Metal-supported multi-time sintering device for solid oxide fuel cell and sintering method of metal-supported multi-time sintering device
Through multiple sintering devices and methods, the problem of material performance degradation during SOFC sintering at high temperatures is solved, faster startup speed, higher mechanical strength and longer life are achieved, making it suitable for mass production.
Patent Information
- Application Number
- CN202410992693.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional solid oxide fuel cells (SOFC) have problems such as oxidation, coarsening, and diffusion during the sintering process at high temperatures, resulting in a decline in material performance. Moreover, traditional preparation methods are costly and complex to operate, making them unsuitable for mass production.
A metal-supported multiple sintering device and method is designed, using porous 430L stainless steel plates and ScSZ ceramic materials, through multiple sintering at low and medium temperatures, combined with air extraction and driving mechanisms to achieve gas circulation, ensuring that the material is heated evenly and at high temperatures. Under protective gas protection to avoid oxidation and thermal expansion.
It improves the startup speed, mechanical strength and high temperature resistance of SOFC, extends its life, enhances battery performance, reduces costs, and is suitable for mass production.
Smart Images

Figure CN118729776A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid oxide fuel cells, and in particular to a metal-supported multiple sintering device for solid oxide fuel cells and a sintering method thereof. Background Art
[0002] Compared with other fuel cell technologies, SOFC has a high operating temperature and takes a long time to reach the critical operating temperature and play an energy supply role, and the startup time is long. The high-temperature operation of SOFC will have a great impact on the surroundings, so good thermal shielding is required, which leads to an increase in system mass. This is the main reason why SOFC has a low share in the portable field and emergency power supply field; The new generation of metal-supported SOFC (MS-SOFC) is expected to solve such problems better; compared with the traditional structure SOFC, MS-SOFC has the following advantages: mature welding technology makes the battery stack easy to seal; good mechanical properties make the battery stack have better thermal shock resistance; excellent thermal conductivity makes the battery stack have a high start-stop rate; more compact size and lower manufacturing cost.
[0003] Although metal-supported SOFC (MS-SOFC) has lower cost, faster startup speed, higher mechanical strength, and simpler sealing method compared with electrolyte-supported SOFC and electrode-supported SOFC, the preparation problem of the battery has always greatly restricted the development of MS-SOFC. When the mature wet chemical preparation method of traditional batteries is applied to the preparation of MS-SOFC, many problems will arise due to the characteristics of the metal support itself; for example, the metal support, especially Fe-based metal materials, will be oxidized and destroyed in the sintering process due to high temperature and air atmosphere, so it is necessary to maintain a reducing atmosphere; under a reducing atmosphere, Ni in the anode active layer will coarsen and agglomerate under high temperature conditions, and will also diffuse with the elements in the support, reducing the performance of the support and anode materials; the reducing atmosphere also puts higher requirements on the cathode material, and traditional cathode materials such as LSM will be decomposed in a reducing atmosphere; and during the sintering process, since the heating rods are distributed inside the side wall of the sintering furnace, it is difficult to keep the metal support heated evenly during the heating process. After sintering, the metal support will naturally take too long and cause heat waste.
[0004] The main preparation method of MS-SOFC is to prepare a metal support and then deposit the anode active layer, electrolyte layer and cathode active layer on its surface using thin film preparation methods such as plasma spraying, pulsed laser deposition, magnetron sputtering, and physical vapor deposition. These thin film preparation methods can prepare thinner and denser electrolyte layers at lower temperatures, avoiding various preparation problems caused by high-temperature sintering required by traditional preparation processes. However, these preparation and molding methods are complex to operate and costly, which is not conducive to large-scale production.
[0005] Therefore, it is necessary to provide a new metal-supported multiple sintering device for solid oxide fuel cells and a sintering method thereof to solve the above-mentioned technical problems. Summary of the invention
[0006] The technical problem solved by the present invention is to provide a multiple sintering device and a sintering method of a metal support for a solid oxide fuel cell which is cheap, simple and easy to realize large-scale production.
[0007] In order to solve the above technical problems, the metal-supported multiple sintering device for solid oxide fuel cells provided by the present invention comprises: a sintering furnace, wherein partitions are symmetrically installed inside the sintering furnace, and multiple heating rods are installed between the partitions and the sintering furnace and inside the bottom end of the sintering furnace; an exhaust mechanism for driving the gas to circulate inside the sintering furnace is installed at the top of the sintering furnace, and the exhaust mechanism comprises a cylinder, and multiple cylinders are installed at the center of the top surface of the sintering furnace, and the interior of the cylinder is rotatably connected to a fixed shaft and a fan blade, and the two ends of the fixed shaft are respectively connected to the fan blade and a motor; the cylinder is connected to the second solid The fixed pipe is connected to the interior of the suction cylinder, and a funnel-shaped fixing block and a nozzle are installed inside the suction cylinder, and the nozzle is connected to the second fixed pipe. An annular groove is provided inside the fixing block, and the interior of the groove is connected to the suction pipe with an "L"-shaped side wall, and the bottom end of the suction pipe is connected to the interior of the sintering furnace; a driving mechanism for driving the gas movement is installed at the bottom end of the sintering furnace, and a drying box is symmetrically installed on the side wall of the sintering furnace; the drying box and the interior of the sintering furnace are connected to the exhaust mechanism through a connecting mechanism, and a heat dissipation mechanism for accelerating the heat dissipation efficiency inside the sintering furnace is installed inside the sintering furnace.
[0008] Preferably, the connecting mechanism comprises a main pipe, the main pipe is symmetrically installed at the edge of the top surface of the sintering furnace, a plurality of second connecting pipes are installed on the side wall of the main pipe, and the bottom end of the second connecting pipe is located between the partition and the sintering furnace.
[0009] Preferably, a plurality of first connecting pipes are installed on the side wall of the main pipe, a flow control valve is installed on the side wall of the first connecting pipe, and the bottom end of the first connecting pipe is connected to the interior of the drying box.
[0010] Preferably, a plurality of mounting frames are installed inside the drying box, and the exhaust pipe is installed at the bottom end of the drying box.
[0011] Preferably, one end of the suction cylinder is fixedly connected to a first fixed pipe, and one end of the first fixed pipe is fixedly connected to the main pipe.
[0012] Preferably, the heat dissipation mechanism includes a fan, which is installed on the surface of the drying box and is connected to a heat dissipation pipe; the heat dissipation pipe is fixed to the top of the sintering furnace, and a plurality of nozzles are obliquely installed on the side wall of the heat dissipation pipe, and the bottom end of the nozzle is located between the partition and the sintering furnace.
[0013] Preferably, the driving mechanism includes a first mounting tube and a second mounting tube, a plurality of second mounting tubes are installed at the bottom end of the partition, and the first mounting tubes are vertically installed on the side walls of the second mounting tubes; a clamping block is installed at one end of the second mounting tube, and one end of the first mounting tube and the interior of the clamping block are both funnel-shaped.
[0014] Preferably, an industrial computer is installed on the side wall of the drying box, and the industrial computer is electrically connected to the thermometer, the heating rod, the motor, the flow control valve and the fan respectively, and the thermometer is installed inside the sintering furnace.
[0015] A multiple sintering method for a metal support for a solid oxide fuel cell comprises the following steps: Step 1: Use laser drilling technology to punch holes in a 430L stainless steel plate. A layer of fused quartz coating is applied on the surface of the stainless steel plate. The punched porous stainless steel plate is used as a metal support for the solid oxide fuel cell. The thickness of the plate groove is 200-500 μm. Step 2: Select 500 mesh 430L stainless steel powder and ScSZ ceramic material as the initial powder, select DM-55 as the dispersant, butanone and anhydrous ethanol as the organic solvent, B-50 as the plasticizer, B-72 as the binder, ammonium oxalate as the pore-forming agent, prepare the porous 430L stainless steel-ScSZ composite layer slurry, set the tape casting knife height to 200um, use the tape casting molding technology to make the film tape, dry it at room temperature for use; select ... agent, B-72 as a binder to prepare electrolyte layer slurry, set the casting knife height to 50um, use the casting molding technology to make a membrane tape, and dry it at room temperature for use; select ScSZ ceramic material as the initial powder, select DM-55 as the dispersant, butanone and anhydrous ethanol as organic solvents, B-50 as the plasticizer, B-72 as the binder, and ammonium oxalate as the pore-forming agent to prepare porous ScSZ slurry, set the casting knife height to 100um, and use the casting molding technology to make a membrane tape; put the membrane tape into the drying oven for drying, and use the heat and gas emitted by the sintering furnace to quickly dry the membrane tape; Step 3: Put the dried porous 430L stainless steel-ScSZ composite layer membrane tape and the porous ScSZ layer membrane tape into the sintering furnace for low-temperature sintering, and operate the exhaust mechanism in the sintering furnace to make the gas inside the sintering furnace circulate inside the sintering furnace so that the membrane tape is heated evenly; and at a heating rate of 2°C / min, the temperature is raised to 100°C, and then kept at this temperature for 0.5h, and then heated again to 150°C, and then kept at this temperature for 0.5h, and then heated again to 200°C, and then kept at this temperature for 1h before sintering is terminated; after sintering is completed, open the heat dissipation mechanism, and the heat dissipation mechanism draws air between the partition and the sintering furnace, so that the air is heated and then enters the interior of the sintering furnace through the driving mechanism; open the connecting mechanism, so that part of the gas circulates inside the sintering furnace to prevent the temperature inside the sintering furnace from dropping too fast, and another part of the gas enters the interior of the drying box through the connecting mechanism, so that the workpiece is quickly dried inside the drying box; Step 4: Prepare a mixed aqueous solution of Sm(NO3)3 and Ce(NO3)3 in a stoichiometric ratio, add citric acid in a molar ratio of 1:1 to the metal ions, and prepare a Ni(NO3)2 aqueous solution; alternately immerse the two prepared mixed aqueous solutions on the surface of the porous 430L stainless steel-ScSZ composite layer membrane tape; for the cathode, prepare a mixed aqueous solution of La(NO3)3, Sr(NO3)2, Fe(NO3)3 and Co(NO3)2 in a stoichiometric ratio, add citric acid in a molar ratio of 1:1 to the metal ions, and immerse the prepared L The SCF mixed aqueous solution is impregnated into the cathode side of the porous ScSZ battery and impregnated on the surface of the porous ScSZ membrane strip; the GDC powder is prepared by the EDTA-citric acid double complex method, and the mass ratio is GDC powder: ethyl cellulose: pine alcohol: triolein = 1:0.01:0.125:0.07. The ratio is mixed and ground for 4 hours to obtain a GDC barrier layer slurry, and the solid content of GDC is about 70%. The slurry is attached to the surface of the ScSZ electrolyte layer membrane strip by screen printing; and the processed membrane strip is placed in the drying box for drying; Step 5: Place the dried new porous 430L stainless steel-ScSZ composite layer membrane tape, the ScSZ electrolyte layer membrane tape with a barrier layer and the new porous ScSZ layer membrane tape into the sintering furnace for medium-temperature sintering, and realize gas internal circulation through the exhaust mechanism and the drive mechanism to make the membrane tape evenly heated; increase the temperature to 600°C at a rate of 10°C / min, and then keep it at this temperature for 1h, increase the temperature again to 800°C, and then keep it at this temperature for 1h before ending the sintering. After sintering, use the heat dissipation mechanism to heat the membrane tape The temperature is evenly and quickly lowered; sintering at 600℃ allows the impregnated organic additives to be decomposed as completely as possible, avoiding the influence of carbon elements in the subsequent sintering process. In addition, within the temperature range of 600℃, the thermal shrinkage of 430L stainless steel and ScSZ materials is basically the same, and the two materials will not have expansion rejection. After continuing to rise to 800℃ and keeping warm, the undecomposed organic additives are completely decomposed. At the same time, the 430L stainless steel and ScSZ materials can adapt to high temperatures, and a little rejection occurs, which can be artificially polished and repaired to improve structural stability. Step 6: Cut the prepared functional layer membrane strips into the same size as the metal support porous stainless steel plate, and polish the double-sided functional layer membrane strips with 400-grit sandpaper to increase the roughness for better adhesion of each contact surface; overlap the new membrane strips in the order of porous 430L stainless steel substrate support layer, porous 430L stainless steel-ScSZ composite layer, ScSZ electrolyte layer, GDC barrier layer and porous SSZ layer, and press them together with a hot press to obtain a battery skeleton, put the battery skeleton into the sintering furnace, introduce 5% H2 and 95% N2 mixed gas as protective gas, and sinter at a high temperature of 1350°C. During the sintering process, the gas is circulated internally through the exhaust mechanism and the drive mechanism, so that the battery skeleton is heated evenly and the quality of the battery skeleton is improved; after the sintering is completed, the metal support of the solid oxide fuel cell can be obtained: Compared with the related art, the metal-supported multiple sintering device for solid oxide fuel cells and the sintering method thereof provided by the present invention have the following beneficial effects: The use of porous 430L stainless steel plates coated with fused quartz coating as the support of solid fuel cells makes the fuel cell have a faster startup speed and higher mechanical strength. At the same time, the fused quartz coating can prevent the outer periphery of the stainless steel plate from rapid oxidation at high temperatures. The use of multiple temperature sintering method to calcine various materials of the battery makes the solid oxide fuel cell more stable in high temperature resistance, with a smaller attenuation rate and a longer life. Specifically, multiple low-temperature sintering at different temperature ranges can make the pore size of the ammonium oxalate pores layered and uniform, so as to facilitate the subsequent impregnation of anode and cathode slurries. Compared with the method of direct impregnation sintering and debinding without low-temperature sintering, the porous porosity will increase, the amount of impregnated anode and cathode slurry will increase, making the battery performance more excellent. At the same temperature, the maximum power density of the single battery is significantly improved; multiple medium-temperature sintering at different temperature ranges can completely decompose and discharge the impregnated organic additives, and will not affect the battery performance due to trace amounts of organic matter that has not been completely discharged; at the same time, it can make the material better adapt to high temperatures, and will not increase the temperature rapidly during the subsequent high-temperature sintering, causing the material to have excessive high-temperature thermal expansion rejection, resulting in coil deformation and warping, which will affect the battery life; when a mixed gas of 5% H2 and 95% N2 is introduced as a protective gas, 1350℃ high-temperature sintering can make the contact surfaces of the various parts of the battery more fused, the electrolyte membrane more dense, and at the same time prevent some battery materials from being oxidized at high temperature. The product has a high yield rate and good quality, and is suitable for large-scale batch production; During the process of sintering the film strip and the battery frame being placed in the sintering furnace, the gas is driven by the exhaust mechanism and the driving mechanism to circulate rapidly inside the sintering furnace, so that the film strip and the battery frame are evenly heated inside the sintering furnace and the temperature is quickly increased. The undried film strip and the battery frame are placed in the drying box and are quickly dried by the heat dissipated by the sintering furnace. After the sintering is completed, air is introduced into the internal interlayer of the sintering furnace through the heat dissipation mechanism box, so that the air is mixed with the hot air ejected by the exhaust mechanism and then enters the sintering furnace again, so as to avoid the temperature in the sintering furnace from dropping too fast and affecting the quality of the film strip and the battery frame. After the gas is extracted by the exhaust mechanism, part of the gas circulates inside the sintering furnace, so as to avoid the temperature inside the sintering furnace from dropping too fast, and the other part of the gas enters the drying box through the connecting mechanism, so that the workpiece is quickly dried inside the drying box, and the waste heat of the sintering furnace is reasonably utilized. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A schematic structural diagram of a preferred embodiment of a multiple sintering device and a sintering method for a metal support for a solid oxide fuel cell provided by the present invention; Figure 2 for Figure 1 A side view of the internal structure of the sintering furnace is shown; Figure 3 for Figure 2 An enlarged schematic diagram of the structure at A shown; Figure 4 for Figure 3 An enlarged schematic diagram of the structure at D shown; Figure 5 for Figure 2 An enlarged schematic diagram of the structure at B shown; Figure 6 for Figure 5 A schematic diagram of the internal structure of the second mounting tube shown; Figure 7 for Figure 2 An enlarged schematic diagram of the structure at position C is shown; Figure 8 A schematic diagram of the circuit structure provided by the present invention; Fig. 9 A schematic diagram of the interior of a metal support for a solid oxide fuel cell provided by the present invention; Fig.10 The electrochemical performance test diagram of the metal support provided by the present invention at 650°C to 800°C; Fig.11 The electrochemical performance test diagram of the flat-plate MS-SOFC prepared by one-step co-sintering method at 650℃~800℃; Fig.12A diagram of a 100-hour rapid thermal test of the metal support provided by the present invention.
[0017] Numbers in the figure: 1. sintering furnace, 11. heating rod, 12. partition, 2. exhaust mechanism, 21. first fixed pipe, 22. motor, 23. cylinder, 24. fixed shaft, 25. fan blade, 26. second fixed pipe, 27. suction pipe, 28. suction cylinder, 29. fixed block, 210. groove, 211. nozzle, 3. connecting mechanism, 31. main pipe, 32. first connecting pipe, 33. second connecting pipe, 34. flow control valve, 4. heat dissipation mechanism, 41. fan, 42. heat dissipation pipe, 43. nozzle, 5. drying box, 51. mounting frame, 52. exhaust pipe, 6. driving mechanism, 61. first mounting pipe, 62. second mounting pipe, 63. block, 7. industrial computer. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with the accompanying drawings and implementation modes.
[0019] See also Figures 1 to 8 , Figure 1 A schematic structural diagram of a preferred embodiment of a multiple sintering device and a sintering method for a metal support for a solid oxide fuel cell provided by the present invention; Figure 2 for Figure 1 A side view of the internal structure of the sintering furnace is shown; Figure 3 for Figure 2 An enlarged schematic diagram of the structure at A shown; Figure 4 for Figure 3 An enlarged schematic diagram of the structure at D shown; Figure 5 for Figure 2 An enlarged schematic diagram of the structure at B shown; Figure 6 for Figure 5 A schematic diagram of the internal structure of the second mounting tube shown; Figure 7 for Figure 2 An enlarged schematic diagram of the structure at position C is shown; Figure 8 The schematic diagram of the circuit structure provided by the present invention. The metal-supported multiple sintering device for solid oxide fuel cells comprises: a sintering furnace 1, a partition 12 is symmetrically installed inside the sintering furnace 1, and a plurality of heating rods 11 are installed between the partition 12 and the sintering furnace 1 and inside the bottom of the sintering furnace 1; in order to facilitate the rapid increase of the temperature inside the sintering furnace 1 after the heating rod 11 is powered on, the workpiece is sintered inside the sintering furnace 1.
[0020] The top of the sintering furnace 1 is installed with an exhaust mechanism 2 for driving the gas to circulate inside the sintering furnace 1. The exhaust mechanism 2 includes a cylinder 23. A plurality of cylinders 23 are installed at the center of the top surface of the sintering furnace 1. The interior of the cylinder 23 is rotatably connected to a fixed shaft 24 and a fan blade 25, and the two ends of the fixed shaft 24 are respectively connected to the fan blade 25 and the motor 22; the cylinder 23 is connected to the interior of a suction cylinder 28 through a second fixed pipe 26. A funnel-shaped fixed block 29 and a nozzle 211 are installed inside the suction cylinder 28. The nozzle 211 is connected to the second fixed pipe 26. The fixed block 2 9 is provided with an annular groove 210, the interior of the groove 210 is connected to the suction pipe 27 with an "L"-shaped side wall, and the bottom end of the suction pipe 27 is connected to the interior of the sintering furnace 1; the bottom end of the sintering furnace 1 is installed with a driving mechanism 6 for driving the gas movement, the driving mechanism 6 includes a first mounting tube 61 and a second mounting tube 62, a plurality of second mounting tubes 62 are installed at the bottom end of the partition 12, and the side wall of the second mounting tube 62 is vertically installed with the first mounting tube 61; a clamping block 63 is installed at one end of the second mounting tube 62, and one end of the first mounting tube 61 and the interior of the clamping block 63 are both funnel-shaped;When the membrane strip and the battery skeleton are placed in the sintering furnace 1 for sintering, the motor 22 is turned on to drive the fixed shaft 24 and the fan blades 25 to rotate inside the cylinder 23, so that the hot air in the center of the sintering furnace 1 enters the inside of the nozzle 211 through the second fixed pipe 26, and the hot air is accelerated inside the funnel-shaped nozzle 211 and passes through the fixed block 29. When the hot air flows between the fixed blocks 29, according to the wall attachment effect, suction is generated in the gap between the fixed block 29 and the nozzle 211, so that suction is generated inside the groove 210 and the suction pipe 27, so that the suction pipe 27 quickly draws the air inside the top of the sintering furnace 1. By using the principle of air amplifier, the suction pipe 27 quickly draws the air inside the sintering furnace 1 and mixes with the gas ejected from the nozzle 211 and then enters the inside of the first fixed pipe 21. The air passes through in turn. The main pipe 31 and the second connecting pipe 33 enter between the sintering furnace 1 and the partition 12, so that the gas moves downward between the sintering furnace 1 and the partition 12 and contacts the heating rod 11. The heating rod 11 heats the air again and then enters the interior of the second mounting pipe 62. One end of the first connecting pipe 61 is funnel-shaped, so that part of the air inside the second mounting pipe 62 moves upward along the side wall of the sintering furnace 1 through the first connecting pipe 61, and the other part of the air enters the center of the bottom end of the interior of the sintering furnace 1 through the funnel-shaped block 63. Since the second connecting pipes 62 are relatively arranged, the air moving along the bottom end of the interior of the sintering furnace 1 converges with each other at the center of the bottom end of the sintering furnace 1 and moves upward. The air inside the sintering furnace 1 is extracted by the exhaust mechanism 2 and then ejected from two directions through the driving mechanism 6. The gas flow direction inside the sintering furnace 1 is as shown in the attached figure. Figure 2 As shown by the middle arrow, the gas is continuously heated inside the sintering furnace 1 and then circulates, so that the heat inside the sintering furnace 1 is evenly distributed, and the membrane strip and the battery frame are evenly heated.
[0021] The connecting mechanism 3 includes a main pipe 31, which is symmetrically installed at the edge of the top surface of the sintering furnace 1. A plurality of second connecting pipes 33 are installed on the side wall of the main pipe 31, and the bottom end of the second connecting pipe 33 is located between the partition 12 and the sintering furnace 1.
[0022] A drying box 5 is symmetrically installed on the side wall of the sintering furnace 1; a plurality of mounting frames 51 are installed inside the drying box 5, and the exhaust pipe 52 is installed at the bottom end of the drying box 5. In order to facilitate placing the membrane strip and the battery skeleton on the surface of the mounting frame 51, the residual heat inside the sintering furnace 1 is used to quickly dry the membrane strip and the battery skeleton, and the hot air inside the drying box 5 is discharged through the exhaust pipe 52, so that the hot air inside the drying box 5 moves downward, so that the surface of the membrane strip and the battery skeleton is evenly dried.
[0023] The interior of the drying box 5 and the sintering furnace 1 are connected to the exhaust mechanism 2 via a connecting mechanism 3, one end of the suction cylinder 28 is fixedly connected to the first fixed pipe 21, and one end of the first fixed pipe 21 is fixedly connected to the main pipe 31, in order to facilitate the air inside the suction cylinder 28 to enter the interior of the main pipe 31 through the first fixed pipe 21.
[0024] The sintering furnace 1 is provided with a heat dissipation mechanism 4 for accelerating the heat dissipation efficiency inside the sintering furnace 1; a plurality of first connecting pipes 32 are provided on the side wall of the main pipe 31, a flow control valve 34 is provided on the side wall of the first connecting pipe 32, and the bottom end of the first connecting pipe 32 is connected to the inside of the drying box 5; the heat dissipation mechanism 4 includes a fan 41, the fan 41 is provided on the surface of the drying box 5, and the fan 41 is connected to a heat dissipation pipe 42; the heat dissipation pipe 42 is fixed to the top of the sintering furnace 1, a plurality of nozzles 43 are obliquely provided on the side wall of the heat dissipation pipe 42, and the bottom end of the nozzle 43 is located between the partition 12 and the sintering furnace 1, when the inside of the sintering furnace 1 needs to be cooled, the fan 41 operates to draw outside air into the inside of the heat dissipation pipe 42, and the air then obliquely enters between the partition 12 and the sintering furnace 1 through the plurality of nozzles 43, and the air is mixed with the hot air ejected from the second connecting pipe 33 and then passes through the drive The driving mechanism 6 performs a circulating motion to prevent air from suddenly entering the interior of the sintering furnace 1, causing uneven temperature distribution and affecting the quality of the membrane strip and the battery skeleton; and at this time, the flow control valve 34 is opened to allow part of the hot air inside the main pipe 31 to enter the first connecting pipe 32 and the interior of the drying box 5, thereby increasing the internal temperature of the drying box 5 and accelerating the drying efficiency of the membrane strip and the battery skeleton. Another part of the air is passed into the interior of the sintering furnace 1 again through the second connecting pipe 33 to prevent the internal temperature of the sintering furnace 1 from dropping too quickly. During the cooling process, the fan 41 continuously draws air into the interior of the sintering furnace 1, and the air is first mixed with hot air to heat up and then enters the interior of the sintering furnace 1 for movement, so that the interior of the sintering furnace 1 is cooled evenly, and part of the air discharged from the interior of the sintering furnace 1 enters the interior of the drying box 5 for preheating, and the other part enters the interior of the sintering furnace 1 again for circulation, thereby allowing the membrane strip and the battery skeleton to be cooled quickly and evenly.
[0025] An industrial computer 7 is installed on the side wall of the drying box 5. The industrial computer 7 is electrically connected to the thermometer, the heating rod 11, the motor 22, the flow control valve 34 and the fan 41 respectively. The thermometer is installed inside the sintering furnace 1. In order to facilitate the thermometer to record the temperature inside the drying box 1 and transmit the information to the industrial computer 7, the industrial computer 7 adjusts the heating rate inside the sintering furnace 1 by controlling the number of the heating rods 11 opened; the industrial computer 7 operates to turn on the motor 22, so that the gas inside the sintering furnace 1 is heated. Thermal cycle makes the membrane strip and the battery skeleton heated evenly; when the temperature inside the sintering furnace 1 drops, the industrial computer 7 turns on the fan 41 and the flow control valve 34 to pass air into the sintering furnace 1 to cool down the inside of the sintering furnace 1, and during the cooling process, the gas is continuously drawn into the main pipe 31 by the exhaust mechanism 2, and a part of the main pipe 31 enters the drying box 5 for preheating, and the other part is mixed with the cold air and enters the sintering furnace 1 again for circulation, so that the membrane strip and the battery skeleton are cooled quickly and evenly.
[0026] A multiple sintering method for a metal support for a solid oxide fuel cell comprises the following steps: Step 1: Use laser drilling technology to punch holes in a 430L stainless steel plate. A layer of fused quartz coating is applied on the surface of the stainless steel plate. The punched porous stainless steel plate is used as a metal support for the solid oxide fuel cell. The thickness of the plate groove is 200-500 μm. Step 2: Select 500 mesh 430L stainless steel powder and ScSZ ceramic material as initial powder, select DM-55 as dispersant, butanone and anhydrous ethanol as organic solvents, B-50 as plasticizer, B-72 as binder, ammonium oxalate as pore-forming agent, prepare porous 430L stainless steel-ScSZ composite layer slurry, set the tape casting knife height to 200um, use tape casting technology to make film tape, dry at room temperature for use; select ScSZ ceramic material as initial powder, select DM-55 as dispersant, butanone and anhydrous ethanol as organic solvents, B-50 as plasticizer , B-72 is used as a binder to prepare electrolyte layer slurry, the height of the tape casting knife is set to 50um, and a film strip is made by tape casting technology, which is dried at room temperature for use; ScSZ ceramic material is selected as the initial powder, DM-55 is selected as a dispersant, butanone and anhydrous ethanol are used as organic solvents, B-50 is used as a plasticizer, B-72 is used as a binder, and ammonium oxalate is used as a pore-forming agent to prepare a porous ScSZ slurry, the height of the tape casting knife is set to 100um, and a film strip is made by tape casting technology; the film strip is placed in the drying box 5 for drying, and the heat and gas emitted by the sintering furnace 1 are used to quickly dry the film strip; Step 3: Put the dried porous 430L stainless steel-ScSZ composite layer membrane tape and the porous ScSZ layer membrane tape into the sintering furnace 1 for low-temperature sintering. The exhaust mechanism 2 in the sintering furnace 1 operates to make the gas inside the sintering furnace 1 circulate inside the sintering furnace 1 so that the membrane tape is heated evenly; and the temperature is raised to 100°C at a rate of 2°C / min, and then kept at this temperature for 0.5h, and then heated again to 150°C, and then kept at this temperature for 0.5h, and then heated again to 200°C , and then the sintering is terminated after the temperature is kept at this temperature for 1 hour; after the sintering is completed, the heat dissipation mechanism 4 is turned on, and the heat dissipation mechanism 4 draws air into the space 1 between the partition 12 and the sintering furnace, so that the air enters the interior of the sintering furnace 1 through the driving mechanism 6 after being heated; the connecting mechanism 3 is turned on, so that part of the gas circulates inside the sintering furnace 1 to prevent the temperature inside the sintering furnace 1 from dropping too quickly, and the other part of the gas enters the interior of the drying box 5 through the connecting mechanism 3, so that the workpiece is quickly dried inside the drying box 5; Step 4: Prepare a mixed aqueous solution of Sm(NO3)3 and Ce(NO3)3 in a stoichiometric ratio, add citric acid in a molar ratio of 1:1 with the metal ions, and prepare a Ni(NO3)2 aqueous solution; alternately immerse the two prepared mixed aqueous solutions on the surface of the porous 430L stainless steel-ScSZ composite layer membrane tape; for the cathode, prepare a mixed aqueous solution of La(NO3)3, Sr(NO3)2, Fe(NO3)3 and Co(NO3)2 in a stoichiometric ratio, add citric acid in a molar ratio of 1:1 with the metal ions, and immerse the prepared LS The CF mixed aqueous solution is impregnated into the cathode side of the porous ScSZ battery and impregnated on the surface of the porous ScSZ membrane strip; the GDC powder is prepared by the EDTA-citric acid double complex method, and the GDC powder: ethyl cellulose: pinene alcohol: triolein is mixed and ground for 4 hours according to the mass ratio of 1:0.01:0.125:0.07 to obtain a GDC barrier layer slurry with a solid content of about 70% of GDC, and the slurry is attached to the surface of the ScSZ electrolyte layer membrane strip by screen printing; and the processed membrane strip is placed in the drying box 5 for drying; Step 5: Place the dried new porous 430L stainless steel-ScSZ composite layer membrane strip, the ScSZ electrolyte layer membrane strip with a barrier layer and the new porous ScSZ layer membrane strip into the sintering furnace 1 for medium-temperature sintering, and realize gas internal circulation through the exhaust mechanism 2 and the driving mechanism 6 to make the membrane strip heated evenly; increase the temperature to 600°C at a rate of 10°C / min, and then keep it at this temperature for 1h, increase the temperature again to 800°C, and then keep it at this temperature for 1h before ending the sintering. After sintering, use the heat dissipation mechanism 4 to The membrane strip is cooled evenly and quickly; sintering at 600℃ allows the impregnated organic additives to be decomposed as completely as possible, avoiding the influence of carbon elements in the subsequent sintering process. In addition, within the temperature range of 600℃, the thermal shrinkage of 430L stainless steel and ScSZ materials is basically the same, and the two materials will not have expansion rejection. After continuing to rise to 800℃ and keeping warm, the undecomposed organic additives are completely decomposed. At the same time, the 430L stainless steel and ScSZ materials can adapt to high temperatures, and a little rejection occurs, which can be artificially polished and repaired to improve structural stability. Step 6: Cut the prepared functional layer membrane strips into the same size as the metal support porous stainless steel plate, and polish both sides of each functional layer membrane strip with 400-grit sandpaper to increase the roughness for better adhesion of each contact surface; overlap the new membrane strips in the order of porous 430L stainless steel substrate support layer, porous 430L stainless steel-ScSZ composite layer, ScSZ electrolyte layer, GDC barrier layer and porous SSZ layer, and press them together with a hot press to obtain a battery skeleton (such as attached Fig. 9 As shown), the battery skeleton is placed in the sintering furnace 1, and a mixed gas of 5% H2 and 95% N2 is introduced as a protective gas, and sintering is performed at a high temperature of 1350°C. During the sintering process, the gas is circulated internally through the exhaust mechanism 2 and the driving mechanism 6, so that the battery skeleton is heated evenly and the quality of the battery skeleton is improved; after the sintering is completed, the metal support of the solid oxide fuel cell can be obtained.
[0027] The electrochemical performance of the flat-plate MS-SOFC prepared according to the above method was tested at 650℃~800℃. The atmosphere on the anode side of the battery was humid H2 containing 3% H2O, and the cathode side was flowing air. Under different temperature conditions, the battery voltage, current density and corresponding power density are as follows Fig.10 As shown: Using the same SOFC battery material, the flat-plate MS-SOFC prepared by one-step co-sintering method was tested for electrochemical performance at 650℃~800℃. The atmosphere on the anode side of the battery was humid H2 containing 3% H2O, and the cathode side was flowing air. Under different temperature conditions, the battery voltage, current density and corresponding power density are as follows Fig.11 As shown; By comparing the two figures, it can be seen that the maximum power density of the single cell of the flat-plate MS-SOFC prepared by multiple temperature stage sintering is significantly improved compared with the MS-SOFC prepared by one-step co-sintering, which is 228mWcm-2 at 650℃, 246mWcm-2 at 700℃, 334mWcm-2 at 750℃, and 421mWcm-2 at 800℃. Compared with the single cell prepared by one-step co-sintering, the power density is increased by nearly 25%.
[0028] The MS-SOFC prepared by the multiple sintering method was subjected to a 100-hour rapid thermal test. Fig.12 As shown, the peak power attenuation rate is only 2% at 800°C, which has demonstrated good stability performance.
[0029] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A metal-supported multiple sintering device for a solid oxide fuel cell, characterized in that: include: A sintering furnace (1), wherein a partition (12) is symmetrically installed inside the sintering furnace (1), and a plurality of heating rods (11) are installed between the partition (12) and the sintering furnace (1) and inside the bottom end of the sintering furnace (1); The top of the sintering furnace (1) is provided with an exhaust mechanism (2) for driving the gas to circulate in the sintering furnace (1), the exhaust mechanism (2) comprising a cylinder (23), a plurality of cylinders (23) being installed at the center of the top surface of the sintering furnace (1), the interior of the cylinder (23) being rotatably connected to a fixed shaft (24) and a fan blade (25), and the two ends of the fixed shaft (24) are respectively connected to the fan blade (25) and the motor (22); the cylinder (23) is connected to the interior of a suction cylinder (28) through a second fixed pipe (26), the interior of the suction cylinder (28) is provided with a fixed block (29) having a funnel-shaped interior and a nozzle (211), the nozzle (211) being connected to the second fixed pipe (26), the interior of the fixed block (29) being provided with an annular groove (210), the interior of the groove (210) being connected to a suction pipe (27) having an "L"-shaped side wall, and the bottom end of the suction pipe (27) is connected to the interior of the sintering furnace (1); A driving mechanism (6) for driving gas movement is installed at the bottom end of the sintering furnace (1), and a drying box (5) is symmetrically installed on the side wall of the sintering furnace (1); the drying box (5) and the interior of the sintering furnace (1) are connected to the exhaust mechanism (2) via a connecting mechanism (3), and a heat dissipation mechanism (4) for accelerating the heat dissipation efficiency inside the sintering furnace (1) is installed inside the sintering furnace (1).
2. The multiple sintering device for metal support for solid oxide fuel cell according to claim 1, characterized in that: The connecting mechanism (3) comprises a main pipe (31), the main pipe (31) being symmetrically mounted at the edge of the top surface of the sintering furnace (1), a plurality of second connecting pipes (33) being mounted on the side wall of the main pipe (31), the bottom ends of the second connecting pipes (33) being located between the partition plate (12) and the sintering furnace (1).
3. The multiple sintering device of the metal support for solid oxide fuel cell according to claim 2, characterized in that: A plurality of first connecting pipes (32) are installed on the side wall of the main pipe (31), a flow control valve (34) is installed on the side wall of the first connecting pipe (32), and the bottom end of the first connecting pipe (32) is connected to the interior of the drying box (5).
4. The multiple sintering device of the metal support for solid oxide fuel cell according to claim 3, characterized in that: A plurality of mounting frames (51) are installed inside the drying box (5), and the exhaust pipe (52) is installed at the bottom end of the drying box (5).
5. The multiple sintering device for metal support for solid oxide fuel cell according to claim 4, characterized in that: One end of the suction cylinder (28) is fixedly connected to the first fixed pipe (21), and one end of the first fixed pipe (21) is fixedly connected to the main pipe (31).
6. The multiple sintering device for metal support for solid oxide fuel cell according to claim 5, characterized in that: The heat dissipation mechanism (4) comprises a fan (41), the fan (41) is mounted on the surface of the drying box (5), and the fan (41) is connected to a heat dissipation pipe (42); the heat dissipation pipe (42) is fixed to the top of the sintering furnace (1), a plurality of nozzles (43) are obliquely mounted on the side wall of the heat dissipation pipe (42), and the bottom end of the nozzle (43) is located between the partition (12) and the sintering furnace (1).
7. The multiple sintering device for a metal support for a solid oxide fuel cell according to claim 6, characterized in that: The driving mechanism (6) comprises a first mounting tube (61) and a second mounting tube (62); a plurality of second mounting tubes (62) are mounted on the bottom end of the partition (12); the first mounting tube (61) is mounted perpendicularly to the side wall of the second mounting tube (62); a clamping block (63) is mounted on one end of the second mounting tube (62); one end of the first mounting tube (61) and the interior of the clamping block (63) are both funnel-shaped.
8. The multiple sintering device for a metal support for a solid oxide fuel cell according to claim 7, characterized in that: An industrial computer (7) is installed on the side wall of the drying box (5); the industrial computer (7) is electrically connected to the thermometer, the heating rod (11), the motor (22), the flow control valve (34) and the fan (41), respectively; and the thermometer is installed inside the sintering furnace (1).
9. The multiple sintering device for a metal support for a solid oxide fuel cell according to claim 8, characterized in that: A multiple sintering method for a metal support for a solid oxide fuel cell is provided, which specifically comprises the following steps: Step 1: Use laser drilling technology to punch holes in a 430L stainless steel plate. A layer of fused quartz coating is applied on the surface of the stainless steel plate. The punched porous stainless steel plate is used as a metal support for the solid oxide fuel cell. The thickness of the plate groove is 200-500 μm. Step 2: Select 500 mesh 430L stainless steel powder and ScSZ ceramic material as initial powder, select DM-55 as dispersant, butanone and anhydrous ethanol as organic solvents, B-50 as plasticizer, B-72 as binder, ammonium oxalate as pore-forming agent, and prepare porous 430L stainless steel-ScSZ composite layer slurry. The mass ratio of 430 stainless steel and ScSZ powder in the prepared slurry is 1:1, and the total mass accounts for 53.5% of the slurry mass, the binder mass accounts for 5.6% of the slurry mass, the plasticizer accounts for 2% of the total slurry mass, the dispersant DM-55 mass accounts for 5.7% of the slurry mass, the pore-forming agent ammonium oxalate accounts for 20% of the total slurry mass, the butanone and anhydrous ethanol mass ratio is 1:2, and the mass of the organic solvent accounts for 13.2% of the slurry mass. After the slurry is configured, set the casting knife height to 200um, and use the casting molding technology to make a porous 430L stainless steel-ScSZ composite layer membrane belt, which is dried at room temperature for use; ScSZ ceramic material was selected as the initial powder, DM-55 was selected as the dispersant, butanone and anhydrous ethanol were selected as the organic solvents, B-50 was selected as the plasticizer, and B-72 was selected as the binder to prepare the electrolyte layer slurry. In the prepared slurry, the mass of ScSZ powder accounted for 58.5% of the total mass of the slurry, the mass of B-72 binder accounted for 6% of the total mass of the slurry, the plasticizer accounted for 2% of the total mass of the slurry, the mass of DM-55 dispersant accounted for 4% of the total mass of the slurry, the mass ratio of butanone and anhydrous ethanol was 1:2, and the mass of the organic solvent accounted for 29.5% of the mass of the slurry; after the slurry was prepared, the height of the casting knife was set to 50um, and the ScSZ electrolyte layer membrane tape was made by using the casting molding technology, and dried at room temperature for use; Selecting ScSZ ceramic material as initial powder, selecting DM-55 as dispersant, butanone and anhydrous ethanol as organic solvents, B-50 as plasticizer, B-72 as binder, and ammonium oxalate as pore-forming agent to prepare porous ScSZ slurry, wherein the mass of ScSZ powder accounts for 53.5% of the total mass of the slurry, the mass of B-72 binder accounts for 6% of the total mass of the slurry, the plasticizer accounts for 2% of the total mass of the slurry, the mass of DM-55 dispersant accounts for 4% of the total mass of the slurry, the pore-forming agent ammonium oxalate accounts for 20% of the total mass of the slurry, the mass ratio of butanone and anhydrous ethanol is 1:2, and the mass of organic solvent accounts for 14.5% of the mass of the slurry. After the slurry is prepared, the height of the casting knife is set to 100um, and the porous ScSZ layer film strip is produced by using the casting molding technology; the film strip is placed in the drying box (5) for drying, and the heat and gas emitted by the sintering furnace (1) are used to quickly dry the film strip; Step 3: Place the dried porous 430L stainless steel-ScSZ composite layer membrane strip and the porous ScSZ layer membrane strip into the sintering furnace (1) for low-temperature sintering, operate the exhaust mechanism (2) in the sintering furnace (1), so that the gas inside the sintering furnace (1) circulates inside the sintering furnace (1), so that the membrane strip is heated evenly; and heat up to 100°C at a rate of 2°C / min, then keep at this temperature for 0.5h, heat up again to 150°C, then keep at this temperature for 0.5h, heat up again to 200°C, and then heat at this temperature. After 1 hour of heat preservation, sintering is terminated; after sintering is completed, the heat dissipation mechanism (4) is opened, and the heat dissipation mechanism (4) draws air into the space between the partition (12) and the sintering furnace (1), so that the air is heated and then enters the interior of the sintering furnace (1) through the driving mechanism (6); the connecting mechanism (3) is opened, so that part of the gas circulates inside the sintering furnace (1) to prevent the temperature inside the sintering furnace (1) from dropping too quickly, and the other part of the gas enters the interior of the drying box (5) through the connecting mechanism (3), so that the workpiece is quickly dried inside the drying box (5); Step 4: Prepare Sm(NO<-sub2515226b-84a9-4737-9e45-1acec4a1b93d->)<-sub19dc8d3c-de9d-4a26-bfe2-715419a63e00-> and Ce(NO<-sub033841db-38f8-4a29-a586-b3a42d491cbe->)<-sub9cd3eaac-c01d-4ce3-bd5b respectively according to the stoichiometric ratio of Sm:Ce=0.2:0.8 -c1d2afedee4d-> mixed aqueous solution, add citric acid in a molar ratio of 1:1 with metal ions to prepare Ni(NO<-sub8cf2cbe1-7035-4609-85ae-d16d49343f50->)<-sub9c8a7a7e-8578-4633-a99f-5e5736dad5cc-> aqueous solution; the two prepared mixed aqueous solutions are alternately immersed in the surface of the porous 430L stainless steel-ScSZ composite layer membrane tape; for the cathode, La(NO<-s ub2e252897-f64d-4979-bb6b-4f36dee35d9e->)<-sub6e6be348-2729-495a-be8f-4135ed29eff4->, Sr(NO<-sub597a0 260-9c8d-4ac9-bd1f-c4a907d1db8a->)<-subfbdd0c12-0b2b-429a-9a77-e42c86e40553->, Fe(NO<-sub77b52adb-03a 8-49c9-ae9c-f44bc91edc36->)<-sub38f3cf84-f94f-423a-bc79-e10c4863f2cc-> and Co(NO<-sub61eb8296-d1c8-400c-aaa0-7c66637cbef3->)<-sub4a7c6caa-2c87-4ab3-9146-872a6c387f15-> mixed aqueous solution, citric acid in a molar ratio of 1:1 with metal ions was added to obtain a LSCF mixed aqueous solution, Among them La(NO<-sub1a95c828-1748-4af4-8d1a-4490b7e44416->)<-sub5c29b4e1-288c-418c-85f8-7fc19ca9552b->, Sr(NO<-sub4ce7b882- 9bce-411d-93bf-87ee9a4e35dc->)<-sub73a5a747-efca-4248-ba19-e1196b46660b->, Fe(NO<-sub33b34498-d9a5-4d40-b7c9-e03fce The ratio of the amount of each metal ion substance in 3a2a6b->)<-sub48fe9d67-0983-40e3-b871-1b7ca6cb5119-> and Co(NO<-sub311dddff-fe8e-40e9-b983-0f4f998ffc35->)<-subef7d4b1f-1653-43fc-aa78-d71e49b53ce7-> is La:Sr:Co:Fe=0.6:0.4:0.2:0.8; the prepared LSCF mixed aqueous solution is impregnated into the cathode side of the porous ScSZ battery and impregnated on the surface of the porous ScSZ membrane strip; The GDC powder is prepared by the EDTA-citric acid double complex method. The mixture is mixed and ground for 4 hours in a mass ratio of GDC powder: ethyl cellulose: pinene alcohol: triolein = 1:0.01:0.125:0.07 to obtain a GDC barrier layer slurry with a solid content of about 70%. The slurry is attached to the surface of the ScSZ electrolyte layer membrane tape by screen printing. The processed membrane tape is placed in the drying oven (5) for drying. Step 5: Place the dried new porous 430L stainless steel-ScSZ composite layer membrane strip, the ScSZ electrolyte layer membrane strip with a barrier layer, and the new porous ScSZ layer membrane strip into the sintering furnace (1) for medium-temperature sintering, and realize gas internal circulation through the exhaust mechanism (2) and the drive mechanism (6) so that the membrane strip is heated evenly; heat up at a rate of 10°C / min to 600°C, then keep at this temperature for 1 hour, heat up again to 800°C, and then keep at this temperature for 1 hour before sintering is terminated, and use the heat dissipation mechanism after sintering (4) The membrane strip is cooled evenly and quickly; sintering at 600°C allows the impregnated organic additives to be decomposed as completely as possible, avoiding the influence of carbon elements in the subsequent sintering process. In addition, within the temperature range of 600°C, the thermal shrinkage of 430L stainless steel and ScSZ materials is basically the same, and the two materials will not have expansion rejection. The temperature is further increased to 800°C and then kept warm, so that the undecomposed organic additives are completely decomposed. At the same time, the 430L stainless steel and ScSZ materials can adapt to high temperatures, and a small rejection phenomenon will occur. They can be artificially polished and repaired to improve the structural stability. Step 6: Cut the prepared functional layer membrane strips into the same size as the metal support porous stainless steel plate, and polish the double sides of the functional layer membrane strips with 400-grit sandpaper to increase the roughness so that the contact surfaces can adhere better; overlap the new membrane strips in the order of porous 430L stainless steel substrate support layer, porous 430L stainless steel-ScSZ composite layer, ScSZ electrolyte layer, GDC barrier layer and porous SSZ layer, and press them together with a hot press to obtain a battery skeleton, put the battery skeleton into the sintering furnace (1), introduce a mixed gas of 5% H2 and 95% N2 as a protective gas, and sinter at a high temperature of 1350°C. During the sintering process, the gas is circulated internally through the exhaust mechanism (2) and the driving mechanism (6), so that the battery skeleton is heated evenly and the quality of the battery skeleton is improved; after the sintering is completed, the metal support of the solid oxide fuel cell can be obtained.