Method for reducing pilling of regenerated polyester-cotton knitted napped fabric

By adjusting the raising agent and process parameters, combined with the steel wire raising machine and dry setting treatment, the problem of easy pilling of recycled polyester-cotton knitted brushed flannel after washing has been solved, and the fluff effect and anti-pilling performance have been improved, which is in line with environmental protection. and sustainable development requirements.

CN118727337APending Publication Date: 2024-10-01ZHEJIANG YINHE PRINTING & DYEING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410715272.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Regenerated polyester-cotton knitted brushed velvet fabric is prone to pilling after washing, which affects its use effect and environmental performance.

Method used

By adjusting the raising agent and raising process parameters, a steel wire raising machine is used for three consecutive passes. The cylinder speed and raising roller speed of the third pass are lower than those of the first two passes, and the squat roller speed is higher than the first two passes. During the process Add fluffing agent and softener, combined with dry styling treatment to reduce pilling.

Benefits of technology

Significantly improves the pile effect and anti-pilling performance of the recycled polyester-cotton knitted brushed flannel, enhances its wear resistance and service life, and meets the requirements of environmental protection and sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004875406190000061
    Figure BDA0004875406190000061
  • Figure BDA0004875406190000062
    Figure BDA0004875406190000062
  • Figure BDA0004875406190000071
    Figure BDA0004875406190000071
Patent Text Reader

Abstract

The invention relates to the technical field of textile finishing, and provides a method for reducing pilling of a regenerated polyester-cotton knitted napped fabric aiming at the problem that the suede surface of the regenerated polyester-cotton knitted napped fabric is easy to pilling after being washed, and the method comprises the following steps: (1) treating a gray fabric containing regenerated polyester by using a fuzzing agent; (2) carrying out napping and raising on the gray fabric by using a steel wire napping machine, continuously carrying out napping for three times, enabling the cylinder rotating speed and the napping roller rotating speed of the third time to be lower than those of the previous two times, and enabling the squatting roller rotating speed of the third time to be higher than those of the previous two times; and (3) shearing, and carrying out dry setting to obtain the regenerated polyester-cotton knitted napped fabric. According to the invention, by adjusting the fuzzing agent and fuzzing process parameters, the prepared regenerated polyester-cotton knitted napped fabric has excellent fluff effect and anti-pilling and wear-resisting properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile finishing, in particular to a method for reducing pilling of recycled polyester-cotton knitted brushed fleece. Background Art

[0002] Recycled polyester is a green and environmentally friendly polyester fiber made from old polyester fabrics or polyester bottle flakes and other waste materials. With the promotion of sustainable development and low-carbon economy concepts, the polyester fiber of conventional knitted polyester-cotton blended fabrics has gradually been replaced by recycled polyester, and the proportion of recycled polyester fiber is increasing year by year.

[0003] When the knitted grey fabric replaced by recycled polyester is dyed and finished, since its characteristics have not changed and it is still polyester fiber, the raw material additives and dyeing and finishing process required for dyeing are the same as those of conventional polyester-cotton fabric. For example, Chinese patent CN103614785A discloses a process for preparing recycled polyester, and its process steps are as follows: 1) firstly, the recycled polyester raw material is dried; 2) the recycled polyester after drying is melt-extruded by a screw; 3) the extruded recycled polyester is filtered in two stages with high precision to remove inorganic impurities; 4) after high precision filtration, it is depolymerized in a reactor to break the molecular chain, and then repolymerized, and organic impurities are removed in vacuum; 5) after passing through a spinning box, the spinning process is carried out. The process steps of the present invention are simple, high precision filtration is used, and inorganic impurities are removed by physical methods, and then organic small molecule impurities are removed in vacuum by a combination of chemical and physical methods, the viscosity of the polyester melt is changed, and the quality of the polyester melt is improved. However, the recycled polyester-cotton knitted flannel obtained by the conventional raising process is easy to pill after washing, and an ideal solution is needed. Summary of the invention

[0004] The invention aims to overcome the problem that the napped surface of recycled polyester-cotton knitted brushed fleece is easy to pilling after washing, and provides a method for reducing the pilling of recycled polyester-cotton knitted brushed fleece. By adjusting a raising agent and raising process parameters, the obtained recycled polyester-cotton knitted brushed fleece has excellent fluff effect, anti-pilling and wear resistance.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: The method for reducing pilling of recycled polyester-cotton knitted brushed fleece fabric comprises the following steps: 1) First treat the grey fabric containing recycled polyester with a raising agent; 2) Use a wire napping machine to nap the grey cloth for three consecutive passes. The speed of the cylinder and the napping roller in the third pass is lower than that of the previous two passes, and the speed of the squatting roller in the third pass is higher than that of the previous two passes. 3) Then the wool is sheared and dry-shaped to obtain the recycled polyester-cotton knitted brushed plush fabric.

[0006] Grey fabric is obtained with fine and dense nap of required length through napping process. The napping process is to pass the fabric through a series of napping rollers wrapped with steel wire needle cloth, and the needle tips of the metal needle cloth pick up the fibers of the fabric, and then hook and break them to generate nap. The steel wire napping machine is equipped with two types of napping rollers on a drum. One type of napping roller is equipped with metal needles bent in the same direction as the fabric movement, and the other type of napping roller is equipped with metal needles bent in the opposite direction of the fabric movement, which are commonly called combing napping rollers and drawing napping rollers. When the fabric runs on the napping machine, the rotating combing napping rollers and drawing napping rollers have a relative movement to the fabric at the same time. It is this relative movement that makes the needle tips of the napping rollers scrape the fabric in one direction and then in the opposite direction, so that the nap of the fabric is scratched, thereby achieving the purpose of napping. This is the principle of fabric napping.

[0007] The raising force and combing force are constantly changing during the raising process. The raising force decreases as the raised fluff increases, and the combing force increases as the raised fluff increases. Therefore, during the production process, it is necessary to continuously adjust the speed of the raising and combing rollers, that is, adjust the raising force and combing force.

[0008] Preferably, the mass of the raising agent added is 3-5% of the mass of the grey cloth, and the raising agent is used together with a softener, and the mass of the softener added is 6-8% of the mass of the grey cloth. A large amount of raising agent needs to be added during the raising process to make the fabric fluffy and easy to handle. The main function of the raising agent is to form fiber bundles on the surface of the fabric, and to tilt or stand up the fibers on the surface of the fabric. If the raising agent is not added, it will inevitably lead to fabric surface defects such as broken hair and pinholes on the fabric suede. However, excessive use of the raising agent may cause the fabric to be over-raised, making its surface appear rough and affecting the overall appearance. Therefore, when using the raising agent, it is necessary to control the degree of raising to avoid excessive treatment.

[0009] Preferably, in the softening step, the grey cloth is soaked with water, half of the additive is added first, and the remaining half is added during the treatment process. Adding in batches can make the softening more uniform.

[0010] Preferably, in the softening step, the cloth feeding roller has a pressure of 4-5 kg ​​and a rotation speed of 250-400 r / min.

[0011] Preferably, the preparation method of the raising agent is: (1) mixing terminal hydrogen silicone oil, allyl epoxy polyether and castor oil in a molar ratio of 1:(1.2-1.5):(0.1-0.4), adding the mixture to a solvent, and heating the mixture under nickel catalysis to obtain polyether epoxy silicone oil; (2) Mix polyether epoxy silicone oil and lysine, and heat them under the catalysis of TEBAC to obtain a raising agent.

[0012] Preferably, the solvent of step (1) is isopropanol, and the heating reaction is reflux heating for 8-10 hours; the heating conditions of step (2) are 200-230° C. for 2-4 hours.

[0013] At present, the raising agents on the market are mainly prepared by compounding emulsions such as dimethyl silicone oil, hydroxy silicone oil, amino silicone oil and fatty amide compounds. In addition to having a conventional structure, the raising agent prepared by the present invention also has long-chain alkane branches, hydroxyl groups and a small amount of amino and carboxyl groups in the molecule.

[0014] Preferably, after softening the grey cloth, it is first dehydrated, stretched, shaped, and dried, and then napped, with a temperature of 130-135°C, an overfeed of 20-25%, a fan speed of 1500-1800r / min, a speed of 28-36m / min, and an expanded width 20-25cm larger than the finished product.

[0015] Preferably, the conditions for napping and raising are that the cloth head inverted according to the raising pile loop enters first, the cloth speed is 16-25 m / min, the tension of the front and rear cloth guide rollers is -30 to 30%; the cylinder speed of the first and second passes is 110-130 r / min, the squatting roller speed is 10-30 r / min, and the raising roller speed is 30-50 r / min; the cylinder speed of the third pass is 100-110 r / min, the squatting roller speed is 40-50 r / min, and the raising roller speed is 10-20 r / min.

[0016] As a preferred method, the shearing processing conditions are: cloth feeding tension 1.5-2, speed 28-36 m / min. The shear gap is adjusted according to the cloth surface effect.

[0017] Preferably, the dry setting treatment conditions are: the rolling groove is not immersed in water, the temperature is 130-140° C., the speed is 26-30 m / min, the fan speed is 1000-1200 r / min, and the overfeed is 8-16%.

[0018] Therefore, the beneficial effects of the present invention are as follows: (1) First, a suitable raising agent is selected to make the recycled polyester blended grey fabric easy to raise while preventing the recycled polyester blended yarn from slipping and causing long hair and shedding; when raising the grey fabric, the raising and combing process parameters are adjusted by an efficient raising machine so that the raised hair stands upright, and then a shearing process is added to trim the hair of different lengths flat, thereby reducing the chance of the raised surface being easy to pilling after washing; finally, the final product is formed in a rolling groove without being immersed in water, and a dry shaping process is adopted to reduce the air volume of the shaping machine, thereby ensuring that the hair is flat and no long hair is generated. Through the above process steps, the problem of the raised surface of recycled polyester-cotton knitted flannel being easy to pilling after washing is solved. (2) Recycled polyester is a green and environmentally friendly polyester fiber made from recycled resources, which can be widely used in the textile and garment industry, and is of great significance to reducing air pollution, protecting the environment and sustainable development. DETAILED DESCRIPTION

[0019] The technical solution of the present invention is further described below through specific embodiments.

[0020] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the embodiments, unless otherwise specified, are all conventional methods in the art. Unless otherwise specified, parts are all weight parts, temperatures are expressed in ° C or at ambient temperature, and pressures are atmospheric pressure or near atmospheric pressure. There are many variations and combinations of reaction conditions (such as component concentrations, desired solvents, solvent mixtures, temperatures, pressures, and other reaction ranges) and conditions that can be used to optimize the purity and yield of the product obtained by the method, and only reasonable routine experiments will be required to optimize such method conditions.

[0021] Example The method for reducing pilling of recycled polyester-cotton knitted brushed fleece fabric comprises the following steps: 1) Treat the grey fabric containing recycled polyester with a raising agent in a softening machine; The raising agent can be purchased from the market or homemade. Among the commercially purchased raising agents, the preferred one is the high-concentration soft raising agent RF-2 from Suzhou Liansheng Chemical Co., Ltd., which is a specially processed emulsion of higher fatty acids and is used for raising and sanding finishing of cotton, T / C, polyester, nylon and other fabrics, and raising and polarizing finishing of polyester warp and weft knitted fabrics. The high-concentration soft raising agent RF-2 has an appearance of milky white or slightly yellow milky white emulsion, ionicity: cationic, pH value of 4.0-6.0 (1% aqueous solution), and solubility: soluble in water in any proportion.

[0022] The preparation method of the homemade raising agent is: (1) mixing terminal hydrogen silicone oil, allyl epoxy polyether and castor oil in a molar ratio of 1:(1.2-1.5):(0.1-0.4), adding to isopropanol solvent, heating under reflux reaction for 8-10 hours under nickel catalysis to obtain polyether epoxy silicone oil; (2) Mix polyether epoxy silicone oil and lysine in a molar ratio of (2-3):1, heat to 200-230°C under the catalysis of benzyltriethylammonium chloride TEBAC, and react for 2-4 hours to obtain a raising agent.

[0023] The raising agent can also be used together with a softener. The softener is preferably soft film S400, which is a fatty amide compound and is suitable for softening cotton, linen and their blended fabrics or yarns to obtain a soft and smooth feel with minimal effect on whiteness.

[0024] The added mass of raising agent is 3-5% of the mass of grey fabric, and the added mass of softener is 6-8% of the mass of grey fabric.

[0025] The manufacturer of the upper softening machine is Wuxi Xinqi Machinery Co., Ltd. In the processing steps, the water level in the upper softening machine is half of the baffle, and half of the auxiliary agent is added. The remaining half of the auxiliary agent is added during the processing operation. The pressure of the cloth feeding roller is 4-5kg, and the speed is 250-400r / min. After dehydration and fabric sorting, the cloth is stretched, shaped and dried: the shaping machine is produced by Shaoxing Hongtao, the temperature is 130-135℃, the overfeed is 20-25%, the fan speed is 1500-1800r / min, the speed is 28-36m / min, and the expansion width is 20-25cm larger than the finished product.

[0026] 2) Use a wire napping machine to nap the grey cloth for three consecutive passes. The speed of the cylinder and the napping roller in the third pass is lower than that of the previous two passes, and the speed of the squatting roller in the third pass is higher than that of the previous two passes. The ME409A high-efficiency raising machine of Haining Textile Machinery Factory is used for raising and combing the napping. The cloth head with the napping loop inverted enters first, the cloth speed is 16-22 m / min, the cylinder speed is 110-130r / min, the tension of the front and rear cloth guide rollers is -30-30%, the squatting roller speed is 10-30r / min, the raising roller speed is 30-50r / min, and the two passes are pulled continuously. After the two passes are pulled continuously, an additional pass is added, the cloth speed is 16-25 m / min, the cylinder speed is 100-110r / min, the tension of the front and rear cloth guide rollers is -30-30%, the squatting roller speed is 40-50r / min, and the raising roller speed is 10-20r / min.

[0027] The cylinder speed, also known as the cylinder doffer speed of the carding machine, refers to the speed at which the blades installed on the carding machine rotate. The blades of the carding machine gradually comb out the fine hair or hair by rotating, so that it has better gloss and softness. Therefore, the speed of the cylinder doffer of the carding machine directly affects the carding effect and work efficiency of the carding machine. As the main carding component, the cylinder uses a higher cylinder speed to reduce the impurities of the raw sliver cotton knots, increase the cover plate flowers, and improve the combing effect (better cotton knot removal rate). The cylinder speed of the first and second passes of the present invention is large, and the large cylinder speed can increase the fluffing density of the fabric, which is beneficial to fluffing. The cylinder speed of the third pass is small, which improves the combing effect. However, if the cylinder speed is too high, the damage to the fiber will increase, and the yarn defects will also increase accordingly, so the cylinder speed needs to be controlled within a reasonable range.

[0028] The raising speed of the raising roller is the relative speed of the needle tip on the raising roller relative to the fabric, which is a concept of relative speed. The raising roller speeds of the first and second passes of the present invention are high, which is conducive to rapid raising, and the raising roller speed of the third pass can be appropriately reduced.

[0029] The speed of the squatting roller is also called the speed of the combing roller. The faster the squatting roller speed, the better the combing effect, the more cotton knots and impurities are thrown off, the greater the impact force on the cotton block and the higher the fiber damage rate; on the contrary, the combing is poor and the fiber damage rate is low. The first and second squatting roller speeds of the present invention are low, and the fiber damage rate is low; the third squatting roller speed is high, and at this time there is already a lot of fluff, so a better combing effect is needed, and because there is a lot of fluff protection, even if the squatting roller speed is increased, the fiber damage rate will not be very high.

[0030] 3) shearing and dry shaping to obtain recycled polyester-cotton knitted brushed fleece; The shearing processing conditions are as follows: the shearing machine manufacturer is Yuantu Textile Machinery Co., Ltd., the cloth feeding tension is 1.5-2, the speed is 28-36 m / min, and the scissors gap is adjusted according to the cloth surface effect.

[0031] The processing conditions for the final product are as follows: the setting machine is produced by Shaoxing Hongtao, dry setting, the rolling groove is not immersed in water, the temperature is 130-140℃, the speed is 26-30m / min, the fan speed is 1000-1200r / min, and the overfeed is 8-16%.

[0032] Example 1 CVC60 / 40 recycled polyester low-elastic velvet cloth blue A method for reducing pilling of recycled polyester-cotton knitted brushed plush fabric, comprising the following steps: 1) Softening treatment: After the dyeing sample of 250g CVC recycled polyester low-elastic velvet cloth is checked and qualified, the water level in the upper softening machine is half of the baffle, and half of the auxiliary material is added. The remaining half of the auxiliary material is added during the softening process. The pressure of the cloth feeding roller is 4kg, the speed is 350r / min, and the auxiliary material preparation ratio is: the mass of the high-concentration soft raising agent RF-2 is 3% of the mass of the grey cloth, and the mass of the soft film S400 is 8% of the mass of the grey cloth. Among them, CVC fabric (chief value of cotton) is a fabric with only two components of polyester and cotton. CVC60 / 40 means that the cotton content is 60% and the polyester content is 40%.

[0033] 2) After dehydration, stretching, shaping and drying: temperature 130℃, overfeed 25%, fan speed 1600r / min, speed 32m / min, the expanded width is 25cm larger than the finished product.

[0034] 3) Napping and raising: The cloth head with the napping loop inverted enters first, the cloth speed is 20m / min, the cylinder speed is 130r / min, the tension of the front and rear guide rollers is 25%, the speed of the squatting roller is 30r / min, the speed of the raising roller is 50r / min, and two passes are pulled continuously.

[0035] 4) Combing: in the above step 3), after two continuous pulling, one more pulling is performed. The cloth speed is 18 m / min, the cylinder speed is 100 r / min, the tension of the front and rear cloth guide rollers is 25%, the speed of the squatting roller is 40 r / min, and the speed of the raising roller is 20 r / min.

[0036] 5) Shearing process: cloth feeding tension 2, speed 32 m / min, scissors gap is adjusted according to cloth surface effect.

[0037] 6) Finished product: dry setting, the rolling groove is not immersed in water, the temperature is 140°C, the speed is 28 m / min, the fan speed is 1200 r / min, and the overfeed is 12% to obtain the finished product recycled polyester-cotton knitted brushed plush fabric.

[0038] The finished product has been tested for soap fastness, abrasion fastness, shrinkage and pH value, and all quality indicators have reached the industry standards. The results are shown in Table 1. Visual inspection shows that the suede effect of the velvet cloth after washing meets the requirements.

[0039] Table 1. Example 2 CVC55 / 45 recycled polyester low-elastic velvet cloth 310g coconut milk A method for reducing pilling of recycled polyester-cotton knitted brushed plush fabric, comprising the following steps: 1) Softening treatment: After the dyeing sample of 310g CVC55 / 45 recycled polyester low-elastic velvet cloth is checked as qualified, the water level in the softening machine is half of the baffle, and half of the auxiliary material is added. The remaining half of the auxiliary material is added in the softening process. The pressure of the cloth feeding roller is 5kg, the speed is 280 r / min, and the proportion of auxiliary materials is as follows: the mass of high-concentration soft raising agent RF-2 is 3% of the mass of the grey cloth, and the mass of soft film S400 is 8% of the mass of the grey cloth.

[0040] 2) After dehydration, stretching, shaping and drying: temperature 135 ℃, overfeed 20%, fan speed 1600 r / min, speed 28 m / min, the expanded width is 25 cm larger than the finished product.

[0041] 3) Napping and raising: The cloth head with the napping loop inverted enters first, the cloth speed is 16 m / min, the cylinder speed is 100 r / min, the tension of the front and rear guide rollers is 20%, the speed of the squatting roller is 20 r / min, the speed of the raising roller is 40 r / min, and two passes are pulled continuously.

[0042] 4) Combing: cloth speed 16 m / min, cylinder speed 110 r / min, front and rear cloth guide roller tension 25%, squatting roller speed 40 r / min, raising roller speed 20 r / min.

[0043] 5) Shearing: cloth feeding tension 1.8, speed 32 m / min. The shear gap is adjusted according to the cloth surface effect.

[0044] 6) Finished product: dry setting, the rolling groove is not immersed in water, the temperature is 135°C, the speed is 28 m / min, the fan speed is 1000 r / min, and the overfeed is 15% to obtain the finished product recycled polyester-cotton knitted brushed plush fabric.

[0045] The finished product has been tested for soap fastness, abrasion fastness, shrinkage and pH value, and all quality indicators have reached the industry standards. The results are shown in Table 2. Visual inspection shows that the suede effect of the velvet cloth after washing meets the requirements.

[0046] Table 2. Example 3 T / C75 / 25 recycled polyester towel fleece cloth 220g military green A method for reducing pilling of recycled polyester-cotton knitted brushed plush fabric, comprising the following steps: 1) Softening treatment: After the dyeing sample of 220g T / C75 / 25 recycled polyester towel napped cloth is checked and qualified, the water level in the upper softening machine is half of the baffle, and half of the auxiliary material is added. The remaining half of the auxiliary material is added during the softening process. The pressure of the cloth feeding roller is 5 kg, the speed is 400 r / min, and the auxiliary material preparation ratio is: the addition amount of RF-2 high-concentration soft raising agent is 2% of the weight of the grey cloth, and the addition amount of soft film S400 is 6% of the weight of the grey cloth. Among them, T / C fabric is a fabric made of polyester and cotton yarn interwoven according to a certain rule on a shuttle weaving machine. T is the abbreviation code of polyester, TERYLENE; C is the abbreviation code of cotton, COTTON. T / C75 / 25 means that polyester accounts for 75% and cotton accounts for 25% of the fabric.

[0047] 2) After dehydration, stretching, shaping and drying: temperature 135 ℃, overfeed 20%, fan speed 1600 r / min, speed 36 m / min, the expanded width is 20 cm larger than the finished product.

[0048] 3) Napping and raising: The cloth head with the napping loop inverted enters first, the cloth speed is 20 m / min, the cylinder speed is 110 r / min, the tension of the front and rear guide rollers is 20%, the speed of the squatting roller is 20 r / min, the speed of the raising roller is 40 r / min, and two passes are pulled continuously.

[0049] 4) Combing: cloth speed 20 m / min, cylinder speed 100 r / min, front and rear cloth guide roller tension 25%, squatting roller speed 40 r / min, raising roller speed 20 r / min.

[0050] 5) Shearing process: cloth feeding tension 1.8, speed 32 m / min, scissors gap is adjusted according to cloth surface effect.

[0051] 6) Finished product: dry setting, no water immersion in the rolling groove, temperature 135 ℃, speed 30 m / min, fan speed 1000 r / min, overfeed 10%.

[0052] The finished product has been tested for soap fastness, abrasion fastness, shrinkage and pH value, and all quality indicators have reached the industry standards. The results are shown in Table 3. Visual inspection shows that the suede effect of the velvet cloth after washing meets the requirements.

[0053] Table 3. Example 4 The difference from Example 1 is that the raising agent used is a homemade raising agent.

[0054] The preparation method of the raising agent is: (1) Add hydrogenated silicone oil Allyl epoxy polyether and castor oil (CAS registration number: 8001-79-4) at a molar ratio of 1:1.2:0.1, added into isopropanol solvent, heated under reflux reaction for 8 hours under nickel catalysis to obtain polyether epoxy silicone oil; (2) Polyether epoxy silicone oil and lysine were mixed in a molar ratio of 2:1, and reacted at 220°C for 3 h under the catalysis of benzyltriethylammonium chloride TEBAC to obtain a raising agent.

[0055] Example 5 The difference from Example 4 is that castor oil is not added during the preparation of the raising agent, which is as follows.

[0056] The preparation method of the raising agent is: (1) mixing terminal hydrogen silicone oil and allyl epoxy polyether in a molar ratio of 1:1.2, adding the mixture into isopropanol solvent, and heating under reflux reaction for 8 hours under nickel catalysis to obtain polyether epoxy silicone oil; (2) Polyether epoxy silicone oil and lysine were mixed in a molar ratio of 2:1, and reacted at 220°C for 3 h under the catalysis of benzyltriethylammonium chloride TEBAC to obtain a raising agent.

[0057] Example 6 The difference from Example 4 is that no lysine is added during the preparation of the raising agent, that is, step (2) is not performed, as follows.

[0058] The preparation method of the raising agent is as follows: terminal hydrogen silicone oil, allyl epoxy polyether and castor oil are mixed in a molar ratio of 1:1.2:0.1, added into isopropanol solvent, and heated under reflux reaction for 8 hours under nickel catalysis to obtain the raising agent.

[0059] Example 7 The difference from Example 4 is that the amount of lysine used in the preparation of the raising agent exceeds the preferred range, as shown below.

[0060] The preparation method of the raising agent is: (1) mixing terminal hydrogen silicone oil, allyl epoxy polyether and castor oil in a molar ratio of 1:1.2:0.1, adding the mixture into isopropanol solvent, and heating under reflux reaction for 8 hours under nickel catalysis to obtain polyether epoxy silicone oil; (2) Polyether epoxy silicone oil and lysine were mixed in a molar ratio of 4:3, and reacted at 220° C. for 3 h under the catalysis of benzyltriethylammonium chloride TEBAC to obtain a raising agent.

[0061] Comparative Example Comparative Example 1 The difference from Example 1 is that a conventional raising process is adopted, specifically: after the flannel dyeing sample is checked and qualified, a conventional soft film S400 is added to the softening machine, the addition amount is 3-6% of the mass of the grey cloth, the addition amount of silicone oil 856 is 2-3% of the mass of the grey cloth, and the addition amount of RF-2 high-concentration softening and raising agent is 2-3% of the mass of the grey cloth, and then the cloth is dried on a conventional drying machine for dehydration and fabric sorting, and then the cloth head is first entered according to the raising loop, the cylinder speed is 100-110r / min, the tension of the front and rear guide rollers is -20--20%, the squatting raising needle roller speed is 0-30r / min, the cloth speed is 20-26 m / min, 2-3 passes are continuously pulled, and finally the finished product is directly put into the tentering setting machine for finalization.

[0062] The test results of soap fastness, abrasion fastness, shrinkage and pH value of the finished product are shown in Table 4. Visually, the suede effect of the velvet cloth after washing does not meet the requirements.

[0063] Table 4. From the above table, we can see that although the test results of soap washing fastness, abrasion fastness, shrinkage and pH value are not much different, the conventional raising process is not effective for raising the recycled polyester.

[0064] Comparative Example 2 CVC60 / 40 recycled polyester low-elastic velvet cloth blue The difference from Example 1 is that, during the combing process in step 4), the cylinder speed is higher than that in the previous two processes.

[0065] 1) Softening treatment: After the dyeing sample of 250g CVC recycled polyester low-elastic velvet cloth is checked and qualified, the water level in the upper softening machine is half of the baffle, and half of the auxiliary material is added. The remaining half of the auxiliary material is added during the softening process. The pressure of the cloth feeding roller is 4 kg, the speed is 350 r / min, and the auxiliary material preparation ratio is: the mass of high-concentration soft raising agent RF-2 is 3% of the mass of the grey cloth, and the mass of soft film S400 is 8% of the mass of the grey cloth. Among them, CVC fabric (chief value of cotton) is a fabric with only two components of polyester and cotton. CVC60 / 40 means that the cotton content is 60% and the polyester content is 40%.

[0066] 2) After dehydration, stretching, shaping and drying: temperature 130 ℃, overfeed 25%, fan speed 1600 r / min, speed 32 m / min, the expanded width is 25 cm larger than the finished product.

[0067] 3) Napping and raising: The cloth head with the napping loop inverted enters first, the cloth speed is 20 m / min, the cylinder speed is 100 r / min, the tension of the front and rear guide rollers is 25%, the speed of the squatting roller is 30 r / min, the speed of the raising roller is 50 r / min, and two passes are pulled continuously.

[0068] 4) Combing: Combing the napped naps twice in the above step 3) and then adding another one, with a cloth speed of 18 m / min, a cylinder speed of 130 r / min, a tension of the front and rear cloth guide rollers of 25%, a speed of 40 r / min for the nap rollers and a speed of 20 r / min for the napping rollers.

[0069] 5) Shearing process: cloth feeding tension 2, speed 32 m / min, scissor gap is adjusted according to the cloth surface effect.

[0070] 6) Finished product: dry setting, the rolling groove is not immersed in water, the temperature is 140°C, the speed is 28 m / min, the fan speed is 1200 r / min, and the overfeed is 12% to obtain the finished product recycled polyester-cotton knitted brushed plush fabric.

[0071] Comparative Example 3 CVC60 / 40 recycled polyester low-elastic velvet cloth blue The difference from Example 1 is that, during the combing process in step 4), the speed of the squatting roller is lower than that of the previous two processes.

[0072] 1) Softening treatment: After the dyeing sample of 250g CVC recycled polyester low-elastic velvet cloth is checked and qualified, the water level in the upper softening machine is half of the baffle, and half of the auxiliary material is added. The remaining half of the auxiliary material is added during the softening process. The pressure of the cloth feeding roller is 4kg, the speed is 350r / min, and the auxiliary material preparation ratio is: the mass of the high-concentration soft raising agent RF-2 is 3% of the mass of the grey cloth, and the mass of the soft film S400 is 8% of the mass of the grey cloth. Among them, CVC fabric (chief value of cotton) is a fabric with only two components of polyester and cotton. CVC60 / 40 means that the cotton content is 60% and the polyester content is 40%.

[0073] 2) After dehydration, stretching, shaping and drying: temperature 130℃, overfeed 25%, fan speed 1600r / min, speed 32m / min, the expanded width is 25cm larger than the finished product.

[0074] 3) Napping and raising: The cloth head with the napping loop inverted enters first, the cloth speed is 20m / min, the cylinder speed is 130r / min, the tension of the front and rear guide rollers is 25%, the speed of the squatting roller is 40r / min, the speed of the raising roller is 50r / min, and two passes are pulled continuously.

[0075] 4) Combing: in the above step 3), after two continuous pulling, one more pulling is performed. The cloth speed is 18 m / min, the cylinder speed is 100 r / min, the tension of the front and rear cloth guide rollers is 25%, the speed of the squatting roller is 30 r / min, and the speed of the raising roller is 20 r / min.

[0076] 5) Shearing process: cloth feeding tension 2, speed 32 m / min, scissors gap is adjusted according to cloth surface effect.

[0077] 6) Finished product: dry setting, the rolling groove is not immersed in water, the temperature is 140°C, the speed is 28 m / min, the fan speed is 1200 r / min, and the overfeed is 12% to obtain the finished product recycled polyester-cotton knitted brushed plush fabric.

[0078] Performance Testing In order to further compare the fuzz and pilling of recycled polyester-cotton knitted brushed fleece fabric, fuzz density and pilling tests were conducted.

[0079] (1) Fluff density test: Cut the fluff fabric into a circular sample with a diameter of 113 mm. Select the center point and four points on the edge, which are equally distributed. Draw a circle with a diameter of 0.25 cm with the point as the center. Calculate the number of fluff roots within the circle and take the average value.

[0080] (2) The products prepared in the embodiments and comparative examples were tested by the pressurization method specified in GB / T4802.1-1997 "Textiles - Fabric Pilling Test - Circular Locus Method". During the test, five specimens were randomly cut from a position more than 10 cm away from the edge of the fabric according to the third-level standard atmosphere specified in GB6529. The specimens were free of defects that could affect the test results.

[0081] The test method is: on the circular trajectory pilling instrument, adjust the sample chuck, weight and friction speed according to the regulations, use a nylon brush and abrasive or abrasive alone to make the fabric rub and pill. Then compare the pilled sample with the standard sample under the specified lighting conditions. The standard sample has the following levels: Level 5 is slightly fuzzy and no pilling, slightly fuzzy, and the fiber ends are sparse and short; Level 4 is slightly fuzzy and slightly pilling, with cloud-like fluff and silk rings, fiber entanglement, incomplete pilling, and individual complete pills; Level 3 is moderate pilling, with more cloud-like fluff, more incomplete pills, and more complete pills; Level 2 is slightly serious pilling, with strong pilling, incomplete pilling or felting, or long fluff; Level 1 is serious pilling, with serious pilling or obvious felting, the fluff is not separated, and the entanglement is particularly long. The test results are shown in Table 5.

[0082] Table 5. It can be seen from Table 5 that compared with the conventional raising process of Comparative Example 1, the recycled polyester-cotton knitted raised fleece fabric prepared in each embodiment of the present invention has excellent fluff effect, anti-pilling and wear resistance by adjusting the raising agent and raising process parameters. Compared with Example 1, during the combing process of Comparative Example 2, the cylinder speed is higher than the previous two passes; during the combing process of Comparative Example 3, the squatting roller speed is lower than the previous two passes; the fluff density is not as good as that of Example 1, and the fiber is damaged, and the friction fastness is not as good as that of Example 1.

[0083] Compared with Example 1, Example 4 uses a homemade raising agent, and the comprehensive performance is the best. The homemade raising agent first adds castor oil to the polyether epoxy silicone oil preparation process to participate in the polymerization. On the one hand, castor oil is added to the molecular chain through double bonds, and the structure is stable and not easy to fall off; on the other hand, long alkane side chains and hydroxyl groups are introduced into the molecule through castor oil. The long alkane side chains have high degrees of freedom, and the slender shape is conducive to its extension into the gap between the grey cloth fibers, thereby improving the raising rate. Then further react with lysine, so that the raising agent is provided with carboxyl and amino groups with strong polarity, which interact with the hydroxyl and carboxyl groups on the surface of the grey cloth, and form a firm orientation and adsorption with the fiber. In particular, after the amino group is adsorbed on the fiber, carbonic acid is formed by carbon dioxide and moisture in the air, cross-linked with the amino group, highly polymerized, and a high degree of polymerization elastic network structure is generated on the surface and inside of the fiber, giving the fabric a super soft effect and high washability. Therefore, the raising agent can also increase the wear resistance of the fabric. The raising treatment makes the fiber surface more compact and firm, reducing the shedding and wear of the fiber. This makes the fabric more durable and can withstand longer use and washing without deformation or damage. In Example 5, castor oil was not added when preparing the raising agent, and in Example 6, lysine was not added when preparing the raising agent. The effect was not as good as that in Example 4, indicating that these two agents did play a beneficial role. In Example 7, the amount of lysine was too much, resulting in too many polar groups in the raising agent, which made the fiber surface stiffer during the raising process, which was not conducive to raising. Therefore, the amount of each agent used can play the best beneficial effect within a reasonable range.

[0084] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with the profession can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. Methods to reduce pilling of recycled polyester-cotton knitted fleece fabrics. It is characterized in that The following steps are involved: (1) Treating grey fabric containing recycled polyester with a raising agent; (2) The treated grey fabric is napped and raised for three consecutive passes. The speed of the cylinder and the raising roller in the third pass is lower than that of the first two passes, and the speed of the squatting roller in the third pass is higher than that of the first two passes. (3) Shearing and dry shaping to obtain recycled polyester-cotton knitted fleece fabric.

2. The method for reducing pilling of recycled polyester-cotton knitted brushed fabric according to claim 1, It is characterized in that The mass of raising agent added is 3-5% of the mass of grey fabric. Raising agent is used together with softener, and the mass of softener added is 6-8% of the mass of grey fabric.

3. The method for reducing pilling of recycled polyester-cotton knitted brushed fabric according to claim 1, It is characterized in that In the softening step, the grey cloth is soaked with water, half of the additive is added first, and the remaining half is added during the treatment process.

4. The method for reducing pilling of recycled polyester-cotton knitted brushed fabric according to claim 1, 2 or 3, It is characterized in that In the softening step, the cloth feeding roller has a pressure of 4-5 kg ​​and a rotation speed of 250-400 r / min.

5. The method for reducing pilling of recycled polyester-cotton knitted brushed fabric according to claim 1, It is characterized in that The preparation method of the raising agent is: 1) Mix terminal hydrogen silicone oil, allyl epoxy polyether and castor oil in a molar ratio of 1:(1.2-1.5):(0.1-0.4), add to a solvent, and heat to react under nickel catalysis to obtain polyether epoxy silicone oil; 2) Mix polyether epoxy silicone oil and lysine, and heat them under the catalysis of TEBAC to obtain a raising agent.

6. The method for reducing pilling of recycled polyester-cotton knitted brushed fabric according to claim 5, It is characterized in that The solvent of step 1) is isopropanol, and the heating reaction is reflux heating for 8-10 h; the heating condition of step 2) is 200-230 °C for 2-4 h.

7. The method for reducing pilling of recycled polyester-cotton knitted brushed fabric according to claim 1, It is characterized in that After the grey cloth is softened, it is first dehydrated, stretched, shaped, and dried, and then napped at a temperature of 130-135°C, an overfeed of 20-25%, a fan speed of 1500-1800 r / min, a speed of 28-36 m / min, and an expanded width of 20-25 cm larger than the finished product.

8. The method for reducing pilling of recycled polyester-cotton knitted brushed fabric according to claim 1 or 7, It is characterized in that The conditions for napping and raising are as follows: the cloth head inverted according to the raising pile loop enters first, the cloth speed is 16-25 m / min, the tension of the front and rear cloth guide rollers is -30~30%; the cylinder speed of the first and second passes is 110-130 r / min, the squatting roller speed is 10-30 r / min, and the raising roller speed is 30-50 r / min; the cylinder speed of the third pass is 100-110 r / min, the squatting roller speed is 40-50 r / min, and the raising roller speed is 10-20 r / min.

9. The method for reducing pilling of recycled polyester-cotton knitted brushed fabric according to claim 1, It is characterized in that The shearing processing conditions are: cloth feeding tension 1.5-2, speed 28-36 m / min.

10. The method for reducing pilling of recycled polyester-cotton knitted brushed fabric according to claim 1 or 9, It is characterized in that The dry setting treatment conditions are: the rolling groove is not immersed in water, the temperature is 130-140 ℃, the speed is 26-30 m / min, the fan speed is 1000-1200r / min, and the overfeed is 8-16%.