Method for measuring contents of gold and silver in low-grade copper ore
By adding platinum and thiourea solutions to copper ores, the problem of determining the gold and silver content in low-grade copper ores is solved, the simultaneous detection and accurate determination of gold and silver is achieved, the detection efficiency and accuracy are improved, and the requirements are met meet actual production needs.
Patent Information
- Application Number
- CN202410943411.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology cannot effectively measure the gold and silver content in low-grade copper ores, and the existing methods need to be processed separately. The analysis steps are cumbersome, time-consuming, have poor detection timeliness, and occupy a lot of human resources.
A method including batching, melting, soot blowing, dissolving to volume and measurement is adopted. By adding a platinum standard solution and an appropriate amount of thiourea solution, ICP-OES is used for simultaneous detection of gold and silver to avoid the occurrence of AgCl precipitation and ensure the purity of the elements. Fully dissolved and accurately measured.
It achieves the accurate determination of gold and silver content in low-grade copper ores, improves detection efficiency, enhances the accuracy of detection results, and meets the needs for rapid and simultaneous processing of gold and silver in low-grade copper ores.
Smart Images

Figure CN118731004A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for determining the content of gold and silver in an ore, and in particular to the determination of gold and silver in a copper ore sample. Background Art
[0002] At present, the method commonly used for determining the silver content in copper ore is GB / T 14353.11-2010 "Chemical analysis methods for copper ores, lead ores and zinc ores Part 11 Determination of silver content". After the sample is burned and dissolved in acid, the atomic absorption method is used for determination, and the determination range is 10g / t-500g / t; or refer to GB / T 3884.2-2012 "Chemical analysis methods for copper concentrates Part 2: Determination of gold and silver contents Flame atomic absorption spectrometry and fire assay method" and use flame atomic absorption method or fire assay enrichment + titration method for titration, and the determination range is 10-2500g / t.
[0003] The method commonly used for determining the amount of gold in copper ore is YS / T 53.1-2010 "Chemical analysis methods for copper, lead and zinc ores and tailings Part 1: Determination of gold content - Fire assay enrichment-flame atomic absorption spectrometry", and the gold content is determined by fire assay enrichment + flame atomic absorption spectrometry; or DB15 / T 1462-2018 "Determination of gold content in polymetallic ores - Polyurethane foam adsorption-flame atomic absorption spectrometry" is adopted, and the gold content is determined by polyurethane foam adsorption-flame atomic absorption spectrometry or activated carbon adsorption-flame atomic absorption spectrometry.
[0004] When measuring the silver content in copper ore in the prior art, once the silver content in the copper ore is lower than 10g / t, the method is not applicable. In actual production, the silver content in many copper ores is mostly between 0.5-5g / t, and the measurement method of the prior art cannot meet the needs of actual production.
[0005] In addition, in the existing technical methods for determining the content of gold and silver in copper ore, samples can only be processed separately during the determination of the two elements. The analysis steps are many, the process is long and the operation is cumbersome, resulting in a long determination time (requiring 2-3 days), poor timeliness of analysis and detection, and a large amount of human resources occupied by analysis and detection.
[0006] Therefore, there is an urgent need for a method that can simultaneously detect the gold and silver content in low-grade copper ore. Summary of the invention
[0007] The object of the present invention is to provide a method for simultaneously detecting the gold and silver contents in low-grade copper ore, so as to solve the above-mentioned defects of the prior art.
[0008] In order to achieve the above objectives, the inventors provide the following technical solutions:
[0009] A method for determining the gold and silver content in low-grade copper ore comprises the following steps:
[0010] Ingredients: Weigh the copper ore sample, put it into a clay crucible containing lead tetroxide, starch, silicon dioxide, borax, and sodium carbonate, then add the platinum standard solution and stir evenly;
[0011] Melting: Place the clay crucible into the assay furnace for high temperature melting, pour the melt into the preheated steel film, cool it, and separate the slag to get the lead buckle;
[0012] Ash blowing: Put the lead button into the preheated magnesia ash dish and place it in an electric furnace for ash blowing until all the lead is blown out to obtain gold, silver and platinum particles;
[0013] Dissolve and fix volume: transfer the gold, silver and platinum particles to a porcelain crucible, add concentrated nitric acid and heat on a low-temperature electric hot plate to dissolve the silver, then add a mixed acid of concentrated nitric acid and concentrated hydrochloric acid in a volume ratio of 1:3 to continue dissolving the gold, heat and evaporate until nearly dry and then cool, then add excess concentrated hydrochloric acid and 1-3 mL, 50 g / L thiourea solution and stir to mix, after the precipitate is completely dissolved, transfer the solution together with the washing liquid into a volumetric flask and fix the volume;
[0014] Determination: Use ICP-OES to measure the sample, obtain the ICP-OES intensity value, substitute it into the gold and silver standard curves respectively, and obtain the gold and silver concentrations in the copper ore sample. The gold and silver contents in the copper ore are converted by the formula.
[0015] The difficulty of fire assay gold and silver enrichment treatment in low-grade copper ore lies in the low gold and silver content in low-grade copper ore. The aggregate particles formed in the ash blowing process of fire assay gold enrichment treatment are too small, and the operator cannot obtain the gold and silver aggregate particles in the ash dish.
[0016] The inventor creatively utilized the principle that platinum has similar chemical properties to gold and silver, and was able to effectively enrich the three elements of platinum, gold and silver during fire assay enrichment, and added platinum of appropriate quality during the batching process.
[0017] The inventors further found in the test that it is not suitable to use aqua regia directly to dissolve the gold-silver-platinum composite particles, because after adding aqua regia, a AgCl protective film will quickly form on the surface of the gold-silver-platinum composite particles, which will terminate the reaction and cause the gold and silver to not be fully dissolved. First, HNO3 is added to dissolve the silver, and then 3 parts of hydrochloric acid and 1 part of nitric acid are added to form the aqua regia effect and then dissolve the gold. Although this can improve the solubility of gold and silver, the Cl generated by the addition of concentrated hydrochloric acid - Still with the generated Ag +The reaction generates AgCl precipitate. The presence of AgCl precipitate prevents all silver in the copper ore from being dissolved in the solution. On the other hand, the AgCl precipitate will wrap the gold, which prevents all gold from being dissolved in the solution. This ultimately leads to a low gold and silver content in the test. The inventors found that after adding excess concentrated hydrochloric acid during the dissolution process, the excess Cl - Will react with AgCl to precipitate AgCl+Cl - =[AgCl 2 ] - reacts to form soluble [AgCl 2 ] - or [AgCl 3 ] - The solubility of AgCl precipitate is greatly improved, but the excess chloride ions cannot complex all the AgCl precipitates in the solution to form soluble [AgCl 2 ] - or [AgCl 3 ] - Therefore, even an excess of Cl- cannot completely dissolve the AgCl precipitate, and a small amount of AgCl precipitate still remains in the solution. The inventors found that after adding an excess of hydrochloric acid and then adding an appropriate amount of thiourea solution, thiourea can react with the AgCl precipitate to generate Ag(SN2H4) with better solubility. 3+ , which can completely eliminate the AgCl precipitation in the solution, so this method creatively uses excess Cl - + The method of adding appropriate amount of thiourea can completely eliminate the influence of AgCl precipitation on the accuracy of gold and silver determination and improve the accuracy of test results.
[0018] Furthermore, in the batching step, the mass of the copper ore sample weighed is 10-30 g; the mass of borax is 5-20 g; the mass ratio of copper ore, lead tetroxide, silicon dioxide, and sodium carbonate is 1:(5-10):(0.5-1.5):(1-3), and the mass determination formula of starch is: In the formula,
[0019] m 淀粉 —Mass of starch to be added, g;
[0020] m 试样 —mass of sample, g;
[0021] m Pb3O4 —Mass of lead tetroxide to be added, g;
[0022] S%—Sulfur content percentage in the sample.
[0023] Furthermore, in the batching step, the added platinum standard solution contains 80 to 120 μg of platinum.
[0024] Furthermore, during high-temperature melting, the clay crucible was placed in a gold assay furnace at a temperature of 900°C, heated to 1100°C within 40 minutes, and kept at this temperature for 20 minutes before being taken out of the furnace.
[0025] Furthermore, the mass of the lead buckles separated in the melting step is 30 to 45 g.
[0026] Furthermore, in the soot blowing step, the temperature of the electric furnace is 800-900°C.
[0027] Further, the dissolving and volume setting step is specifically as follows: transferring the gold, silver and platinum particles to a porcelain crucible, adding 2 mL of concentrated nitric acid with a density of 1.42 g / mL to heat and dissolve the silver on a low-temperature electric hot plate, adding 6 mL of concentrated hydrochloric acid with a density of 1.19 g / mL and 2 mL of 1.42 g / mL concentrated nitric acid to continue to dissolve the gold, continuing to heat and evaporate until nearly dry and then cooling, adding 10 mL of concentrated hydrochloric acid with a density of 1.19 g / mL, and then adding 2 mL of 50 g / L thiourea solution, stirring and mixing, after the precipitate is completely dissolved, the solution and the washing solution are all transferred into a 50 mL volumetric flask, deionized water is added to the scale, the volume is set and mixed;
[0028] Furthermore, the method for drawing the gold and silver standard working curves is:
[0029] Prepare 100 μg / mL silver standard stock solution: Pipette 10.00 mL of 1000 ug / mL silver standard stock solution into a 100 mL volumetric flask, add 10 mL of concentrated nitric acid with a density of 1.42 g / mL, and dilute to the mark with deionized water, cool, make up to volume, shake well and set aside;
[0030] Prepare 100 μg / mL gold standard stock solution: Pipette 10.00 mL of 1000 μg / mL gold standard stock solution into a 100 mL volumetric flask, add 20 mL of 1.19 g / mL concentrated hydrochloric acid and dilute to scale with deionized water, cool, make up to volume, shake well and set aside;
[0031] Prepare 10 μg / mL gold standard stock solution: Pipette 10.00 mL of 100 μg / mL gold standard stock solution into a 100 mL volumetric flask, add 20 mL of 1.19 g / mL concentrated hydrochloric acid and dilute to scale with deionized water, cool, make up to volume, shake well and set aside;
[0032] Prepare gold and silver mixed standard solution: pipette 0mL, 1.00mL, 2.00mL, 5.00mL, 10.00mL, 15.00mL of 10μg / mL gold standard stock solution and 0mL, 0.50mL, 1.00mL, 2.00mL, 3.00mL, 5.00mL of 100μg / mL silver standard stock solution respectively, add 20mL of concentrated hydrochloric acid with a density of 1.19g / mL and 4mL of 50g / L thiourea solution into a 100mL volumetric flask, add deionized water to dilute to the scale, cool, make up to volume, shake well and set aside;
[0033] The gold and silver standard working curves are drawn with the gold and silver concentrations as the horizontal axis and the intensity value of the gold-silver mixed working standard solution measured by ICP-OES as the vertical axis.
[0034] Furthermore, the measurement wavelength of gold is 242.8 nm; the measurement wavelength of silver is 328.1 nm.
[0035] Furthermore, in the determination step, the gold and silver concentrations in the copper ore sample are obtained and the gold and silver content is calculated according to the following formula:
[0036]
[0037] Where W (Au) —Gold content, g / t
[0038] W (Ag) —Silver content, g / t
[0039] m—sample mass, g
[0040] C Au —Concentration of the sample solution found from the gold standard curve, μg / mL
[0041] C Ag —Concentration of the sample solution found from the silver standard curve, μg / mL
[0042] V—fixed volume of solution, mL
[0043] Compared with the prior art, the present invention has the following advantages and effects:
[0044] (1) A method for determining the gold and silver contents in low-grade copper ores with gold contents of 0.05-0.5 g / t and silver contents of 0.5-10 g / t was established. The accuracy was verified by the spike recovery rate, which was between 90.0% and 95.1%, meeting the accuracy requirements of the spike recovery rate. This method achieved simultaneous and rapid processing of gold and silver enrichment and determination in low-grade copper ores, greatly improving the detection efficiency.
[0045] (2) Based on the principle that platinum has similar chemical properties to gold and silver, the fire assay can effectively enrich platinum, gold and silver at the same time. In the assay analysis process, platinum of appropriate quality is added to enrich the gold, silver and platinum particles, thereby increasing the volume of the particles and facilitating the artificial acquisition of the particles for subsequent instrumental detection and analysis.
[0046] (3) The obtained gold-silver-platinum composite particles are firstly dissolved in nitric acid, and then a mixed acid of concentrated nitric acid and concentrated hydrochloric acid with a volume ratio of 1:3 is added to dissolve gold, and then excess hydrochloric acid and an appropriate amount of thiourea are added to avoid the generation of AgCl precipitation, so that gold and silver are fully dissolved in the solution, which not only utilizes the high solubility of concentrated nitric acid and concentrated hydrochloric acid for gold and silver, but also the excess hydrochloric acid + an appropriate amount of thiourea avoids the generation of Cl - The addition of leads to the formation of AgCl precipitation, which reduces the accuracy of gold and silver detection results. By utilizing the characteristics of ICP-OES that can rapidly detect multiple elements at the same time, rapid detection of gold and silver can be achieved, which can well achieve the project goals. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Attached Figure 1 The gold standard working curve is drawn;
[0048] Attached Figure 2 This is a graph of the silver standard working curve. Specific embodiments
[0049] Example 1
[0050] The internal No. 1 copper ore sample was assayed.
[0051] Ingredients: Weigh 30g of the internal No. 1 copper ore sample, put it into a clay crucible containing 150g of lead tetroxide, 5g of starch, 15g of silicon dioxide, 10g of borax, and 30g of sodium carbonate, and then add 1mL of 100mg / L platinum standard solution, and stir evenly. At the same time, take three cups of the copper ore sample and add 1mL of 10 ug / mL gold standard solution and 4mL of 10 ug / mL silver standard solution according to the above ingredient method, and calculate the spike recovery rate.
[0052] Melting: Place the clay crucible into a gold assay furnace at 900°C, heat it to 1100°C in 40 minutes, keep it warm for 20 minutes, pour the molten material into the preheated iron film, and cool it. The molten metal lead will capture the precious metals in the sample and form a lead buckle after cooling. Other substances in the sample and the flux will produce fusible slag, which will float on the molten lead and separate from the lead buckle. The mass of the smooth lead buckle obtained is 35g.
[0053] Ash blowing: Put the lead button into a magnesia ash dish and place it in an 860℃ electric furnace environment for ash blowing until all the lead is blown out to obtain gold, silver and platinum particles.
[0054] Dissolution: Transfer the gold, silver and platinum particles to a porcelain crucible, add 2 mL of 1.42 g / mL concentrated nitric acid and heat on a low-temperature electric hot plate to dissolve the silver, then add 6 mL of 1.19 g / mL concentrated hydrochloric acid and 2 mL of 1.42 g / mL concentrated nitric acid to continue dissolving the gold, heat and evaporate until nearly dry, remove and cool, add 10 mL of concentrated hydrochloric acid, then add 1 mL of 50 g / L thiourea solution and stir to mix until the precipitate is completely dissolved.
[0055] Make up to volume: Transfer all the solution together with the washing solution into a 50mL volumetric flask, add deionized water to the mark, make up to volume and mix well.
[0056] Determination: Use an inductively coupled plasma emission spectrometer to measure the solution after volume adjustment, and select the wavelength of 242.8nm to measure gold, and the wavelength of 328.1nm to measure silver. Obtain the ICP-OES intensity value of the solution to be tested, and substitute it into the gold and silver working standard curves to obtain the gold and silver concentrations. The same sample is measured three times and the average value is taken. The gold and silver content in the copper ore is calculated according to the following formula:
[0057]
[0058] Where, W(Au)—g / t
[0059] W(Ag)—Silver content, g / t
[0060] m—sample mass, g
[0061] C Au —Concentration of the sample solution found from the gold standard curve, μg / mL
[0062] C Ag —Concentration of the sample solution found from the silver standard curve, μg / mL
[0063] V—fixed volume of solution, mL.
[0064] Example 2
[0065] The internal No. 2 copper ore sample was measured.
[0066] Ingredients: Weigh 30g of copper ore sample, put it into a clay crucible containing 150g of lead tetroxide, 5g of starch, 15g of silicon dioxide, 10g of borax, and 30g of sodium carbonate, then add 1mL of 100 mg / L platinum standard solution and stir evenly. At the same time, take another three cups of the copper ore sample and add 2mL of 10 ug / mL gold standard solution and 5mL of 10 ug / mL silver standard solution according to the above ingredient method, and calculate the spike recovery rate.
[0067] Melting: Place the clay crucible into a gold assay furnace at 900°C, heat it to 1100°C in 40 minutes, keep it warm for 20 minutes, pour the molten material into the preheated iron film, and cool it. The molten metal lead will capture the precious metals in the sample and form lead buckles after cooling. Other substances in the sample and the flux will produce fusible slag, which will float on the molten lead and separate from the lead buckles. The mass of the smooth lead buckles obtained is 38g.
[0068] Ash blowing: Put the lead button into a magnesia ash dish and place it in an 860℃ electric furnace environment for ash blowing until all the lead is blown out to obtain gold, silver and platinum particles.
[0069] Dissolution: Transfer the gold, silver and platinum particles to a porcelain crucible, add 2 mL of 1.42 g / mL concentrated nitric acid and heat on a low-temperature electric hot plate to dissolve the silver, then add 6 mL of 1.19 g / mL concentrated hydrochloric acid and 2 mL of 1.42 g / mL concentrated nitric acid to continue dissolving the gold, heat and evaporate until nearly dry, remove and cool, add 10 mL of concentrated hydrochloric acid, and then add 2 mL of 50 g / L thiourea solution and stir to mix until the precipitate is completely dissolved.
[0070] Make up to volume: Transfer all the solution together with the washing solution into a 50mL volumetric flask, add deionized water to the mark, make up to volume and mix well.
[0071] Determination: Use an inductively coupled plasma emission spectrometer to measure the solution after volume adjustment, and select the wavelength of 242.8nm to measure gold, and the wavelength of 328.1nm to measure silver. Obtain the ICP-OES intensity value of the solution to be tested, and substitute it into the gold and silver working standard curves to obtain the gold and silver concentrations. The same sample is measured three times and the average value is taken. The gold and silver content in the copper ore is calculated according to the following formula:
[0072]
[0073] Where, W(Au)—g / t
[0074] W(Ag)—Silver content, g / t
[0075] m—sample mass, g
[0076] C Au —Concentration of the sample solution found from the gold standard curve, μg / mL
[0077] C Ag —Concentration of the sample solution found from the silver standard curve, μg / mL
[0078] V—fixed volume of solution, mL.
[0079] Example 3
[0080] The determination was carried out on the internal No. 3 copper ore sample.
[0081] Ingredients: Weigh 10g of copper ore sample, put it into a clay crucible containing 150g of lead tetroxide, 5g of starch, 15g of silicon dioxide, 10g of borax, and 30g of sodium carbonate, then add 1mL of 100mg / L platinum standard solution and stir evenly. At the same time, take another three cups of the copper ore sample and add 1mL of 5ug / mL gold standard solution and 1mL of 100ug / mL silver standard solution according to the above ingredient method to calculate the spike recovery rate.
[0082] Melting: Place the clay crucible into a gold assay furnace at 900°C, heat it to 1100°C in 40 minutes, keep it warm for 20 minutes, pour the molten material into the preheated iron film, and cool it. The molten metal lead will capture the precious metals in the sample and form a lead buckle after cooling. Other substances in the sample and the flux will produce fusible slag, which will float on the molten lead and separate from the lead buckle. The mass of the smooth lead buckle obtained is 40g.
[0083] Ash blowing: Put the lead button into a magnesia ash dish and place it in an 860℃ electric furnace environment for ash blowing until all the lead is blown out to obtain gold, silver and platinum particles.
[0084] Dissolution: Transfer the gold, silver and platinum particles to a porcelain crucible, add 2 mL of 1.42 g / mL concentrated nitric acid, heat on a low-temperature electric hot plate to dissolve the silver, then add 6 mL of 1.19 g / mL concentrated hydrochloric acid and 2 mL of 1.42 g / mL concentrated nitric acid to continue dissolving the gold, heat and evaporate until nearly dry, remove and cool, add 10 mL of concentrated hydrochloric acid, then add 3 mL of 50 g / L thiourea solution and stir to mix until the precipitate is completely dissolved.
[0085] Make up to volume: Transfer all the solution together with the washing solution into a 50mL volumetric flask, add deionized water to the mark, make up to volume and mix well.
[0086] Determination: Use inductively coupled plasma emission spectrometer to measure the fixed volume solution, select the wavelength of 242.8nm to measure gold, and the wavelength of 328.1nm to measure silver, obtain the ICP-OES intensity value of the solution to be tested, substitute it into the gold and silver working standard curves, respectively, to obtain the gold and silver concentrations, and measure the same sample three times to take the average value.
[0087]
[0088]
[0089] Where, W(Au)—g / t
[0090] W(Ag)—Silver content, g / t
[0091] m—sample mass, g
[0092] CAu —Concentration of the sample solution found from the gold standard curve, μg / mL
[0093] C Ag —Concentration of the sample solution found from the silver standard curve, μg / mL
[0094] V—fixed volume of solution, mL.
[0095] Example 4
[0096] The purchased copper ore standard sample GBW(E)070073 (the standard value of silver content is 6.1g / t) was measured.
[0097] Ingredients: Weigh 20g of copper ore standard sample, put it into a clay crucible containing 150g of lead tetroxide, 4g of starch, 15g of silicon dioxide, 10g of borax, and 30g of sodium carbonate, then add 1mL of 100 mg / L platinum standard solution and stir evenly. At the same time, take three cups of the copper ore sample and add 1mL of 5 ug / mL gold standard solution according to the above ingredient method to calculate the spike recovery rate.
[0098] Melting: Put the clay crucible into the assay furnace with a temperature of 900℃, heat it to 1100℃ in 40 minutes, keep it warm for 20 minutes, pour the molten material into the preheated iron film, and cool it. After cooling, the molten metal lead captures the precious metals in the sample and forms a lead buckle after cooling. Other substances in the sample and the flux produce fusible slag, which floats on the molten lead and separates from the lead buckle. The mass of the obtained smooth lead buckle is 37g.
[0099] Ash blowing: Put the lead button into a magnesia ash dish and place it in an 860℃ electric furnace environment for ash blowing until all the lead is blown out to obtain gold, silver and platinum particles.
[0100] Dissolution: Transfer the gold, silver and platinum particles to a porcelain crucible, add 2 mL of 1.42 g / mL concentrated nitric acid, heat on a low-temperature electric hot plate to dissolve the silver, then add 6 mL of 1.19 g / mL concentrated hydrochloric acid and 2 mL of 1.42 g / mL concentrated nitric acid to continue dissolving the gold, heat and evaporate until nearly dry, remove and cool, add 10 mL of concentrated hydrochloric acid, then add 2 mL of 50 g / L thiourea solution and stir to mix until the precipitate is completely dissolved.
[0101] Make up to volume: Transfer all the solution together with the washing solution into a 50mL volumetric flask, add deionized water to the mark, make up to volume and mix well.
[0102] Determination: Use an inductively coupled plasma emission spectrometer to measure the solution after volume adjustment, and select the wavelength of 242.8nm to measure gold, and the wavelength of 328.1nm to measure silver. Obtain the ICP-OES intensity value of the solution to be tested, and substitute it into the gold and silver working standard curves to obtain the gold and silver concentrations. The same sample is measured three times and the average value is taken. The gold and silver content in the copper ore is calculated according to the following formula:
[0103]
[0104] Where, W(Au)—g / t
[0105] W(Ag)—Silver content, g / t
[0106] m—sample mass, g
[0107] C Au —Concentration of the sample solution found from the gold standard curve, μg / mL
[0108] C Ag —Concentration of the sample solution found from the silver standard curve, μg / mL
[0109] V—fixed volume of solution, mL
[0110] Comparative Example 1
[0111] The difference between Comparative Example 1 and Example 3 is only the dissolution step. The dissolution step of Comparative Example 1 is: transfer the gold, silver and platinum particles into a porcelain crucible, add 2 mL of 1.42 g / mL concentrated nitric acid to heat and dissolve the silver on a low-temperature electric hot plate, add 6 mL of 1.19 g / mL concentrated hydrochloric acid and 2 mL of 1.42 g / mL concentrated nitric acid to continue to dissolve the gold, heat and evaporate to nearly dry, remove and cool, add 10 mL of concentrated hydrochloric acid and stir to mix.
[0112] Comparative Example 2
[0113] The difference between Comparative Example 1 and Example 3 is only the dissolution step. The dissolution step of Comparative Example 2 is: transfer the gold, silver and platinum particles to a porcelain crucible, add 2 mL of 1.42 g / mL concentrated nitric acid to heat and dissolve the silver on a low-temperature electric hot plate, add 6 mL of 1.19 g / mL concentrated hydrochloric acid and 2 mL of 1.42 g / mL concentrated nitric acid to continue to dissolve the gold, heat and evaporate until nearly dry, remove and cool, add a sufficient amount of thiourea solution and stir and mix until the precipitate is completely dissolved. When the precipitate is completely dissolved, 10 mL of 50 g / L thiourea solution is added.
[0114] The standard curve preparation method used in the above Examples 1-4 and Comparative Examples 1-2 is:
[0115] Prepare 100 μg / mL silver standard stock solution: Pipette 10.00 mL of 1000 ug / mL silver standard stock solution into a 100 mL volumetric flask, add 10 mL of concentrated nitric acid with a density of 1.42 g / mL, and dilute to the mark with deionized water, cool, make up to volume, shake well and set aside;
[0116] Prepare 100 μg / mL gold standard stock solution: Pipette 10.00 mL of 1000 μg / mL gold standard stock solution into a 100 mL volumetric flask, add 20 mL of 1.19 g / mL concentrated hydrochloric acid and dilute to scale with deionized water, cool, make up to volume, shake well and set aside;
[0117] Prepare 10 μg / mL gold standard stock solution: Pipette 10.00 mL of 100 μg / mL gold standard stock solution into a 100 mL volumetric flask, add 20 mL of 1.19 g / mL concentrated hydrochloric acid and dilute to scale with deionized water, cool, make up to volume, shake well and set aside;
[0118] Prepare gold and silver mixed standard solution: pipette 0mL, 1.00mL, 2.00mL, 5.00mL, 10.00mL, 15.00mL of 10μg / mL gold standard stock solution and 0mL, 0.50mL, 1.00mL, 2.00mL, 3.00mL, 5.00mL of 100μg / mL silver standard stock solution respectively, add 20mL of concentrated hydrochloric acid with a density of 1.19g / mL and 4mL of 50g / L thiourea solution into a 100mL volumetric flask, add deionized water to dilute to the scale, cool, make up to volume, shake well and set aside;
[0119] The standard working curves of gold and silver content are drawn with the gold and silver concentrations as the horizontal axis and the strength value of the gold-silver mixed standard working solution measured by ICP-OES as the vertical axis.
[0120] Measurement results
[0121] Table 1 shows the concentration values obtained by substituting the intensity values of the copper ore samples of Examples 1-4 and Comparative Examples 1-2 measured by inductively coupled plasma emission spectrometer into the standard curve, and the copper ore content calculated by substituting into the formula.
[0122] Table 1 Gold and silver content values in copper ore samples measured in Examples 1-4 and Comparative Examples 1-2
[0123]
[0124]
[0125] Accuracy Verification:
[0126] In addition, according to the formulation method of Examples 1-4 and Comparative Examples 1-2, gold and silver standard solutions were added, and the molten ash was blown to dissolve and then the volume was determined. The fixed solution was measured using an inductively coupled plasma emission spectrometer, and gold was measured at a wavelength of 242.8 nm and silver was measured at a wavelength of 328.1 nm. The average spiked recovery rate was investigated, and the same sample was measured three times to take the average value. The analysis results are listed in Table 2.
[0127]
[0128]
[0129] Attached Figure 1-2 The gold-silver standard curves show that in the range of 0μg / mL to 1.5μg / mL, the gold concentration has a good linear relationship with the instrument signal intensity, and in the range of 0μg / mL to 5.0μg / mL, the silver concentration has a good linear relationship with the instrument signal intensity, and the correlation coefficients of the fitting curves are all above 0.9995.
[0130] The gold and silver spiked recovery rates of Examples 1-3 are between 90.0% and 95%; the silver content of the purchased copper ore standard sample GBW(E)070073 (the standard value of the silver content of the copper ore standard sample is 6.1 g / t) measured in Example 4 is 5.8 g / t, the direct recovery rate of silver is 95.1%, and the spiked recovery rate of gold is 91.4%. The high recovery rates of Examples 1-4 prove the reliability and accuracy of the method for determining the gold and silver content of low-grade copper ore in this application.
[0131] It can be seen from Example 4 and Comparative Example 1 that in Comparative Example 1, only excessive hydrochloric acid solution is added without adding thiourea, and the measured gold and silver contents are low, and the gold and silver spike recovery rates are lower than those in Example 4. This is because although excessive concentrated hydrochloric acid is added during the dissolution process, the excessive Cl - It will react with the AgCl precipitate to form a soluble complex to dissolve the AgCl precipitate, but only the excess Cl - The AgCl precipitate still cannot be completely dissolved, and a small amount of AgCl precipitate still remains in the solution. The presence of AgCl precipitate leads to low gold and silver detection results and low spike recovery rate. After adding thiourea solution, thiourea can react with AgCl precipitate to generate Ag(SN2H4) with better solubility. 3+ The added thiourea will completely dissolve the AgCl precipitate that has not been completely dissolved by the excess Cl-, thereby improving the accuracy of the gold and silver content detection results in the copper ore.
[0132] It can be seen from Example 4 and Comparative Example 2 that if no excess Cl is added -Instead of dissolving part of the AgCl precipitate first, thiourea is directly added to completely dissolve the AgCl precipitate. Although the AgCl precipitate is eliminated, a large amount of thiourea needs to be added to dissolve the AgCl precipitate. Too much thiourea in the determination solution will affect the signal strength of the inductively coupled plasma emission spectrometer, resulting in a low signal strength, which ultimately leads to low gold and silver content and spike recovery in the detected copper ore. Therefore, only by adding an excess of hydrochloric acid + an appropriate amount of thiourea can the AgCl precipitate be dissolved without affecting the signal strength of the inductively coupled plasma emission spectrometer, thereby improving the accuracy of the determination of the gold and silver content of low-grade copper ore.
[0133] In summary, the determination method provided in the present application can accurately and quickly determine the gold and silver content in low-grade copper ore.
Claims
1. A method for determining the gold and silver content in low-grade copper ore, characterized in that: The following steps are involved: Ingredients: Weigh the copper ore sample, put it into a clay crucible containing lead tetroxide, starch, silicon dioxide, borax, and sodium carbonate, then add the platinum standard solution and stir evenly; Melting: Place the clay crucible into the assay furnace for high temperature melting, pour the melt into the preheated steel film, cool it, and separate the slag to get the lead buckle; Ash blowing: Put the lead button into the preheated magnesia ash dish and place it in an electric furnace for ash blowing until all the lead is blown out to obtain gold, silver and platinum particles; Dissolve and fix volume: transfer the gold, silver and platinum particles to a porcelain crucible, add concentrated nitric acid and heat on a low-temperature electric hot plate to dissolve the silver, then add a mixed acid of concentrated nitric acid and concentrated hydrochloric acid in a volume ratio of 1:3 to continue dissolving the gold, heat and evaporate until nearly dry and then cool, then add excess concentrated hydrochloric acid and 1-3mL50 g / L thiourea solution and stir to mix, after the precipitate is completely dissolved, transfer the solution together with the washing liquid into a volumetric flask and fix the volume; Determination: Use ICP-OES to measure the sample, obtain the ICP-OES intensity value, substitute it into the standard curve of gold and silver respectively, get the gold and silver concentration in the copper ore sample, and convert it into the gold and silver content in the copper ore through the formula.
2. The method for determining the gold and silver content in low-grade copper ore according to claim 2, characterized in that: In the batching step, the mass of the copper ore sample weighed is 10-30 g; the mass of borax is 5-20 g; the mass ratio of copper ore, lead tetroxide, silicon dioxide and sodium carbonate is 1:(5-10):(0.5-1.5):(1-3); The formula for determining the quality of starch is: In the formula, m 淀粉 —Mass of starch to be added, g; m 试样 —mass of sample, g; m Pb3O4 —Mass of lead tetroxide added, g; S—Sulfur content percentage in the sample.
3. The method for determining the gold and silver content in low-grade copper ore according to claim 2, characterized in that: In the batching step, the added platinum standard solution contains 80-120 μg of platinum.
4. The method for determining the gold and silver content in low-grade copper ore according to any one of claims 1 to 3, characterized in that: The high temperature melting is to put the clay crucible into a gold assay furnace with a furnace temperature of 900° C., raise the temperature to 1100° C. within 40 minutes, keep the temperature for 20 minutes and then take it out of the furnace.
5. The method for determining the gold and silver content in low-grade copper ore according to any one of claims 1 to 3, characterized in that: The mass of the lead buttons separated in the melting step is 30 to 45 g.
6. The method for determining the gold and silver content in low-grade copper ore according to any one of claims 1 to 3, characterized in that: The temperature of the electric furnace in the soot blowing step is 800-900°C.
7. The method for determining the gold and silver content in low-grade copper ore according to claim 4, characterized in that: The dissolving and volume setting step is specifically as follows: transferring the gold, silver and platinum particles into a porcelain crucible, adding 2 mL of concentrated nitric acid with a density of 1.42 g / mL, heating on a low-temperature electric hot plate to dissolve the silver, adding 6 mL of concentrated hydrochloric acid with a density of 1.19 g / mL and 2 mL of concentrated nitric acid with a density of 1.42 g / mL to continue to dissolve the gold, continuing to heat and evaporate until nearly dry and then cooling, adding 10 mL of concentrated hydrochloric acid with a density of 1.19 g / mL, and then adding 2 mL of 50 g / L thiourea solution, stirring and mixing to completely dissolve the precipitate, and then transferring the solution together with the washing solution into a 50 mL volumetric flask, adding deionized water to the scale, setting the volume and mixing.
8. The method for determining the gold and silver content in low-grade copper ore according to any one of claims 1 to 3, characterized in that: The method for drawing the gold and silver standard working curves is: Prepare 100 μg / mL silver standard stock solution: Pipette 10.00 mL of 1000 ug / mL silver standard stock solution into a 100 mL volumetric flask, add 10 mL of concentrated nitric acid with a density of 1.42 g / mL, and dilute to the mark with deionized water, cool, make up to volume, shake well and set aside; Prepare 100 μg / mL gold standard stock solution: Pipette 10.00 mL of 1000 μg / mL gold standard stock solution into a 100 mL volumetric flask, add 20 mL of 1.19 g / mL concentrated hydrochloric acid and dilute to scale with deionized water, cool, make up to volume, shake well and set aside; Prepare 10 μg / mL gold standard stock solution: Pipette 10.00 mL of 100 μg / mL gold standard stock solution into a 100 mL volumetric flask, add 20 mL of 1.19 g / mL concentrated hydrochloric acid and dilute to scale with deionized water, cool, make up to volume, shake well and set aside; Prepare gold and silver mixed standard solution: pipette 0mL, 1.00mL, 2.00mL, 5.00mL, 10.00mL, 15.00mL of 10μg / mL gold standard stock solution and 0mL, 0.50mL, 1.00mL, 2.00mL, 3.00mL, 5.00mL of 100μg / mL silver standard stock solution respectively, add 20mL of concentrated hydrochloric acid with a density of 1.19g / mL and 4mL of thiourea solution with a density of 50g / L into a 100mL volumetric flask, add deionized water to dilute to the scale, cool, make up to volume, shake well for later use; The standard working curves of gold and silver content are drawn with the gold and silver concentrations as the horizontal axis and the strength value of the gold-silver mixed standard working solution measured by ICP-OES as the vertical axis.
9. The method for determining the gold and silver content in low-grade copper ore according to claim 1, characterized in that: The measurement wavelength for gold is 242.8nm and the measurement wavelength for silver is 328.1nm.
10. The method for determining the gold and silver content in low-grade copper ore according to claim 1, characterized in that: In the determination step, the gold and silver concentrations in the copper ore sample are obtained by calculating the gold and silver content according to the following formula: Where W (Au) —Gold content, g / t W (Ag) —Silver content, g / t m—sample mass, g C Au —Concentration of the sample solution found from the gold standard curve, μg / mL C Ag —Concentration of the sample solution found from the silver standard curve, μg / mL V—fixed volume of solution, mL.