Thin sheet packaging paper, packaging paper bag and preparation process thereof

Through the coordination and coordination of the functional multi-adjustment stabilizer and kaolin modifier of coniferous wood pulp and broadleaf wood pulp, the problem of insufficient barrier performance and waterproof and oil resistance of packaging paper bags is solved, and the coordination between strength and barrier performance is achieved. Improved waterproof and oil-resistant performance.

CN118727513BActive Publication Date: 2024-11-22PUTIAN CHAOQI PAPER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411233680.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-22
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The barrier properties, strength properties and waterproof and oil-proof properties of existing packaging paper bags are insufficient, which limits their efficiency.

Method used

Using coniferous wood pulp and broadleaf wood pulp as matrix materials, combined with functional multi-adjustment stabilizer, kaolin-doped modifier, silane coupling agent KH560, polyvinyl alcohol and gelatin, the paper is enhanced through specific preparation processes and treatment methods. Strength and barrier properties, and optimize the modification treatment of wollastonite and kaolin to improve waterproof and oil-proof performance.

Benefits of technology

It significantly improves the strength and barrier properties of packaging paper bags, and significantly improves its waterproof and oil-proof performance, achieving coordination between strength and barrier properties and improving waterproof and oil-proof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of packaging paper bags, and in particular to a thin packaging paper, a packaging paper bag and a preparation process thereof, comprising the following steps: preparing the thin packaging paper: weighing raw materials by weight: 55-60 parts of coniferous wood pulp, 45-50 parts of broadleaf wood pulp, 15-20 parts of starch, 8-12 parts of functional multi-adjustable stabilizer, 4-7 parts of a modifier doped with kaolin, 4-7 parts of a silane coupling agent KH560, 2-5 parts of polyvinyl alcohol, and 2-4 parts of gelatin. In the preparation of the packaging paper bag of the present invention, the thin packaging paper is obtained by film sealing, cutting, folding, pasting, and printing. The thin packaging paper is made of coniferous wood pulp, broadleaf wood pulp, and starch as a base material, and is matched with a silane coupling agent KH560, polyvinyl alcohol, and gelatin as functional additives. The functional multi-adjustable stabilizer and the modifier doped with kaolin are added, and the two are coordinated with each other and work together, so that the obtained packaging paper has coordinated improvement in strength performance and barrier property, and has remarkable waterproof and oil-proof performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of packaging paper bags, and in particular to a thin sheet packaging paper, a packaging paper bag and a preparation process thereof. Background Art

[0002] Packaging materials refer to materials used to manufacture packaging containers, packaging decoration, packaging printing, packaging transportation, etc. to meet product packaging requirements; while packaging paper bags refer to paper bags used to package various supplies, which make it convenient to transport and store goods during the production and circulation process, and are widely used in daily life and industrial production.

[0003] Existing packaging paper bags are made of ordinary paper materials, and the barrier properties of packaging paper bags are poor. At the same time, the strength performance of the product is difficult to coordinate and improve with the barrier properties, and the waterproof and oil-proof properties of the packaging paper bags are poor, which further limits the use efficiency of the product. Summary of the invention

[0004] In view of the defects of the prior art, the object of the present invention is to provide a thin wrapping paper, a wrapping paper bag and a preparation process thereof, so as to solve the problems raised in the above background technology.

[0005] The present invention solves the technical problem by adopting the following technical solution:

[0006] The present invention provides a thin wrapping paper, comprising the following raw materials in parts by weight:

[0007] 55-60 parts of conifer pulp, 45-50 parts of broadleaf pulp, 15-20 parts of starch, 8-12 parts of functional multi-adjustable stabilizer, 4-7 parts of modifier doped with kaolin, 4-7 parts of silane coupling agent KH560, 2-5 parts of polyvinyl alcohol, and 2-4 parts of gelatin.

[0008] Preferably, the preparation method of the functional multi-adjustable stabilizer is:

[0009] S01: first prepare a sodium silicate solution with a mass fraction of 4-7% and a phosphate buffer solution with a pH value of 5.0; then stir the flaky talc, the sodium silicate solution and the phosphate buffer solution in a weight ratio of 3:5:1, filter and dry after stirring to obtain a flaky talc;

[0010] S02: Preparation of conditioning solution based on wollastonite modification:

[0011] S021: irradiating the wollastonite in a proton irradiation box for 5-10 minutes at an irradiation power of 350-400W, and then preheating the wollastonite at a temperature of 55-65°C for 10-20 minutes to obtain preheated wollastonite;

[0012] S022: then immerse the preheated wollastonite in a yttrium nitrate solution 3-5 times the total mass of the wollastonite and fully immerse it in ultrasound, with an ultrasound power of 350-400W and an ultrasound time of 20-30min. After the immersion is completed, a wollastonite agent is obtained;

[0013] S023: 3-5 parts of wollastonite agent, 1-3 parts of silane coupling agent KH560 and 4-7 parts of chitosan solution are fully mixed, and then 2-4 parts of hydroxyapatite and 1-2 parts of nano-silica sol are added and mixed thoroughly to obtain a wollastonite-modified conditioning solution;

[0014] S03: The flaky talc powder is immersed in a wollastonite-modified regulating liquid of 2-5 times the total mass of the flaky talc powder. After the immersion is completed, the liquid is filtered and dried to obtain a functional multi-adjustable stabilizer.

[0015] Preferably, the stirring temperature of the stirring treatment in S01 is 55-60°C, the stirring speed is 450-550r / min, and the stirring time is 20-30min; the impregnation power of the impregnation treatment in S03 is 350-400W, and the impregnation time is 20-30min.

[0016] Preferably, the mass fraction of the yttrium nitrate solution is 3-6%; the mass fraction of the chitosan solution is 2-5%.

[0017] Preferably, the preparation method of the kaolin-doped modifier is:

[0018] S11: adding kaolin to the sodium dodecylbenzene sulfonate solution at a weight ratio of 2:5 and dispersing the mixture evenly to obtain a kaolin solution;

[0019] S12: Preparation of modified melamine body:

[0020] Melamine and paraformaldehyde are mixed in a weight ratio of 1:4, and then water and alkali are added, reacting at 75-85°C for 20 minutes, and then terephthalaldehyde is added, the pH is adjusted to 7.5, and stirred sufficiently to obtain a modified melamine body;

[0021] S13: The kaolin liquid, modified melamine and the active agent are mixed in a weight ratio of 5:1:2, and the mixture is ball-milled at a speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a modifier doped with kaolin.

[0022] Preferably, the mass fraction of the sodium dodecylbenzene sulfonate solution is 4-7%.

[0023] Preferably, the preparation method of the activator is:

[0024] 2-4 parts of silane coupling agent KH550 and 1-3 parts of urea are added to 5-8 parts of ethanol solvent, and then 3-5 parts of silicon carbide whiskers and 1-2 parts of amino silicone oil are added and mixed thoroughly, and then washed with water and dried to obtain an active agent.

[0025] The present invention provides a process for preparing a thin wrapping paper, comprising the following steps:

[0026] (1) Weigh the raw materials by weight: 55-60 parts of softwood pulp, 45-50 parts of hardwood pulp, 15-20 parts of starch, 8-12 parts of functional multi-adjustable stabilizer, 4-7 parts of modifier doped with kaolin, 4-7 parts of silane coupling agent KH560, 2-5 parts of polyvinyl alcohol, and 2-4 parts of gelatin;

[0027] (2) beating softwood pulp and hardwood pulp to form a slurry, and then mixing the slurry with starch, a functional multi-adjusting stabilizer, a modifier doped with kaolin, a silane coupling agent KH560, polyvinyl alcohol, and gelatin to obtain a base paper agent;

[0028] (3) The base paper is dehydrated and formed in a screen section and a press section, and pressed on a paper press to obtain a thin sheet of packaging paper.

[0029] Preferably, the concentration of the pulp formed by the beating treatment of coniferous wood pulp and hardwood wood pulp is 4.5%.

[0030] The invention provides a packaging paper bag, which is prepared from the thin sheet packaging paper.

[0031] The present invention provides a process for preparing a packaging paper bag, comprising the following steps:

[0032] Step 1: preparing the thin wrapping paper;

[0033] Step 2: sealing the thin wrapping paper with a film, wherein a PE film is pressed onto the thin wrapping paper for sealing;

[0034] Step 3: Cut, fold, glue and print the sealed thin wrapping paper to obtain a wrapping paper bag.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] In the preparation of the packaging paper bag of the present invention, thin packaging paper is used through film sealing, cutting, folding, pasting and printing to obtain the thin packaging paper. The thin packaging paper is made of softwood pulp, hardwood pulp and starch as a base material, and is matched with an alkane coupling agent KH560, polyvinyl alcohol and gelatin as functional additives. A functional multi-adjustable stabilizer and a modifier doped with kaolin are added, and the two are coordinated with each other and work together to obtain a packaging paper with coordinated improvement in strength performance and barrier property, and a remarkable effect of waterproof and oil-proof performance; the functional multi-adjustable stabilizer is a sheet-shaped slip The stone powder, sodium silicate solution and phosphate buffer solution are blended and improved to optimize the dispersion stability of flaky talcum powder. At the same time, the adjustment solution based on wollastonite modification is coordinated and improved. The adjustment solution based on wollastonite modification is irradiated in a proton irradiation box for 5-10 minutes with an irradiation power of 350-400W, and then preheated at a temperature of 55-65°C for 10-20 minutes to optimize the activity of wollastonite. Then, the wollastonite is immersed in ultrasound in a yttrium nitrate solution to coordinate the wollastonite and the silane coupling agent K. The coordination and coordination effect between H560 and chitosan solution, hydroxyapatite and nano-silica sol, wollastonite as a needle-like structure, coordinated with point-shaped hydroxyapatite as point adsorption, and the coordination and coordination between the raw materials in the adjustment liquid modified by wollastonite are further enhanced. The improved functional multi-adjusting stabilizer in the product system enhances the strength of the system, the coordination of barrier properties, and optimizes the waterproof and oil-proof properties of the product; The modifier of mixed kaolin is kaolin that is evenly dispersed in a sodium dodecylbenzene sulfonate solution, combined with a modified melamine body structure, the modified melamine body provides multiple active groups, and then coordinated with a matching effector, with the silicon carbide whiskers in the effector as the whisker-like structure, distributed in the system, and at the same time coordinated and improved with silane coupling agent KH550, urea and amino silicone oil, and reinforced with lamellar kaolin, which further enhances the performance coordination stability of the system, and improves the waterproof and oil-proof properties of the product. DETAILED DESCRIPTION

[0037] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] A thin wrapping paper of the present embodiment includes the following raw materials in parts by weight:

[0039] 55-60 parts of conifer pulp, 45-50 parts of broadleaf pulp, 15-20 parts of starch, 8-12 parts of functional multi-adjustable stabilizer, 4-7 parts of modifier doped with kaolin, 4-7 parts of silane coupling agent KH560, 2-5 parts of polyvinyl alcohol, and 2-4 parts of gelatin.

[0040] The preparation method of the functional multi-adjustable stabilizer of this embodiment is:

[0041] S01: first prepare a sodium silicate solution with a mass fraction of 4-7% and a phosphate buffer solution with a pH value of 5.0; then stir the flaky talc, the sodium silicate solution and the phosphate buffer solution in a weight ratio of 3:5:1, filter and dry after stirring to obtain a flaky talc;

[0042] S02: Preparation of conditioning solution based on wollastonite modification:

[0043] S021: irradiating the wollastonite in a proton irradiation box for 5-10 minutes at an irradiation power of 350-400W, and then preheating the wollastonite at a temperature of 55-65°C for 10-20 minutes to obtain preheated wollastonite;

[0044] S022: then immerse the preheated wollastonite in a yttrium nitrate solution 3-5 times the total mass of the wollastonite and fully immerse it in ultrasound, with an ultrasound power of 350-400W and an ultrasound time of 20-30min. After the immersion is completed, a wollastonite agent is obtained;

[0045] S023: 3-5 parts of wollastonite agent, 1-3 parts of silane coupling agent KH560 and 4-7 parts of chitosan solution are fully mixed, and then 2-4 parts of hydroxyapatite and 1-2 parts of nano-silica sol are added and mixed thoroughly to obtain a wollastonite-modified conditioning solution;

[0046] S03: The flaky talc powder is immersed in a wollastonite-modified regulating liquid of 2-5 times the total mass of the flaky talc powder. After the immersion is completed, the liquid is filtered and dried to obtain a functional multi-adjustable stabilizer.

[0047] In the stirring treatment in S01 of this embodiment, the stirring temperature is 55-60°C, the stirring speed is 450-550r / min, and the stirring time is 20-30min; the immersion power of the immersion treatment in S03 is 350-400W, and the immersion time is 20-30min.

[0048] The mass fraction of the yttrium nitrate solution in this embodiment is 3-6%; the mass fraction of the chitosan solution is 2-5%.

[0049] The preparation method of the modifier doped with kaolin in this embodiment:

[0050] S11: adding kaolin to the sodium dodecylbenzene sulfonate solution at a weight ratio of 2:5 and dispersing the mixture evenly to obtain a kaolin solution;

[0051] S12: Preparation of modified melamine body:

[0052] Melamine and paraformaldehyde are mixed in a weight ratio of 1:4, and then water and alkali are added, reacting at 75-85°C for 20 minutes, and then terephthalaldehyde is added, the pH is adjusted to 7.5, and stirred sufficiently to obtain a modified melamine body;

[0053] S13: The kaolin liquid, modified melamine and the active agent are mixed in a weight ratio of 5:1:2, and the mixture is ball-milled at a speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a modifier doped with kaolin.

[0054] The mass fraction of the sodium dodecylbenzenesulfonate solution of the present embodiment is 4-7%.

[0055] The preparation method of the activator of this embodiment is:

[0056] 2-4 parts of silane coupling agent KH550 and 1-3 parts of urea are added to 5-8 parts of ethanol solvent, and then 3-5 parts of silicon carbide whiskers and 1-2 parts of amino silicone oil are added and mixed thoroughly, and then washed with water and dried to obtain an active agent.

[0057] A process for preparing a thin wrapping paper of this embodiment comprises the following steps:

[0058] (1) Weigh the raw materials by weight: 55-60 parts of softwood pulp, 45-50 parts of hardwood pulp, 15-20 parts of starch, 8-12 parts of functional multi-adjustable stabilizer, 4-7 parts of modifier doped with kaolin, 4-7 parts of silane coupling agent KH560, 2-5 parts of polyvinyl alcohol, and 2-4 parts of gelatin;

[0059] (2) beating softwood pulp and hardwood pulp to form a slurry, and then mixing the slurry with starch, a functional multi-adjusting stabilizer, a modifier doped with kaolin, a silane coupling agent KH560, polyvinyl alcohol, and gelatin to obtain a base paper agent;

[0060] (3) The base paper is dehydrated and formed in a screen section and a press section, and pressed on a paper press to obtain a thin sheet of packaging paper.

[0061] The concentration of the pulp formed by the beating treatment of coniferous wood pulp and hardwood wood pulp in this embodiment is 4.5%.

[0062] A packaging paper bag in this embodiment is made from the above-mentioned thin sheet packaging paper.

[0063] A preparation process of a packaging paper bag in this embodiment includes the following steps:

[0064] Step 1: preparing the thin wrapping paper;

[0065] Step 2: sealing the thin wrapping paper with a film, wherein a PE film is pressed onto the thin wrapping paper for sealing;

[0066] Step 3: Cut, fold, glue and print the sealed thin wrapping paper to obtain a wrapping paper bag.

[0067] Embodiment 1: A process for preparing a packaging paper bag, comprising the following steps:

[0068] Step 1: Prepare the tissue wrapping paper:

[0069] (1) Weigh the raw materials by weight: 55 parts of softwood pulp, 45 parts of hardwood pulp, 15 parts of starch, 8 parts of functional multi-adjustable stabilizer, 4 parts of modifier doped with kaolin, 4 parts of silane coupling agent KH560, 2 parts of polyvinyl alcohol, and 2 parts of gelatin;

[0070] (2) beating softwood pulp and hardwood pulp to form a slurry, and then mixing the slurry with starch, a functional multi-adjusting stabilizer, a modifier doped with kaolin, a silane coupling agent KH560, polyvinyl alcohol, and gelatin to obtain a base paper agent;

[0071] (3) Dehydrating the base paper through a screen section and a press section to form the base paper, and pressing it on a paper press to obtain a thin sheet packaging paper;

[0072] Step 2: sealing the thin wrapping paper with a film, wherein a PE film is pressed onto the thin wrapping paper for sealing;

[0073] Step 3: Cut, fold, glue and print the sealed thin wrapping paper to obtain a wrapping paper bag.

[0074] The concentration of the pulp formed by the beating treatment of coniferous wood pulp and hardwood wood pulp in this embodiment is 4.5%.

[0075] The preparation method of the functional multi-adjustable stabilizer of this embodiment is:

[0076] S01: first prepare a sodium silicate solution with a mass fraction of 4% and a phosphate buffer solution with a pH value of 5.0; then stir the flaky talc, the sodium silicate solution and the phosphate buffer solution in a weight ratio of 3:5:1, filter and dry after stirring to obtain a flaky talc;

[0077] S02: Preparation of conditioning solution based on wollastonite modification:

[0078] S021: irradiating the wollastonite in a proton irradiation box for 5 minutes at an irradiation power of 350 W, and then preheating the wollastonite at 55° C. for 10 minutes to obtain preheated wollastonite;

[0079] S022: then immerse the preheated wollastonite in a yttrium nitrate solution 3 times the total mass of the wollastonite and fully immerse it in ultrasound, with an ultrasound power of 350 W and an ultrasound time of 20 minutes. After the immersion is completed, a wollastonite agent is obtained;

[0080] S023: 3 parts of wollastonite agent, 1 part of silane coupling agent KH560 and 4 parts of chitosan solution are mixed thoroughly, and then 2 parts of hydroxyapatite and 1 part of nano silica sol are added and mixed thoroughly to obtain a wollastonite-modified conditioning solution;

[0081] S03: The flaky talc powder is immersed in a wollastonite-modified regulating liquid which is twice the total mass of the flaky talc powder. After the immersion is completed, the liquid is filtered and dried to obtain a functional multi-adjustable stabilizer.

[0082] In the stirring treatment in S01 of this embodiment, the stirring temperature is 55° C., the stirring speed is 450 r / min, and the stirring is for 20 minutes; the immersion power of the immersion treatment in S03 is 350 W, and the immersion time is 20 minutes.

[0083] The mass fraction of the yttrium nitrate solution in this embodiment is 3%; the mass fraction of the chitosan solution is 2%.

[0084] The preparation method of the modifier doped with kaolin in this embodiment:

[0085] S11: adding kaolin to the sodium dodecylbenzene sulfonate solution at a weight ratio of 2:5 and dispersing the mixture evenly to obtain a kaolin solution;

[0086] S12: Preparation of modified melamine body:

[0087] Melamine and paraformaldehyde are mixed in a weight ratio of 1:4, and then water and alkali are added, and the mixture is reacted at 75° C. for 20 minutes, and then terephthalaldehyde is added, and the pH is adjusted to 7.5, and the mixture is stirred sufficiently to obtain a modified melamine body;

[0088] S13: The kaolin liquid, modified melamine and the active agent are mixed in a weight ratio of 5:1:2, and the mixture is ball-milled at a speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a modifier doped with kaolin.

[0089] The mass fraction of the sodium dodecylbenzenesulfonate solution of the present embodiment is 4%.

[0090] The preparation method of the activator of this embodiment is:

[0091] 2 parts of silane coupling agent KH550 and 1 part of urea are added to 5 parts of ethanol solvent, and then 3 parts of silicon carbide whiskers and 1 part of amino silicone oil are added and mixed thoroughly, and then washed with water and dried to obtain an active agent.

[0092] Embodiment 2: A process for preparing a packaging paper bag, comprising the following steps:

[0093] Step 1: Prepare the tissue wrapping paper:

[0094] (1) Weigh the raw materials by weight: 60 parts of softwood pulp, 50 parts of hardwood pulp, 20 parts of starch, 12 parts of functional multi-adjustable stabilizer, 7 parts of kaolin-doped modifier, 7 parts of silane coupling agent KH560, 5 parts of polyvinyl alcohol, and 4 parts of gelatin;

[0095] (2) beating softwood pulp and hardwood pulp to form a slurry, and then mixing the slurry with starch, a functional multi-adjusting stabilizer, a modifier doped with kaolin, a silane coupling agent KH560, polyvinyl alcohol, and gelatin to obtain a base paper agent;

[0096] (3) Dehydrating the base paper through a screen section and a press section to form the base paper, and pressing it on a paper press to obtain a thin sheet packaging paper;

[0097] Step 2: sealing the thin wrapping paper with a film, wherein a PE film is pressed onto the thin wrapping paper for sealing;

[0098] Step 3: Cut, fold, glue and print the sealed thin wrapping paper to obtain a wrapping paper bag.

[0099] The concentration of the pulp formed by the beating treatment of coniferous wood pulp and hardwood wood pulp in this embodiment is 4.5%.

[0100] The preparation method of the functional multi-adjustable stabilizer of this embodiment is:

[0101] S01: first prepare a sodium silicate solution with a mass fraction of 7% and a phosphate buffer solution with a pH value of 5.0; then stir the flaky talc, the sodium silicate solution and the phosphate buffer solution in a weight ratio of 3:5:1, filter and dry after stirring to obtain a flaky talc;

[0102] S02: Preparation of conditioning solution based on wollastonite modification:

[0103] S021: irradiating the wollastonite in a proton irradiation box for 10 minutes at an irradiation power of 400 W, and then preheating the wollastonite at 65° C. for 20 minutes to obtain preheated wollastonite;

[0104] S022: then immerse the preheated wollastonite in a yttrium nitrate solution of 5 times the total mass of the wollastonite and fully immerse it in ultrasound, with the ultrasound power of 400 W and the ultrasound time of 30 minutes. After the immersion is completed, a wollastonite agent is obtained;

[0105] S023: 5 parts of wollastonite agent, 3 parts of silane coupling agent KH560 and 7 parts of chitosan solution are fully mixed, and then 4 parts of hydroxyapatite and 2 parts of nano-silica sol are added and mixed thoroughly to obtain a wollastonite-modified conditioning solution;

[0106] S03: The flaky talc powder is immersed in a wollastonite-modified regulating liquid of 5 times the total mass of the flaky talc powder. After the immersion is completed, the liquid is filtered and dried to obtain a functional multi-adjustable stabilizer.

[0107] In the stirring treatment in S01 of this embodiment, the stirring temperature is 60° C., the stirring speed is 550 r / min, and the stirring is for 30 minutes; the immersion power of the immersion treatment in S03 is 400 W, and the immersion time is 30 minutes.

[0108] The mass fraction of the yttrium nitrate solution in this embodiment is 6%; the mass fraction of the chitosan solution is 5%.

[0109] The preparation method of the modifier doped with kaolin in this embodiment:

[0110] S11: adding kaolin to the sodium dodecylbenzene sulfonate solution at a weight ratio of 2:5 and dispersing the mixture evenly to obtain a kaolin solution;

[0111] S12: Preparation of modified melamine body:

[0112] Melamine and paraformaldehyde are mixed in a weight ratio of 1:4, and then water and alkali are added, and the mixture is reacted at 85° C. for 20 minutes, and then terephthalaldehyde is added, and the pH is adjusted to 7.5, and the mixture is stirred sufficiently to obtain a modified melamine body;

[0113] S13: The kaolin liquid, modified melamine and the active agent are mixed in a weight ratio of 5:1:2, and the mixture is ball-milled at a speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a modifier doped with kaolin.

[0114] The mass fraction of the sodium dodecylbenzenesulfonate solution of the present embodiment is 7%.

[0115] The preparation method of the activator of this embodiment is:

[0116] 4 parts of silane coupling agent KH550 and 3 parts of urea were added to 8 parts of ethanol solvent, and then 5 parts of silicon carbide whiskers and 2 parts of amino silicone oil were added and mixed thoroughly, and then washed with water and dried to obtain an active agent.

[0117] Embodiment 3: A process for preparing a packaging paper bag, comprising the following steps:

[0118] Step 1: Prepare the tissue wrapping paper:

[0119] (1) Weigh the following raw materials by weight: 57.5 parts of softwood pulp, 47.5 parts of hardwood pulp, 17.5 parts of starch, 10 parts of functional multi-adjustable stabilizer, 5.5 parts of kaolin-doped modifier, 5.5 parts of silane coupling agent KH560, 3.5 parts of polyvinyl alcohol, and 3 parts of gelatin;

[0120] (2) beating softwood pulp and hardwood pulp to form a slurry, and then mixing the slurry with starch, a functional multi-adjusting stabilizer, a modifier doped with kaolin, a silane coupling agent KH560, polyvinyl alcohol, and gelatin to obtain a base paper agent;

[0121] (3) Dehydrating the base paper through a screen section and a press section to form the base paper, and pressing it on a paper press to obtain a thin sheet packaging paper;

[0122] Step 2: sealing the thin wrapping paper with a film, wherein a PE film is pressed onto the thin wrapping paper for sealing;

[0123] Step 3: Cut, fold, glue and print the sealed thin wrapping paper to obtain a wrapping paper bag.

[0124] The concentration of the pulp formed by the beating treatment of coniferous wood pulp and hardwood wood pulp in this embodiment is 4.5%.

[0125] The preparation method of the functional multi-adjustable stabilizer of this embodiment is:

[0126] S01: first prepare a sodium silicate solution with a mass fraction of 5.5% and a phosphate buffer solution with a pH value of 5.0; then stir the flaky talc, the sodium silicate solution and the phosphate buffer solution in a weight ratio of 3:5:1, filter and dry after stirring to obtain a flaky talc;

[0127] S02: Preparation of conditioning solution based on wollastonite modification:

[0128] S021: irradiating the wollastonite in a proton irradiation box for 7.5 minutes at an irradiation power of 370 W, and then preheating the wollastonite at 60° C. for 15 minutes to obtain preheated wollastonite;

[0129] S022: then immerse the preheated wollastonite in a yttrium nitrate solution of 4 times the total mass of the wollastonite and fully immerse it in ultrasound with an ultrasound power of 370 W and an ultrasound time of 25 min. After the immersion is completed, a wollastonite agent is obtained;

[0130] S023: 4 parts of wollastonite agent, 2 parts of silane coupling agent KH560 and 5.5 parts of chitosan solution are fully mixed, and then 3 parts of hydroxyapatite and 1.5 parts of nano-silica sol are added and mixed thoroughly to obtain a wollastonite-modified conditioning solution;

[0131] S03: The flaky talc powder is immersed in a wollastonite-modified regulating liquid which is 3.5 times the total mass of the flaky talc powder. After the immersion is completed, the liquid is filtered and dried to obtain a functional multi-adjustable stabilizer.

[0132] In the stirring treatment in S01 of this embodiment, the stirring temperature is 57.5° C., the stirring speed is 500 r / min, and the stirring is for 25 minutes; the immersion power of the immersion treatment in S03 is 375 W, and the immersion time is 25 minutes.

[0133] The mass fraction of the yttrium nitrate solution in this embodiment is 4.5%; the mass fraction of the chitosan solution is 3.5%.

[0134] The preparation method of the modifier doped with kaolin in this embodiment:

[0135] S11: adding kaolin to the sodium dodecylbenzene sulfonate solution at a weight ratio of 2:5 and dispersing the mixture evenly to obtain a kaolin solution;

[0136] S12: Preparation of modified melamine body:

[0137] Melamine and paraformaldehyde are mixed in a weight ratio of 1:4, and then water and alkali are added, and the mixture is reacted at 80° C. for 20 minutes, and then terephthalaldehyde is added, and the pH is adjusted to 7.5, and the mixture is stirred sufficiently to obtain a modified melamine body;

[0138] S13: The kaolin liquid, modified melamine and the active agent are mixed in a weight ratio of 5:1:2, and the mixture is ball-milled at a speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a modifier doped with kaolin.

[0139] The mass fraction of the sodium dodecylbenzenesulfonate solution of the present embodiment is 5.5%.

[0140] The preparation method of the activator of this embodiment is:

[0141] 3 parts of silane coupling agent KH550 and 2 parts of urea were added to 6.5 parts of ethanol solvent, and then 4 parts of silicon carbide whiskers and 1.5 parts of amino silicone oil were added and mixed thoroughly, and then washed with water and dried to obtain an active agent.

[0142] Comparative Example 1:

[0143] The difference from Example 3 is that no multi-functional stabilizer is added.

[0144] Comparative Example 2:

[0145] The difference from Example 3 is that no wollastonite-modified regulating liquid treatment is added in the preparation of the functional multi-regulating stabilizer.

[0146] Comparative Example 3:

[0147] The difference from Example 3 is that no flaky talc powder is added in the preparation of the multi-functional stabilizer.

[0148] Comparative Example 4:

[0149] The difference from Example 3 is that the flaky talc agent is replaced by flaky talc powder.

[0150] Comparative Example 5:

[0151] The difference from Example 3 is that no modifier doped with kaolin is added.

[0152] Comparative Example 6:

[0153] The difference from Example 3 is that no kaolin liquid is added in the preparation of the kaolin-doped modifier.

[0154] Comparative Example 7:

[0155] The difference from Example 3 is that no modified melamine is added in the preparation of the modifier doped with kaolin.

[0156] Comparative Example 8:

[0157] The difference from Example 3 is that no activator is added in the preparation of the modifier doped with kaolin.

[0158] Comparative Example 9:

[0159] The difference from Example 3 is that no silane coupling agent KH550 or urea is added to the active agent.

[0160] Comparative Example 10:

[0161] The difference from Example 3 is that silicon carbide whiskers and amino silicone oil are not added to the active agent. The active agent is prepared by adding 3 parts of silane coupling agent KH550 and 2 parts of urea to 6.5 parts of ethanol solvent and mixing them thoroughly to obtain the active agent.

[0162] The products of Examples 1-3 and Comparative Examples 1-10 were tested for strength and barrier properties. The test results are shown in Table 1.

[0163] Table 1: Test results of product strength and barrier properties of Examples 1-3 and Comparative Examples 1-10

[0164]

[0165] As can be seen from Table 1, the product of Example 3 has excellent tensile strength performance, low oxygen permeability, and excellent barrier performance. The tensile strength and barrier performance of the product can be improved in a coordinated manner.

[0166] The present invention does not add any of the functional multi-adjusting stabilizer and the modifier doped with kaolin, and the performance of the product deteriorates significantly. The two are coordinated and coordinated to enhance the performance together, and the product performance effect is most significant;

[0167] The performance of the products tended to deteriorate when the flaky talc powder was not added in the preparation of the functional multi-adjusting stabilizer, when the flaky talc powder was replaced by the flaky talc powder, and when the flaky talc powder was obtained by the method of the present invention and treated with the flaky talc powder and the flaky talc powder, the product performance effect was the most significant. At the same time, the product performance deteriorated significantly when the flaky talc powder was not added and treated with the wollastonite-modified regulating liquid.

[0168] In the preparation of the modifier doped with kaolin, no kaolin liquid was added, no modified melamine body was added, no activator was added, no silane coupling agent KH550 and urea were added to the activator, and no silicon carbide whisker and amino silicone oil were added to the activator. The performance of the products all tended to deteriorate to varying degrees. The performance effect of the doped kaolin modifier prepared by combining the activator obtained by the specific method of the present invention with kaolin liquid and modified melamine body was the most significant.

[0169] Based on the strength and barrier performance tests, the present invention further explores the waterproof and oil-proof properties of the product. The waterproof and oil-proof performance test results are shown in Table 2.

[0170] Table 2: Test results of waterproof and oil-proof performance of products of Examples 1-3 and Comparative Examples 1-10

[0171]

[0172] As can be seen from Table 2, the product of Example 3 of the present invention has excellent strength and barrier properties, and has a significant water contact angle and oil resistance level. The product achieves coordination of strength, barrier, and water and oil resistance performances.

[0173] The multifunctional stabilizer and the kaolin-doped modifier obtained by the specific method of the present invention are coordinated and matched to enhance the synergy together, and the product performance effect is most significant. The technical effect of the present invention cannot be achieved by using other methods instead.

[0174] The present invention further explores the product performance through the preparation of a regulating liquid based on wollastonite modification. The test results of the product strength, barrier, waterproof and oil-proof properties are shown in Table 3.

[0175] Experimental Example 1:

[0176] The only difference from Example 3 is that no wollastonite agent is added in the preparation of the wollastonite-modified regulating solution.

[0177] Experimental Example 2:

[0178] The only difference from Example 3 is that the wollastonite agent was not fully immersed in the yttrium nitrate solution and ultrasonically immersed in the solution during preparation.

[0179] Experimental Example 3:

[0180] The only difference from Example 3 is that no hydroxyapatite is added in the preparation of the conditioning solution based on wollastonite modification.

[0181] Experimental Example 4:

[0182] The only difference from Example 3 is that no silane coupling agent KH560 and nano-silica sol are added in the preparation of the regulating solution based on wollastonite modification.

[0183] Experimental Example 5:

[0184] The only difference from Example 3 is that no chitosan solution is added in the preparation of the regulating solution based on wollastonite modification.

[0185] Table 3: Product performance test results of Experimental Examples 1-5

[0186]

[0187] As can be seen from Table 3, wollastonite was not added in the preparation of the regulating solution modified by wollastonite, which had the greatest influence on the preparation factors of the regulating solution modified by wollastonite, followed by the fact that hydroxyapatite was not added. At the same time, the yttrium nitrate solution was not immersed in ultrasound sufficiently in the preparation of the wollastonite agent, the silane coupling agent KH560 and nano-silica sol were not added in the preparation of the regulating solution modified by wollastonite, and the chitosan solution was not added in the preparation of the regulating solution modified by wollastonite. The performance of the products all had a trend of deterioration to varying degrees. The preparation of the regulating solution modified by wollastonite was proprietary. The regulating solution modified by wollastonite obtained by the specific method of the present invention had the most significant product performance effect. Other methods were not as obvious as the effect of the present invention.

[0188] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0189] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A process for preparing a packaging paper bag, characterized in that: The following steps are involved: Step 1: Prepare the tissue wrapping paper: (1) Weigh the raw materials by weight: 55-60 parts of softwood pulp, 45-50 parts of hardwood pulp, 15-20 parts of starch, 8-12 parts of functional multi-adjustable stabilizer, 4-7 parts of modifier doped with kaolin, 4-7 parts of silane coupling agent KH560, 2-5 parts of polyvinyl alcohol, and 2-4 parts of gelatin; (2) beating softwood pulp and hardwood pulp to form a slurry, and then mixing the slurry with starch, a functional multi-adjusting stabilizer, a modifier doped with kaolin, a silane coupling agent KH560, polyvinyl alcohol, and gelatin to obtain a base paper agent; (3) Dehydrating the base paper through a screen section and a press section to form the base paper, and pressing it on a paper press to obtain a thin sheet packaging paper; Step 2: sealing the thin wrapping paper with a film, wherein a PE film is pressed onto the thin wrapping paper for sealing; Step 3: cutting, folding, gluing and printing the thin wrapping paper after the sealing process to obtain a wrapping paper bag; The preparation method of the functional multi-adjustable stabilizer is: S01: first prepare a sodium silicate solution with a mass fraction of 4-7% and a phosphate buffer solution with a pH value of 5.0; then stir the flaky talc, the sodium silicate solution and the phosphate buffer solution in a weight ratio of 3:5:1, filter and dry after stirring to obtain a flaky talc; S02: Preparation of conditioning solution based on wollastonite modification: S021: irradiating the wollastonite in a proton irradiation box for 5-10 minutes at an irradiation power of 350-400W, and then preheating the wollastonite at a temperature of 55-65°C for 10-20 minutes to obtain preheated wollastonite; S022: then immerse the preheated wollastonite in a yttrium nitrate solution 3-5 times the total mass of the wollastonite and perform ultrasonic treatment sufficiently, with an ultrasonic power of 350-400 W and an ultrasonic time of 20-30 min. After the immersion is completed, a wollastonite agent is obtained; S023: 3-5 parts of wollastonite agent, 1-3 parts of silane coupling agent KH560 and 4-7 parts of chitosan solution are fully mixed, and then 2-4 parts of hydroxyapatite and 1-2 parts of nano-silica sol are added and mixed thoroughly to obtain a wollastonite-modified conditioning solution; S03: dipping the flaky talc in a wollastonite-modified regulating liquid in an amount of 2-5 times the total mass of the flaky talc, filtering and drying after the dipping is completed to obtain a functional multi-regulating stabilizer; The preparation method of the modifier doped with kaolin: S11: adding kaolin to the sodium dodecylbenzene sulfonate solution at a weight ratio of 2:5 and dispersing the mixture evenly to obtain a kaolin solution; S12: Preparation of modified melamine body: Melamine and paraformaldehyde are mixed in a weight ratio of 1:4, and then water and alkali are added, reacting at 75-85°C for 20 minutes, and then terephthalaldehyde is added, the pH is adjusted to 7.5, and stirred sufficiently to obtain a modified melamine body; S13: mixing kaolin liquid, modified melamine and activator in a weight ratio of 5:1:2, and ball milling at a ball milling speed of 1500 r / min for 2 h. After the ball milling is completed, filtering and drying are performed to obtain a modifier doped with kaolin; The preparation method of the effect agent is: 2-4 parts of silane coupling agent KH550 and 1-3 parts of urea are added to 5-8 parts of ethanol solvent, and then 3-5 parts of silicon carbide whiskers and 1-2 parts of amino silicone oil are added and mixed thoroughly, and then washed with water and dried to obtain an active agent.

2. The process for preparing a packaging paper bag according to claim 1, characterized in that: The concentration of the pulp formed by the beating treatment of the coniferous wood pulp and the hardwood wood pulp is 4.5%.

3. The process for preparing a packaging paper bag according to claim 1, characterized in that: The stirring temperature of the stirring treatment in S01 is 55-60°C, the stirring speed is 450-550r / min, and the stirring time is 20-30min; the impregnation power of the impregnation treatment in S03 is 350-400W, and the impregnation time is 20-30min.

4. The process for preparing a packaging paper bag according to claim 1, characterized in that: The mass fraction of the yttrium nitrate solution is 3-6%; the mass fraction of the chitosan solution is 2-5%.

5. The process for preparing a packaging paper bag according to claim 1, characterized in that: The mass fraction of the sodium dodecylbenzene sulfonate solution is 4-7%.

6. A packaging paper bag prepared by the process for preparing a packaging paper bag according to any one of claims 1 to 5.

7. The thin wrapping paper prepared by the process for preparing a wrapping paper bag as claimed in any one of claims 1 to 5.