 3 Preparation of a nonwoven fabric (1) Masterbatch preparation: Weigh 82.5 parts of spunbond polypropylene powder, 2 parts of sodium montmorillonite, 6 parts of PP-G-MAH, 8 parts of cetylpyridinium chloride antibacterial agent powder, and 1.5 parts of KH560, and stir them at low speed in a high mixing pot for 1 hour; pour the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 138°C in zone 1, 142°C in zone 2, 157°C in zone 3, 176°C in zone 4, 185°C in zone 5, 185°C in zone 6, 195°C in zone 7, 198°C in zone 8, 198°C in zone 9, and 197°C in die head, feed 14 rpm / min, main engine speed 122rpm / min, and pelletizing speed 355rpm / min; (2) Non-woven fabric preparation: Add 10 parts of montmorillonite antibacterial masterbatch, 45 parts of spunbond polypropylene pellets, and 1 part of masterbatch to the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drafting, and induced air cloth is formed. The spunbond process temperature in zones 1 to 6 is 186°C for zone 1, 228°C for zone 2, 229°C for zone 3, 230°C for zone 4, 230°C for zone 5, and 230°C for zone 6; the cooling, drafting, and blasting related parameters are melt cooling air 7°C; monomer 590 rpm / min; metering pump 24 Hz; suction 1250rpm / min. Web forming speed 209m / min; The prepared non-woven fabric products are tested for appearance, width, weight, stretch and other performances.

[0049] Comparative Example 4 Preparation of a nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 100 parts of sodium montmorillonite (100meq / 100g), add 500 parts of anhydrous ethanol, and stir continuously to obtain a suspension solution A; weigh 36.8 parts of tetradecyl dimethyl benzyl ammonium chloride (1 times the cation exchange amount) and put it into 120 parts of anhydrous ethanol solvent and stir it with a magnetic stirrer to obtain a mixed solution B; put grinding balls into a planetary ball mill, pour in the mixed solution A and B, the ratio of the grinding balls is large (D14), medium (D10), small (D6) = 10:25:65, and the ball-to-material ratio is 80:20 and sealed; turn on the ball mill and grind at 500rpm / min, forward for 1h, reverse for 2h, then add 80 parts of polypropylene powder into the ball mill, continue to grind at 500r / min, reverse for 1h, and forward for 1h; filter the mixed slurry taken out of the ball mill and dry it in a vacuum drying oven at 80°C for 8h to obtain antibacterial modified montmorillonite; prepare more than 5kg cumulatively; (2) Masterbatch preparation: Weigh 20 parts of spunbond polypropylene powder, 0.8 parts of KH570, and 18 parts of the antibacterial modified montmorillonite obtained in step (1), and stir them at a low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 136°C for zone 1, 140°C for zone 2, 148°C for zone 3, 167°C for zone 4, 189°C for zone 5, 193°C for zone 6, 201°C for zone 7, 205°C for zone 8, 205°C for zone 9, and 205°C for die head, the feed speed is 12.1 rpm / min, the main engine speed is 115 rpm / min, and the pelletizing speed is 361 rpm / min; (3) Non-woven fabric preparation: Add 10 parts of montmorillonite antibacterial masterbatch, 90 parts of spunbond polypropylene pellets, and 2 parts of masterbatch into the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drafting, and induced draft, the fabric is formed. The spunbond process temperature in zones 1 to 6 is 185°C for zone 1, 225°C for zone 2, 235°C for zone 3, 235°C for zone 4, 235°C for zone 5, and 235°C for zone 6; the cooling, drafting, and blasting related parameters are melt cooling air 6°C; monomer 550 rpm / min; metering pump 23.1 Hz; suction 1210rpm / min. The web forming speed is 221m / min; The prepared non-woven fabric products are tested for appearance, width, weight, stretch and other performances.

[0050] Comparative Example 5 Preparation of a nonwoven fabric (1) Preparation of antibacterial agents: Weigh 57.6 parts of cetylpyridine bromide and put it into 200 parts of anhydrous ethanol solvent and stir it in a magnetic stirrer to prepare a mixed solution B; put grinding balls in a planetary ball mill and pour in the mixed solution B, the ratio of the grinding balls is large (D14), medium (D10), small (D6) = 10:25:65, and the ball-to-material ratio is 80:20 and sealed; open the ball mill and grind it at 500 rpm / min, forward for 1 hour, then add 50 parts of polypropylene grafted maleic anhydride and 30 parts of polypropylene powder into the ball mill, continue to grind at 500r / min, reverse for 1 hour, and forward for 1 hour; filter the mixed slurry taken out of the ball mill and dry it in a vacuum drying oven at 80°C for 8 hours to obtain an antibacterial agent; prepare more than 5kg cumulatively; (2) Masterbatch preparation: Weigh 20 parts of spunbond polypropylene powder, 0.8 parts of KH570, and 18 parts of the antibacterial agent obtained in step (1), and stir them at low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 135°C for zone 1, 140°C for zone 2, 145°C for zone 3, 175°C for zone 4, 185°C for zone 5, 195°C for zone 6, 195°C for zone 7, 195°C for zone 8, 200°C for zone 9, and 200°C for die head, the feed speed is 12.1 rpm / min, the main engine speed is 115 rpm / min, and the pelletizing speed is 361 rpm / min; (3) Non-woven fabric preparation: Add 10 parts of antibacterial masterbatch, 90 parts of spunbond polypropylene pellets, and 2 parts of masterbatch into the corresponding hopper and mix them evenly as the materials are discharged. After melt extrusion, side-blowing cooling, blast drafting, and induced air cloth formation, the spunbond process temperature in zones 1 to 6 is 175°C for zone 1, 215°C for zone 2, 225°C for zone 3, 225°C for zone 4, 225°C for zone 5, and 225°C for zone 6. The cooling, drafting, and blasting related parameters are melt cooling air 6°C; monomer 550 rpm / min; metering pump 23.1 Hz; suction 1210 rpm / min. Web forming speed 221m / min; The prepared non-woven fabric products are tested for appearance, width, weight, stretch and other performances.

[0051] Comparative Example 6 Preparation of a nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 100 parts of sodium montmorillonite (100meq / 100g) and add 500 parts of anhydrous ethanol, and stir continuously to obtain suspension solution A; weigh 23.5 parts of p-chloro-m-xylenol (1.5 times the cation exchange capacity) and put it into 100 parts of anhydrous ethanol solvent and stir it with a magnetic stirrer to obtain mixed solution B; put grinding balls into a planetary ball mill, pour in mixed solutions A and B, the ratio of grinding balls is large (D14): small (D6) = 15:85, and the ball-to-material ratio is 80:20 and sealed; turn on the ball mill and grind at 500 rpm / min, forward for 1.5h, then add 50 parts of polypropylene grafted maleic anhydride and 30 parts of polypropylene powder into the ball mill, continue grinding at 500r / min, reverse for 0.5h, and forward for 0.5h; filter the mixed slurry taken out of the ball mill and dry it in a vacuum drying oven at 80°C for 8h to obtain antibacterial modified montmorillonite; prepare more than 5kg cumulatively; (2) Masterbatch preparation: Weigh 20 parts of spunbond polypropylene powder, 0.8 parts of KH570, and 18 parts of the antibacterial modified montmorillonite obtained in step (1), and stir them at a low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 139°C for zone 1, 144°C for zone 2, 155°C for zone 3, 180°C for zone 4, 199°C for zone 5, 203°C for zone 6, 208°C for zone 7, 208°C for zone 8, 210°C for zone 9, and 210°C for die head, the feed speed is 12.1 rpm / min, the main engine speed is 115 rpm / min, and the pelletizing speed is 361 rpm / min; (3) Non-woven fabric preparation: Add 10 parts of montmorillonite antibacterial masterbatch, 90 parts of spunbond polypropylene pellets, and 2 parts of masterbatch into the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drawing, and induced air cloth is formed. The spunbond process temperature in zones 1 to 6 is 190°C in zone 1, 230°C in zone 2, 241°C in zone 3, 241°C in zone 4, 243°C in zone 5, and 245°C in zone 6; the cooling, drawing, and blast related parameters are melt cooling air 6°C; monomer 550 rpm / min; metering pump 23.1 Hz; suction 1210rpm / min. Web forming speed 221m / min; The prepared non-woven fabric products are tested for appearance, width, weight, stretch and other performances.

[0052] Comparative Example 7 Preparation of a nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 36.8 parts of tetradecyl dimethyl benzyl ammonium chloride and put it into 200 parts of anhydrous ethanol solvent and stir it in a magnetic stirrer to prepare a mixed solution B; put grinding balls in a planetary ball mill and pour in the mixed solution B, the ratio of the grinding balls is large (D14), medium (D10), small (D6) = 10:25:65, and the ball-to-material ratio is 50:50 and sealed; open the ball mill and grind it at 200 rpm / min, forward for 1 hour, and reverse for 1 hour, then add 50 parts of polypropylene grafted maleic anhydride and 20 parts of polypropylene powder into the ball mill, continue to grind at 300r / min, reverse for 1 hour, and forward for 1 hour; filter the mixed slurry taken out of the ball mill and dry it in a vacuum drying oven at 80°C for 8 hours to obtain antibacterial modified montmorillonite; prepare more than 5kg cumulatively; (2) Masterbatch preparation: Weigh 20 parts of spunbond polypropylene powder, 0.8 parts of KH560, and 18 parts of the antibacterial modified montmorillonite obtained in step (1), and stir them at low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 143°C for zone 1, 147°C for zone 2, 159°C for zone 3, 179°C for zone 4, 199°C for zone 5, 204°C for zone 6, 209°C for zone 7, 209°C for zone 8, 210°C for zone 9, and 210°C for die head, the feed speed is 12.1 rpm / min, the main engine speed is 115 rpm / min, and the pelletizing speed is 361 rpm / min; (3) Non-woven fabric preparation: Add 10 parts of montmorillonite antibacterial masterbatch, 90 parts of spunbond polypropylene pellets, and 1 part of masterbatch to the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drawing, and induced air cloth is formed. The spunbond process temperature in zones 1 to 6 is 194°C in zone 1, 232°C in zone 2, 240°C in zone 3, 241°C in zone 4, 243°C in zone 5, and 245°C in zone 6; the cooling, drawing, and blast related parameters are melt cooling air 6°C; monomer 550 rpm / min; metering pump 23.1 Hz; suction 1210rpm / min. Web forming speed 221m / min; The prepared non-woven fabric products are tested for appearance, width, weight, stretch and other performances.

[0053] Comparative Example 8 Preparation of a nonwoven fabric (1) Preparation of antibacterial modified montmorillonite: Weigh 100 parts of sodium montmorillonite (100meq / 100g), add 500 parts of anhydrous ethanol, and stir continuously to obtain suspension solution A; weigh 39.6 parts of hexadecylbenzyldimethylammonium chloride, add 130 parts of anhydrous ethanol solvent, stir in a magnetic stirrer to obtain mixed solution B; put grinding balls in a planetary ball mill, pour mixed solutions A and B, the ratio of grinding balls is large (D14), medium (D10), small (D6) = 10:25:65, and the ball-to-material ratio is 80:20 and sealed; open the ball mill and grind at 500 rpm / min, forward for 1h, reverse for 1.5h, then add 50 parts of polypropylene grafted maleic anhydride and 25 parts of polypropylene powder into the ball mill, continue to grind at 500r / min, reverse for 1h, and forward for 1h; filter the mixed slurry taken out of the ball mill and dry it in a vacuum drying oven at 80°C for 8h to obtain antibacterial modified montmorillonite; prepare more than 5kg cumulatively; (2) Masterbatch preparation: Weigh 20 parts of spunbond polypropylene powder and 18 parts of the antibacterial modified montmorillonite obtained in step (1), stir them at low speed in a high mixing pot for 1 minute; introduce the stirred pellets into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 144°C for zone 1, 149°C for zone 2, 159°C for zone 3, 177°C for zone 4, 199°C for zone 5, 203°C for zone 6, 209°C for zone 7, 209°C for zone 8, 210°C for zone 9, and 215°C for die head, the feed speed is 12.1 rpm / min, the main engine speed is 115 rpm / min, and the pelletizing speed is 361 rpm / min; (3) Non-woven fabric preparation: Add 10 parts of montmorillonite antibacterial masterbatch, 90 parts of spunbond polypropylene pellets, and 1.5 parts of masterbatch to the corresponding hopper and mix them evenly as the materials are fed. After melt extrusion, side-blowing cooling, blast drafting, and induced air cloth formation, the spunbond process temperature in zones 1 to 6 is 194°C in zone 1, 232°C in zone 2, 240°C in zone 3, 241°C in zone 4, 243°C in zone 5, and 245°C in zone 6. The cooling, drafting, and blasting related parameters are melt cooling air 6°C; monomer 550 rpm / min; metering pump 23.1 Hz; suction 1210 rpm / min. Web forming speed 221m / min; The prepared non-woven fabric products are tested for appearance, width, weight, stretch and other performances. Implementation Effect

[0054] The nonwoven fabrics obtained in the above examples and comparative examples were subjected to the following performance tests, respectively. The test results are shown in Tables 1 and 2.

[0055] 1. Biological performance test (1) Antibacterial test: the test is carried out in accordance with GB / T 15979 "Hygiene Standard for Disposable Sanitary Products".

[0056] (2) Cytotoxicity test: refer to GB / T 16886.5-2017 “Biological evaluation of medical devices Part 5: In vitro cytotoxicity test”.

[0057] Table 1 Antibacterial rate and cytotoxicity test results of non-woven fabric examples and comparative examples

[0058] It can be seen from the test results that the antibacterial spunbonded nonwoven fabric obtained by the preparation process provided by the present invention has good antibacterial properties and low cytotoxicity, which is mainly due to the fact that the cationic antibacterial agent can be firmly fixed in the montmorillonite intercalation layer and uniformly dispersed in the resin matrix without dissolving or falling off; the processing temperature range is relatively wide, which is mainly due to the fact that the antibacterial modified montmorillonite has a relatively high thermal stability and can be uniformly dispersed in the resin matrix. Comparative Example 1 uses a post-treatment method to prepare an antibacterial spunbonded non-woven fabric. The obtained non-woven fabric has antibacterial properties but has high cytotoxicity and poor antibacterial effect. This is mainly due to the fact that the non-woven fabric is post-treated by solution immersion, and the antibacterial agent is mainly on the surface of the spunbonded non-woven fabric, and the antibacterial agent is easy to fall off and dissolve; Comparative Example 2 only adds sodium montmorillonite, and no cationic antibacterial agent is intercalated, and the obtained spunbonded non-woven fabric has no antibacterial properties; Comparative Example 3 directly blends polypropylene with an antibacterial agent to prepare an antibacterial masterbatch, and the prepared material has relatively low antibacterial properties, mainly because the antibacterial agent fails to be fully and completely intercalated into montmorillonite, has poor compatibility, and is unevenly dispersed. Part of the antibacterial agent accumulates at the filter screen before the screw and is filtered out during processing. In addition, the antibacterial agent is partially decomposed during high-temperature processing, resulting in low antibacterial properties and high cytotoxicity. In the preparation process of the antibacterial modified montmorillonite in Comparative Example 4, PP-G-MAH was not added, resulting in PP-G-MAH not being intercalated into the montmorillonite, so that the inorganic material montmorillonite could not be effectively dispersed and compatible in the resin PP matrix, resulting in the agglomeration of the montmorillonite, which in turn caused the pores to be blocked during the spinning process and the filter screen to filter out most of the antibacterial components. In Comparative Example 5, no montmorillonite was added during the preparation process of the antibacterial modified montmorillonite, so that the antibacterial agent could not be embedded in the intercalation layer, and could not be protected by the montmorillonite intercalation layer, so that it was easily decomposed during the high-temperature processing, losing its antibacterial properties, and the toxic substances produced by the decomposition caused greater cytotoxicity. In the preparation process of the antibacterial modified montmorillonite in Comparative Example 6, the grinding balls only have large balls and small balls, and the grinding is insufficient, resulting in insufficient and incomplete contact between the montmorillonite and the antibacterial agent, and most of the antibacterial agents fail to be intercalated into the montmorillonite layer, and the antibacterial agent is a non-cationic antibacterial agent, which cannot fully form ion exchange with the sodium-based montmorillonite, and cannot be fully and effectively intercalated into the montmorillonite layer, resulting in its antibacterial property and biosafety failing to achieve the target effect. In the preparation process of the antibacterial modified montmorillonite in Comparative Example 7, the grinding rate is low, and the ball-to-material ratio is low, resulting in insufficient and incomplete contact between the montmorillonite and the antibacterial agent, and most of the antibacterial agents fail to be intercalated into the montmorillonite layer, and the antibacterial property and biosafety fail to achieve the target effect. In Comparative Example 8, the antibacterial masterbatch is not added with a coupling agent during the preparation process, so that the dispersion and compatibility of the antibacterial modified montmorillonite in the resin PP are subject to certain restrictions, resulting in the agglomeration of the montmorillonite, which in turn causes the occurrence of plugging holes in the spinning process and the filter screen filtering out some antibacterial components.

[0059] In addition, it can be seen from the processing technology of the embodiments and the comparative examples that the processing temperature range of embodiments 1-7 is larger, the processing temperature range of the comparative example is relatively small, and the comparative examples 3, 5, 6, and 7 in which the antibacterial agent is not fully and completely intercalated with the montmorillonite need to reduce the processing temperature to reduce the decomposition of the antibacterial agent, but the temperature reduction cannot completely inhibit the decomposition of the antibacterial agent, and low-temperature processing will affect the spinning stability. The preparation method provided by the present invention uses antibacterial modified montmorillonite with good compatibility with polypropylene and is less sensitive to processing technology.

[0060] Figure 1 A schematic diagram of the modification mechanism of montmorillonite is given in the article. Taking the chain quaternary ammonium salt molecules as an example, the lamellar montmorillonite layers are easier to separate during ball milling in a solution environment. The Na ions in the layers exchange ions with the quaternary ammonium salt cation N ions. The quaternary ammonium salt molecules enter between the montmorillonite layers, increasing the interlamellar spacing of the montmorillonite and remain between the layers. The grinding time is prolonged, and the polypropylene and the polypropylene-grafted maleic anhydride part enter the layers.

[0061] from Figure 3 and Figure 4 It can be seen that after ball milling and intercalation, the (001) plane diffraction angle of the nano-montmorillonite decreases from a minimum of 7.08° to 2.52°, and the interlayer spacing increases from 1.45nm to 3.50nm, and it becomes broadened, and a mixed peak appears, indicating that a large amount of quaternary ammonium antibacterial agent is intercalated into the interlayer of the montmorillonite, which fully changes the interlayer spacing of the lamellae and reduces the regularity of the interlayers. After adding PP and PP-G-MAH, the interlayer spacing of the montmorillonite increases further, and the (001) plane diffraction angle decreases from a minimum of 2.52° to 2.28°, and the interlayer spacing increases further to 3.87nm, which may be due to the entry of some PP molecular chains into the lamellae, further expanding the lamellae. After quaternary ammonium salt intercalation, at 2917.45cm -1 ,2849.23cm -1 The CH stretching vibration peaks of -CH2 and -CH3 appeared at 1467.02 cm -1 The CH in-plane bending vibration peaks of -CH2 and -CH3 appeared, indicating that the quaternary ammonium antibacterial agent has been successfully intercalated into the interlayers of montmorillonite.

[0062] Figure 2A schematic diagram of the granulation mechanism of antibacterial masterbatch is given. When the cationic modified montmorillonite and the polypropylene molecular chain are melt extruded, more long-chain polypropylene molecular chains enter between the sheets, further increasing the interlayer spacing of the polypropylene. The maleic anhydride and coupling agent grafted on the exposed polypropylene inside and outside promote the compatibility between the polypropylene and the montmorillonite. Since the quaternary ammonium salt replaces the interlayer cation and connects with the interlayer molecules, the cationic antibacterial agent in the montmorillonite with enlarged or partially peeled sheets can be stably fixed. In addition, the mutual entanglement between the organic molecular chains can further increase the firmness of the antibacterial agent. Therefore, the quaternary ammonium salt molecules are evenly and firmly combined between the polypropylene.

[0063] The antibacterial spunbonded nonwoven fabric provided by the present invention has excellent antibacterial properties, and biological safety can also be guaranteed. The antibacterial properties are shown in Table 2 and Figure 7 shown.

[0064] Attached Figure 7 In the figure, the left side shows the experimental results of the antibacterial ring of Escherichia coli and the right side shows the antibacterial ring of Staphylococcus aureus. The middle point is the non-antibacterial spunbond non-woven fabric, and the three positions around it are samples of non-soluble antibacterial spunbond non-woven fabric. It can be seen from the figure that the non-soluble antibacterial spunbond non-woven fabric has no antibacterial ring, which shows that the antibacterial non-woven fabric is non-soluble antibacterial.

[0065] 2. Physical properties test: The spunbond nonwoven fabric was tested for weight, tensile strength and other properties. The test results are shown in Table 3 and Attachment Figure 5 , Attachment Figure 6 ; Gram weight: GBT 24218.1-2009 Textile nonwoven fabric test methods Part 1: Determination of mass per unit area; Tensile properties: GB / T 24218.3-2010 Textile nonwoven fabric test methods Part 3: Determination of breaking strength and breaking elongation. Table 2 shows the test results of nonwoven fabric physical properties:

[0066] It can be seen from Table 3 that the mechanical properties of the non-woven fabric prepared by the preparation process provided by the present invention are significantly improved in strength and toughness compared with conventional non-woven fabrics, with an improvement ratio of more than 20%. The improvement in mechanical properties is due to the fact that the modified nano-montmorillonite not only promotes compatibility but also promotes the crystallization of polypropylene during the stretching process, making the polypropylene crystallization more sufficient. The mechanical properties of the non-woven fabrics prepared in the comparative example are generally low, mainly due to the poor compatibility of the various components of the material, poor dispersibility, and the decomposition and degradation of some substances during the processing process, which affects the quality and stability of spinning.

[0067] Combination Figure 5 and Figure 6It can be seen that as the spunbond nonwoven fabric is stretched, the slope of the transverse breaking force gradually decreases. After experiencing steady elongation, the fibers are connected and then broken, indicating that the fibers themselves are well entangled. When the overall strength decreases, the fibers will still maintain a certain strength to allow the material to further stretch. The longitudinal displacement is relatively small, which is due to the full crystallization of the fibers during the production of the nonwoven fabric. The reason for the increase in strength is firstly due to the addition of nano-montmorillonite, which can promote the crystallization of polypropylene during the cooling and stretching process, making the arrangement of the molecular chains more regular and orderly; secondly, because the modified montmorillonite has high compatibility with polypropylene, it is overall uniform and is not easy to phase separate during the stretching process; finally, nano-montmorillonite itself is a rigid inorganic substance, and its own rigidity also has an enhancing effect on the strength of the nonwoven fabric, which is fully reflected under the premise of good compatibility.

[0068] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A non-dissolving antibacterial spunbonded nonwoven fabric, characterized in that: The antibacterial modified montmorillonite is prepared by a spunbonding process using polypropylene, antibacterial modified montmorillonite and a silane coupling agent as main raw materials; the antibacterial modified montmorillonite is obtained by inserting a cationic antibacterial agent, polypropylene grafted maleic anhydride and polypropylene powder between its sheets using montmorillonite as a carrier through a mechanical grinding method.

2. The non-dissolving antibacterial spunbonded nonwoven fabric according to claim 1, characterized in that: It has antibacterial properties, with an inhibition rate of >65% against Staphylococcus aureus, >65% against Escherichia coli, >50% against Candida albicans, and a cell survival rate of >92%; it has excellent mechanical strength, with a lateral elongation of 95-110% and a lateral breaking force of 40-47N; the longitudinal elongation is 75-85% and the longitudinal breaking force is 90-100N.

3. A process for preparing the non-dissolving antibacterial spunbonded nonwoven fabric according to claim 1 or 2, characterized in that: The following steps are involved: S1, adding montmorillonite alcohol solution A and cationic antibacterial agent alcohol solution B to a ball mill in proportion, grinding and reacting for a period of time, adding polypropylene powder and polypropylene grafted maleic anhydride in proportion, and continuing grinding, drying and crushing to obtain antibacterial modified montmorillonite; S2, mixing the antibacterial modified montmorillonite, polypropylene powder and silane coupling agent in S1 in proportion, and forming an antibacterial masterbatch after extrusion and cutting by an extruder; S3, the antibacterial masterbatch, polypropylene and color masterbatch described in S2 are mixed in proportion, and then melted, spun, initially pressed and hot rolled to obtain a non-dissolving antibacterial spunbonded nonwoven fabric.

4. The preparation process according to claim 3, characterized in that: The ratio of montmorillonite to solvent in the montmorillonite alcohol solution A in S1 is 1:5-10, and the amount of montmorillonite added is 3-5 parts; the ratio of cationic antibacterial agent to solvent in the antibacterial agent alcohol solution B is 1:3-5, and the amount of cationic antibacterial agent added is 1-6 parts; the amount of polypropylene powder added is 1 part; the amount of polypropylene grafted maleic anhydride added is 1.5-3 parts; wherein the raw material components are measured in parts by weight.

5. The preparation process according to claim 3, characterized in that: The montmorillonite in S1 includes sodium montmorillonite with an ion exchange capacity of 100-200 meq / 100g; the cationic antibacterial agent includes any one or more of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, cetylpyridinium bromide, cetylpyridinium chloride, tetradecyldimethylbenzylammonium chloride, and cetyldimethylbenzylammonium chloride; the solvent includes any one or more of anhydrous ethanol and methanol.

6. The preparation process according to claim 3, characterized in that: The antibacterial modified montmorillonite, polypropylene powder and silane coupling agent added in S2 are in a ratio of 1:0.8-1.2:0.03-0.05; the coupling agent mainly includes any one or two of γ-methacryloxypropyltrimethoxysilane (KH560) and γ-glycidyloxypropyltrimethoxysilane (KH570); wherein the raw material components are measured in parts by weight.

7. The preparation process according to claim 3, characterized in that: The ratio of the antibacterial masterbatch, polypropylene and color masterbatch added in S3 is 1:6-10:0-0.3; wherein the raw material components are calculated by weight.

8. The preparation process according to any one of claims 4 to 7, characterized in that: The mass ratio of large, medium and small agate balls used in the ball mill described in S1 is 10-20:25-40:40-65; the overall ball-to-material ratio is 70-80:20-30, the ball milling speed is 400-500rpm, and after the A and B solutions are mixed, the ball milling time is 1-2h in the forward direction and 1-2h in the reverse direction; after the polypropylene grafted maleic anhydride and polypropylene powder are added, the ball milling time is 1-2h in the reverse direction and 1-2h in the forward direction; after the ball milling, the ball milling is dried for 6-8h at a drying temperature of 80-90°C.

9. The preparation process according to claim 8, characterized in that: The antibacterial masterbatch extrusion parameters described in S2 include: stirring at low speed in a high mixing pot for 1 minute; introducing the stirred raw materials into a twin-screw extruder, the temperatures of the ten zones of the twin-screw extruder are 140±10℃ for zone 1, 145±10℃ for zone 2, 155±5℃ for zone 3, 180±10℃ for zone 4, 195±5℃ for zone 5, 200±5℃ for zone 6, 205±10℃ for zone 7, 205±10℃ for zone 8, 205±10℃ for zone 9, and 205±10℃ for the die head, the feeding speed is 12±2rpm / min, the main engine speed is 120±15 rpm / min, and the pelletizing speed is 370±20rpm / min.

10. The preparation process according to claim 9, characterized in that: The extrusion parameters of the non-dissolving antibacterial spunbond nonwoven fabric described in S3 include: the spunbond process temperatures in zones 1 to 6 are 185±10°C for zone 1, 225±10°C for zone 2, 235±10°C for zone 3, 235±10°C for zone 4, 235±10°C for zone 5, and 235±10°C for zone 6; the cooling, stretching, and blasting related parameters are melt cooling air 6±2°C; monomer 550±50 rpm / min; metering pump 24±1 Hz; suction 1150±100 rpm / min; and web forming speed 215±15m / min.

11. An application of the non-dissolving antibacterial spunbonded nonwoven fabric according to claim 1 or 2, characterized in that: Antibacterial spunbond meltblown composite nonwoven fabric, antibacterial coated nonwoven fabric and antibacterial coated nonwoven fabric are prepared by superimposing and compounding with meltblown nonwoven fabric, breathable film and coating layer.

Citation Information

Patent Citations

  • Functional nylon 66 fiber and preparation method thereof

    CN103882548A

  • Preparation method of composite antibacterial agent and antibacterial plastic

    CN113292688A

  • Flame-retardant antibacterial non-woven fabric and preparation method thereof

    CN114775169A

  • Polypropylene / clay nano complex substance and its preparation method and application

    CN1493607A

  • Process for preparing limellar stripping nano imvite

    CN1792791A