Preparation method of non-adhesion low-porosity nano-silver sintered sample
Through the combined technology of two-stage sintering and sintering auxiliary tooling, the problems of difficult separation of nano-silver sintered samples from the base and high porosity are solved, the preparation of high-density, continuous and intact nano-silver sintered samples is achieved, and the mechanical property testing is improved. accuracy.
Patent Information
- Application Number
- CN202411002444.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-01
AI Technical Summary
Existing nano-silver sintered samples are difficult to separate from the base or matrix, and the porosity after sintering is high, which affects the accuracy and density of mechanical property testing.
Using a two-stage sintering method and sintering auxiliary tooling, a dispensing machine is used to dispense nano-silver glue on the dispensing tooling of non-adhesive materials, and the dispensing position and air pressure are controlled through vacuum adsorption and preset programs. The first stage After sintering, it is demoulded and soaked to reduce adhesion, and then the second stage of sintering is performed in the sintering auxiliary tooling to reduce porosity.
The sintered nano-silver sample is continuously intact and easy to demould, and the porosity is significantly reduced, the curling phenomenon is avoided, and the test reliability of mechanical properties is improved.
Smart Images

Figure CN118730665A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of integrated circuit packaging, and in particular relates to a method for preparing a non-adhesive low-porosity nano-silver sintered sample. Background Art
[0002] In today's electronic and information age, microelectronics technology plays a decisive role in the development of the electronic information industry and other high-tech industries, and its core is the integrated circuit. One of the key technologies in the manufacture of integrated circuit devices is the packaging and interconnection of integrated circuits, which mainly completes three tasks: electrical connection, mechanical connection, and thermal connection.
[0003] The development trend of semiconductor devices is that the structure and function are becoming more and more complex, while the device size is getting smaller and smaller, resulting in an increasing power density of packaged devices. This trend pushes current power packaging and thermal management technologies to the limit. Especially for high-power semiconductor devices, such as ultra-high-speed computer chips and high-power LEDs, heat dissipation becomes a key issue affecting the performance of electronic packaging systems, because the accumulation of heat will seriously reduce the reliability and service performance of the device.
[0004] At present, soft solder is the most commonly used multi-level packaging interconnection material in the electronics industry. However, its relatively low thermal conductivity makes it unable to meet the heat dissipation requirements of high-power density packaging systems. Nano silver paste is a very promising electronic packaging interconnection material. Metallic silver has a very high thermal conductivity (410W / m·K) and can meet the heat dissipation requirements of high-power density systems. At the same time, due to the nano-size effect, the melting point and sintering temperature of nano silver particles are much lower than the melting point and sintering temperature of bulk silver. The surface-melted nanoparticles are easily sintered together by the action of liquid phase capillary forces, and finally form a sintered body with a melting point close to that of bulk silver. Therefore, according to this principle, it is generally believed that nano silver paste sintered joints can be obtained at lower processing temperatures and work at higher temperatures, and the remelting phenomenon can be avoided during the packaging interconnection process. This characteristic is very suitable for multi-level packaging.
[0005] Although nano silver paste is widely used at present, it is difficult to test its mechanical properties after sintering. First, due to its characteristics, it will adhere to the base or substrate after sintering, and it is difficult to separate it during mechanical experiments, resulting in inaccurate test results. Second, at the existing sintering temperature, its internal structure is not tight and the porosity is high. In order to obtain nano silver sintered samples with a tighter structure, its sintering method needs to be improved. Summary of the invention
[0006] In order to solve the above-mentioned problems in the prior art, namely, the problem that the nanosilver sintered sample is difficult to separate from the base or substrate and the porosity is high, the present invention provides a method for preparing a non-adhesive low-porosity nanosilver sintered sample, comprising the following process steps:
[0007] Using a dispensing machine to dispense nano silver glue on a dispensing area of a dispensing tool, to obtain a dispensing tool that has completed dispensing; the dispensing area is composed of a non-adhesive material;
[0008] The glue dispensing tooling after glue dispensing is placed in a sintering furnace for the first stage of sintering to obtain a glue dispensing tooling with a nano-silver sample of a fixed shape, and the nano-silver sample of the fixed shape is demoulded;
[0009] The demoulded nanosilver sample is placed between the upper and lower pressing blocks of the sintering auxiliary tooling, and then placed in a sintering furnace for the second stage of sintering to obtain a non-adhesive and low-porosity nanosilver sintered sample.
[0010] Specifically, the dispensing machine is used to dispense the nano silver glue on the dispensing area of the dispensing tool to obtain the dispensing tool for completing the dispensing, including the following process steps:
[0011] Fixing the dispensing tool on the vacuum adsorption table of the dispensing machine, and starting the dispensing machine to adsorb the dispensing tool;
[0012] Fill the nano silver glue to be sintered on the glue dispensing machine;
[0013] The dispensing position is positioned, and a preset program is used to control the dispensing speed, the position of the dispensing machine glue head and the dispensing air pressure to control the thickness of the nanosilver sample, and the nanosilver glue is evenly applied to the dispensing area of the dispensing tool to obtain a dispensing tool that completes the dispensing.
[0014] Specifically, positioning the dispensing position includes the following process steps:
[0015] An identification area is set in the dispensing tool, and the identification area includes a positioning material, and the positioning material is a non-transparent material with a flatness not exceeding a preset value;
[0016] The position on the identification area is identified by the probe, and the glue dispensing position on the glue dispensing area is obtained according to the projection of the glue dispensing area on the identification area.
[0017] Specifically, the positioning material is aluminum.
[0018] Specifically, the dispensing speed is controlled to 6mm / s, the height of the dispensing machine glue head is controlled to 6mm, the dispensing air pressure is controlled to 40KPa, and the dispensing is performed according to the I-shape, wherein the I-shape head is 30mm long and 10mm wide, and the I-shape middle connecting rod is 80mm long and 10mm wide.
[0019] Specifically, the non-adhesion material is polyimide.
[0020] Specifically, the glue dispensing tooling after glue dispensing is placed in a sintering furnace for the first stage of sintering, which includes the following process steps:
[0021] Put the glue dispensing tooling into the sintering furnace. The initial temperature of the first stage of sintering is room temperature. Preheat for 1 hour within the temperature range of 150℃±5℃ and keep warm for 2 hours within the temperature range of 250℃±5℃.
[0022] Specifically, demoulding the nanosilver sample with a fixed shape includes the following process steps:
[0023] The non-adhesion material with the fixed-shape nanosilver sample is removed from the dispensing tool, and the non-adhesion material with the fixed-shape nanosilver sample is immersed in ethanol. After the immersion lasts for a preset time, the non-adhesion material with the fixed-shape nanosilver sample is taken out from the ethanol, and the nanosilver sample is removed from the non-adhesion material.
[0024] Specifically, the demoulded nanosilver sample is placed between the upper and lower pressing blocks of the sintering auxiliary tooling, and then placed in a sintering furnace for the second stage of sintering, which includes the following process steps:
[0025] The demoulded nanosilver sample is placed between the upper and lower pressing blocks of the sintering auxiliary tooling and placed in the sintering furnace. The initial temperature of the second stage of sintering is room temperature. It is preheated for 1 hour within the temperature range of 150℃±5℃ and kept warm for 2 hours within the temperature range of 400℃±5℃.
[0026] Specifically, the auxiliary tooling includes two stainless steel counterweight blocks, and the two stainless steel counterweight blocks are upper and lower pressure blocks respectively.
[0027] The beneficial effects of the present invention include at least:
[0028] (1) The use of new dispensing tooling materials and designs ensures that the sintered nanosilver samples are continuous and intact and easy to demold.
[0029] (2) A two-stage sintering method is adopted, and a new sintering auxiliary tooling is added, so that the porosity of the nanosilver sample is low after sintering, and the nanosilver sample has no curling. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments made with reference to the following drawings:
[0031] Figure 1 This is a flow chart of a method for preparing a non-adhesive low-porosity nanosilver sintered sample provided by an embodiment of the present invention;
[0032] Figure 2 is a dispensing flow chart provided by an embodiment of the present invention;
[0033] Figure 3Schematic diagram of glue dispensing tooling provided by an embodiment of the present invention;
[0034] Figure 4 It is a schematic diagram of the steps of the glue dispensing sintering process method provided by an embodiment of the present invention;
[0035] Figure 5 It is a surface morphology of nanosilver sintered by the existing process method;
[0036] Figure 6 The figure is a surface morphology of nanosilver sintered by the process method provided by the embodiment of the present invention. DETAILED DESCRIPTION
[0037] The present application will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It is also necessary to explain that, for ease of description, only the parts related to the relevant invention are shown in the accompanying drawings.
[0038] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0039] The present invention provides a method for preparing a non-adhesive low-porosity nanosilver sintered sample. Figure 1 As shown, the process includes process steps S1 to S4, and each step is described in detail as follows:
[0040] Process step S1: Use a dispensing machine to dispense nanosilver glue on the dispensing area of the dispensing tool to obtain a dispensing tool that has completed dispensing; the dispensing area is composed of non-adhesive materials. The dispensing area of the existing dispensing tool is mainly composed of metal materials, but the metal demolding effect is not good. Preferably, the non-adhesive material in this embodiment is polyimide. In the preparation method of the non-adhesive low-porosity nanosilver sintered sample provided in the embodiment of the present invention, polyimide can achieve a better demolding effect for the nanosilver sample obtained by the above preparation method.
[0041] In some specific embodiments of the method for preparing a non-adhesive low-porosity nanosilver sintered sample, as Figure 2 As shown, a dispensing machine is used to dispense nano silver glue on the dispensing area of the dispensing tool to obtain a dispensing tool that has completed dispensing, including the following process steps:
[0042] Process step S11: fix the dispensing tool on the vacuum adsorption table of the dispensing machine, and start the dispensing machine to adsorb the dispensing tool; fill the nano silver glue to be sintered on the dispensing machine; and locate the dispensing position.
[0043] During the dispensing process, the light in the click area of the dispensing tool is strong, making it difficult to accurately see the dispensing position. In order to accurately identify the dispensing position, the dispensing area is projected onto another area that is convenient for identifying the position. In the area that is convenient for identifying the position, accurate dispensing is achieved based on the projection. Therefore, preferably, in some specific embodiments of the present invention, positioning the dispensing position includes the following process steps:
[0044] An identification area is set in the glue dispensing tool, and the identification area includes a positioning material. The positioning material is a non-transparent material with a flatness not exceeding a preset value. Flatness refers to the difference between the surface unevenness and the absolute level, that is, the smaller the flatness, the flatter the surface; the position on the identification area is identified by a probe, and the glue dispensing position on the glue dispensing area is positioned according to the projection of the glue dispensing area on the identification area. Preferably, the positioning material is aluminum. Compared with other non-transparent and relatively flat materials, aluminum has a better positioning effect in the preparation method of the non-adhesive low-porosity nanosilver sintered sample provided in the embodiment of the present invention, which is conducive to uniform glue dispensing. The glue dispensing area and the identification area in the glue dispensing tool are as follows: Figure 3 As shown, the dispensing area and the identification area are adjacent planes with different materials. The above projection can be a proportional projection or a projection after unequal conversion. For example, a projection after reducing the dispensing area is projected on the identification area, so as to achieve positioning and dispensing of a larger dispensing area in a smaller identification area.
[0045] Process step S12: Using a preset program, the thickness of the nanosilver sample is controlled by controlling the dispensing speed, the position of the dispensing machine glue head and the dispensing air pressure, and the nanosilver glue is evenly applied to the dispensing area of the dispensing tool to obtain a dispensing tool for completing the dispensing. Specifically, the dispensing speed is controlled to 6 mm / s, the height of the dispensing machine glue head is controlled to 6 mm, and the dispensing air pressure is controlled to 40 KPa. Figure 4 As shown, glue is dispensed according to the I-shape, wherein the I-shape head is 30mm long and 10mm wide, and the I-shape middle connecting rod is 80mm long and 10mm wide.
[0046] Process step S2: placing the glue dispensing tool after glue dispensing into a sintering furnace for the first stage of sintering to obtain a glue dispensing tool with a fixed shape of the nanosilver sample.
[0047] In some specific embodiments, the glue dispensing tool after glue dispensing is placed in a sintering furnace for the first stage of sintering, which includes the following process steps:
[0048] Put the glue dispensing tooling into the sintering furnace. The initial temperature of the first stage of sintering is room temperature. Preheat for 1 hour within the temperature range of 150℃±5℃ and keep warm for 2 hours within the temperature range of 250℃±5℃.
[0049] Process step S3: demolding the nanosilver sample with a fixed shape.
[0050] In some specific embodiments of the method for preparing a non-adhesive low-porosity nanosilver sintered sample, demolding the nanosilver sample with a fixed shape includes the following process steps:
[0051] The non-adhesive material with the fixed-shape nanosilver sample is removed from the dispensing tool, and the non-adhesive material with the fixed-shape nanosilver sample is soaked in ethanol. After soaking for a preset time, the non-adhesive material with the fixed-shape nanosilver sample is taken out from the ethanol, and the nanosilver sample is removed from the non-adhesive material. Preferably, the non-adhesive material is polyimide. Compared with the use of metal materials, the nanosilver sample obtained by the method for preparing the non-adhesive low-porosity nanosilver sintered sample provided in the embodiment of the present invention can achieve a better demolding effect. Due to the use of the above-mentioned new dispensing tooling material and design, the sintered nanosilver sample is continuous and intact, and is easy to demold.
[0052] Process step S4: placing the demoulded nanosilver sample between the upper and lower pressing blocks of the sintering auxiliary tooling, and placing it in a sintering furnace for the second stage of sintering to obtain a non-adhesive and low-porosity nanosilver sintered sample.
[0053] In some specific embodiments, the demoulded nanosilver sample is placed between the upper and lower pressing blocks of the sintering auxiliary tooling, and placed in a sintering furnace for the second stage of sintering, which includes the following process steps:
[0054] The demoulded nanosilver sample is placed between the upper and lower pressing blocks of the sintering auxiliary tooling and placed in the sintering furnace. The initial temperature of the second stage of sintering is room temperature. It is preheated for 1 hour within the temperature range of 150℃±5℃ and kept warm for 2 hours within the temperature range of 400℃±5℃.
[0055] In some specific embodiments, Figure 4 As shown, the auxiliary tooling includes two stainless steel counterweights, which are upper and lower pressure blocks, respectively, and each stainless steel counterweight is 2.5 kg. Porosity analysis was performed on two nanosilver samples sintered by the existing method and the process method disclosed in the present invention. The surface morphology of the nanosilver sintered by the existing process method is shown in FIG. Figure 5 As shown, the surface morphology of the nanosilver sintered by the process method provided by the embodiment of the present invention is as follows Figure 6 As shown, Figure 5 and Figure 6 In the figure, bright spots represent pores. Larger and brighter bright spots indicate larger pores, while smaller and darker bright spots indicate smaller pores. Figure 5 and Figure 6It can be seen that the porosity of the nanosilver sample sintered by the process disclosed in the present invention is lower. The embodiment of the present invention adopts a two-stage sintering method and adds a new sintering auxiliary tooling to achieve a low porosity of the nanosilver sample after sintering and no curling of the nanosilver sample.
[0056] In another embodiment of the method for preparing a non-adhesive low-porosity nanosilver sintered sample disclosed in the present invention, the Figure 3 The dispensing tool shown is fixed on the dispensing platform of the MUSASHI 350PC Smart dispensing machine to dispense glue on the I-shaped nano-silver tensile specimen. The specific method is as follows:
[0057] Step 1: Fix the dispensing tool on the vacuum adsorption table of the dispensing machine and start the adsorption function of the dispensing machine;
[0058] Step 2: Fill the nano silver glue to be sintered on the glue dispensing machine;
[0059] Step 3: Position according to the identification position, use the I-shaped dispensing program, the shape after dispensing is I-shaped, set the dispensing speed to 6mm / s, and evenly dispense the nano silver glue on the dispensing area of the dispensing tooling. The dispensing pressure is 40KPa, and the dispensing height is 6mm. Through the above factors, the thickness of the nano silver sample after sintering is controlled to be 5mm. The sample is I-shaped, the head is 30mm long and 10mm wide, and the middle connecting rod is 80mm long and 10mm wide.
[0060] Step 4: When the dispensing process is completed, move the glue head to the next dispensing area. Repeat step 3 until all dispensing areas have been dispensing. According to the above dispensing process, the corresponding dispensing program can be set in the dispensing machine auxiliary operation equipment.
[0061] Step 5: Place the glue dispensing tooling into the sintering furnace for the first stage of sintering. The initial temperature is room temperature, preheat at 150℃±5℃ for 1h, and then keep warm at 250℃±5℃ for 2h.
[0062] Step 6: After the first stage of sintering is completed, the dispensing tool with the fixed-shape nanosilver sample is taken out from the heating furnace. The non-adhesive material with the nanosilver sample is removed from the tool and soaked in alcohol. After 5 minutes, the non-adhesive material is taken out and the nanosilver sample is removed from the non-adhesive material.
[0063] Step 7: Place the demoulded nanosilver sample into the sintering auxiliary tooling, and then place the sintering auxiliary tooling into the sintering furnace for the second stage of sintering. The initial temperature is room temperature, preheat at 150℃±5℃ for 1h, and then keep warm at 400℃±5℃ for 2h. After sintering, a non-adhesive and low-porosity nanosilver sample is obtained.
[0064] The term "comprise" or any other similar term is intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus / device that includes a list of elements includes not only those elements but also other elements not expressly listed, or also includes elements inherent to such process, method, article, or apparatus / device.
[0065] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
Claims
1. A method for preparing a non-adhesive low-porosity nanosilver sintered sample. It is characterized in that The following steps are involved: Using a dispensing machine to dispense nano silver glue on a dispensing area of a dispensing tool, to obtain a dispensing tool that has completed dispensing; the dispensing area is composed of a non-adhesive material; The glue dispensing tool after glue dispensing is placed in a sintering furnace for a first stage of sintering to obtain a glue dispensing tool with a nano-silver sample of a fixed shape; Demolding the nanosilver sample with a fixed shape; The demoulded nanosilver sample is placed between the upper and lower pressing blocks of the sintering auxiliary tooling, and then placed in a sintering furnace for the second stage of sintering to obtain a non-adhesive and low-porosity nanosilver sintered sample.
2. The method for preparing a non-adhesive low-porosity nanosilver sintered sample according to claim 1, It is characterized in that Using a dispensing machine to dispense nano silver glue on the dispensing area of the dispensing tool to obtain a dispensing tool that has completed dispensing, including the following steps: Fixing the dispensing tool on the vacuum adsorption table of the dispensing machine, and starting the dispensing machine to adsorb the dispensing tool; Filling the nano silver glue to be sintered on the glue dispensing machine; The dispensing position is positioned, and the thickness of the nanosilver sample is controlled by controlling the dispensing speed, the position of the dispensing machine glue head and the dispensing air pressure. The nanosilver glue is evenly dotted on the dispensing area of the dispensing tool to obtain a dispensing tool that completes the dispensing.
3. The method for preparing a non-adhesive low-porosity nanosilver sintered sample according to claim 2, It is characterized in that Positioning the dispensing position includes the following steps: An identification area is set in the dispensing tool, and the identification area includes a positioning material, and the positioning material is a non-transparent material with a flatness not exceeding a preset value; The position on the identification area is identified by a probe, and the glue dispensing position on the glue dispensing area is obtained according to the projection of the glue dispensing area on the identification area.
4. The method for preparing a non-adhesive low-porosity nanosilver sintered sample according to claim 3, It is characterized in that The positioning material is aluminum.
5. The method for preparing a non-adhesive low-porosity nanosilver sintered sample according to claim 2, It is characterized in that The thickness of the nanosilver sample is controlled by controlling the dispensing speed, the position of the dispensing machine glue head and the dispensing air pressure. The method is as follows: The dispensing speed is controlled to 6mm / s, the height of the dispensing machine glue head is controlled to 6mm, the dispensing air pressure is controlled to 40KPa, and dispensing is performed in an I-shaped shape, wherein the I-shaped head is 30mm long and 10mm wide, and the I-shaped middle connecting rod is 80mm long and 10mm wide.
6. The method for preparing a non-adhesive low-porosity nanosilver sintered sample according to claim 1, It is characterized in that The non-adhesion material is polyimide.
7. The method for preparing a non-adhesive low-porosity nanosilver sintered sample according to claim 1, It is characterized in that The glue dispensing tooling after glue dispensing is placed in a sintering furnace for the first stage of sintering, including the following steps: Put the glue dispensing tooling into the sintering furnace. The initial temperature of the first stage of sintering is room temperature. Preheat for 1 hour within the temperature range of 150℃±5℃ and keep warm for 2 hours within the temperature range of 250℃±5℃.
8. The method for preparing a non-adhesive low-porosity nanosilver sintered sample according to claim 1, It is characterized in that Demolding the nanosilver sample with a fixed shape includes the following steps: The non-adhesion material with the nano-silver sample of fixed shape is removed from the dispensing tool, and the non-adhesion material with the nano-silver sample of fixed shape is immersed in ethanol. After the immersion lasts for a preset time, the non-adhesion material with the nano-silver sample of fixed shape is taken out from the ethanol, and the nano-silver sample is removed from the non-adhesion material.
9. The method for preparing a non-adhesive low-porosity nanosilver sintered sample according to claim 1, It is characterized in that The demoulded nanosilver sample is placed between the upper and lower pressing blocks of the sintering auxiliary tooling, and placed in a sintering furnace for the second stage of sintering, including the following steps: The demoulded nanosilver sample is placed between the upper and lower pressing blocks of the sintering auxiliary tooling and placed in the sintering furnace. The initial temperature of the second stage of sintering is room temperature. It is preheated for 1 hour within the temperature range of 150℃±5℃ and kept warm for 2 hours within the temperature range of 400℃±5℃.