Method for acquiring single-particle valid data of flip-chip bonding circuit

By conducting substrate thinning and single-particle testing on flip-chip soldering process circuit samples, and screening effective data, the shortcomings of the flip-chip soldering process in the evaluation of single particle effects of aerospace integrated circuits in the existing technology have been solved, and more accurate and efficient evaluation has been achieved. Radiation resistance test support.

CN118731641AActive Publication Date: 2024-10-01BEIJING MICROELECTRONICS TECH INST +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410754517.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-01
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

It is difficult to effectively evaluate the single-event effect of the flip-chip soldering process on aerospace integrated circuits using existing technology, resulting in insufficient guidance on radiation-resistant reinforcement.

Method used

By thinning the substrate of the flip-chip soldering process circuit samples, conducting single particle tests, recording and analyzing the data, screening out effective samples, calculating the single particle error cross section and effective LET value of heavy ions, and improving the accuracy and accuracy of the test data. efficiency.

Benefits of technology

It provides accurate single particle test data to support the radiation resistance test evaluation of aerospace integrated circuits using the flip-chip soldering process, improving the effectiveness and efficiency of the test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731641A_ABST
    Figure CN118731641A_ABST
Patent Text Reader

Abstract

The invention relates to a method for acquiring single-particle effective data of a flip-chip bonding circuit. The method comprises the following steps: thinning a test sample substrate; selecting heavy ions for testing; monitoring the temperature of the test circuit; judging data validity; and measuring the thinning thickness and calculating effective data. Compared with a traditional test method, the single-particle test evaluation method can effectively improve the single-particle test efficiency of the flip-chip bonding process circuit. By means of temperature control, multiple verification, error calibration and the like, accuracy and effectiveness of single particle test flip-chip bonding process circuit test data are provided, the blank of a flip-chip bonding circuit single particle evaluation method for aerospace is effectively filled up, and powerful support is provided for radiation resistance reinforcement of flip-chip bonding process aerospace integrated circuits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a single particle effective data acquisition method for a flip-chip circuit, and belongs to the field of single particle effect testing of aerospace integrated circuits. Background Art

[0002] With the full completion and successful operation of the Chinese space station, my country has become one of the world's leading aerospace powers. Faced with major aerospace projects such as deep space exploration and manned lunar landing, various types of high-performance aerospace integrated circuits are urgently needed to meet more complex application requirements. Faced with increasingly complex circuit functions, the flip-chip process has become one of the mainstream packaging technologies for advanced process nodes of 28nm and below. However, due to the particularity of the flip-chip process and the limited ion range of domestic accelerators, the samples required for single-particle testing must be substrate thinned to ensure that the ions can reach the active area of ​​the chip. Therefore, for today's complex aerospace integrated circuits, there is an urgent need for a single-particle test process for evaluating flip-chip process circuits to characterize the single-particle effect characteristics of the target circuit under ion irradiation, and to provide guidance for the anti-radiation reinforcement of flip-chip process aerospace integrated circuits. Summary of the invention

[0003] The technical problem solved by the present invention is: to overcome the deficiencies of the prior art, to provide a single-particle effective data acquisition method for a flip-chip circuit, to improve the validity of single-particle test data of a flip-chip process circuit, and to provide technical support for aerospace integrated circuit radiation resistance test evaluation.

[0004] The technical solution of the present invention is: a method for acquiring single particle effective data of a flip-chip circuit, the method comprising the following steps:

[0005] S1. Thin the substrate of the flip-chip process circuit sample and record the thinning thickness;

[0006] S2. Use heavy ions suitable for flip-chip process circuits to conduct single particle tests on thinned flip-chip process circuit samples to obtain the number of single particle errors of different samples under the same heavy ion irradiation and the number of single particle errors of the same sample under different heavy ion irradiations;

[0007] S3, after the single particle test is completed, the test data is analyzed to determine the validity of the test data. If the test data is valid, the process proceeds to step S4, otherwise, the flip-chip process circuit sample is replaced and steps S1 to S3 are re-executed;

[0008] S4, perform thickness measurement calibration on the flip-chip process circuit samples, and select effective flip-chip process circuit samples from the experimental flip-chip process circuit samples according to the calibration results, and then perform steps S5 and S6 to obtain single-particle valid data corresponding to heavy ions, wherein the single-particle valid data includes effective LETe and single-particle error cross section σm ;

[0009] S5. Calculate the single particle error cross section σ of heavy ions based on the single particle test results of the effective flip chip process circuit sample m ;

[0010] S6, average thickness d of the circuit sample substrate thinned according to the effective flip-chip process r-mean The effective LETe of heavy ions is obtained by simulation using heavy ion LET calculation software.

[0011] Preferably, during the single particle test, the operating temperature of the flip chip process circuit sample is monitored in real time. If the operating temperature of the flip chip process circuit sample is greater than or equal to the temperature alarm threshold, the test is stopped immediately, and the test is continued after the operating temperature of the flip chip process circuit sample returns to between [T1, T2], where [T1, T2] is the rated operating temperature range of the flip chip process circuit.

[0012] Preferably, the thickness l of the flip-chip process circuit sample after thinning satisfies 20 μm<l<40 μm, and the uniformity of the substrate surface meets a preset condition.

[0013] Preferably, the range of the heavy ions selected to be suitable for flip-chip process circuits is greater than 40 μm.

[0014] Preferably, the LET value of the heavy ions selected for flip-chip process circuits covers three energy ranges:

[0015] 0~10MeV·cm 2 / mg, 30~40MeV·cm 2 / mg, 60~100MeV·cm 2 / mg.

[0016] Preferably, the validity criterion of the test data is that if the following two conditions are met at the same time, the test data is considered valid; otherwise, the test data is considered invalid;

[0017] The first condition is that the number of single particle errors of different samples under the same ion irradiation satisfies:

[0018]

[0019] Among them, α i represents the number of single-particle errors in the ith trial;

[0020] n represents the total number of test samples;

[0021] α max Indicates the maximum single-particle error number of the test sample;

[0022] α minIndicates the minimum single particle error number of the test sample;

[0023] ε and τ are constants;

[0024] The second condition is that the number of single particle errors of the same sample under different ion irradiation must satisfy that the number of single particle errors caused by ion irradiation with high LET value is greater than that of ion data with low LET value.

[0025] Preferably, the method for measuring and calibrating the thickness of the flip-chip process circuit sample is: cutting the flip-chip process circuit sample longitudinally along the diagonal line, and the maximum thickness d of the substrate of the flip-chip process circuit sample is r-max and minimum thickness d r-min , calculate the average thickness d of the flip chip process circuit sample substrate thinning r-mean , if d r-max -d r-min Greater than d r-min If the value of the flip-chip process circuit sample is less than 10%, the flip-chip process circuit sample is determined to be an invalid sample; otherwise, the flip-chip process circuit sample is determined to be a valid sample.

[0026] Preferably, the average thickness d of the effective flip chip process circuit sample substrate thinning r-mean =(d r-max +d r-min ) / 2.

[0027] Preferably, the effective LETe is obtained by the following method:

[0028] S6.1. Substitute the surface energy Es of the ions incident on the flip-chip process circuit sample into the heavy ion LET calculation software to obtain the surface range μ of the incident ions;

[0029] S6.2. Subtract the substrate thinning thickness from the surface range μ obtained in S6.1 to obtain the effective range μ-d of the incident ion. r-mean ;

[0030] S6.3. Using the heavy ion LET calculation software, iteratively calculate the effective range to be μ-d r-mean The energy and LET value of the heavy ion corresponding to this time are the effective energy Ee, and the corresponding LET is the effective LETe.

[0031] Preferably, the single particle error cross section σ of the heavy ion is m Obtained by the following method:

[0032] Single-event error cross section = total number of single-event errors / total irradiation dose

[0033] The total number of single-particle errors refers to the total number of single-particle errors generated by the single-particle experiments corresponding to heavy ions;

[0034] The total irradiation dose refers to the total heavy ion irradiation dose in the single particle test corresponding to heavy ions.

[0035] The beneficial effects of the present invention compared with the prior art are:

[0036] (1) The single-particle test result evaluation method for flip-chip process circuits proposed in the present invention provides accurate test data for single-particle effective data through multiple verifications and error calibrations, providing strong support for the evaluation of single-particle effects in aerospace integrated circuits using flip-chip process.

[0037] (2) The present invention clarifies the selection of single particle test and heavy ion selection for flip-chip process circuits, effectively improving the efficiency of single particle testing. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 Schematic diagram of the flow of a method for acquiring single particle valid data of a flip-chip circuit in an embodiment of the present invention. DETAILED DESCRIPTION

[0039] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0040] like Figure 1 As shown, the present invention provides a single particle effective data acquisition method for a flip-chip circuit, the method comprising the following steps:

[0041] S1. Thin the substrate of the flip-chip process circuit sample and record the thinning thickness;

[0042] The specific steps of thinning are:

[0043] (1.1) Remove the thermal layer metal cover on the surface of the circuit sample;

[0044] (1.2) Since the back of the flip-chip process circuit chip faces upward, during the single-particle test, the accelerated ions can only be incident from the back of the chip and pass through the substrate into the active area. However, due to the limited energy and range of heavy ions in domestic accelerators, it is necessary to perform substrate thinning. The thickness of the circuit substrate is reduced from several hundred microns to the target thickness d through a grinding device, ranging from 30μm to 50μm. The distance from the aerospace-grade flip-chip process circuit substrate to the active area is M, and the thinning thickness is K. The actual thickness after thinning is l=MK, and the thickness l of the flip-chip process circuit sample after thinning must satisfy 20μm<l<40μm;

[0045] (1.3) When thinning again, it is necessary to ensure that the uniformity of the substrate surface meets the preset conditions and that the thinning does not cause damage to the circuit. In a specific embodiment of the present invention, the uniformity of the substrate surface meets the following conditions: select a point in the flip-chip process circuit sample after thinning as a base point, set the step length to x, define the points in the four directions of front, back, left, and right with a distance of x from the base point as uniformity measurement points, and the thickness error between these uniformity measurement points and the base point is less than 5%. In this embodiment, the step length is 1um.

[0046] S2. Use heavy ions suitable for flip-chip process circuits to conduct single particle tests on thinned flip-chip process circuit samples to obtain the number of single particle errors of different samples under the same heavy ion irradiation and the number of single particle errors of the same sample under different heavy ion irradiations;

[0047] Due to the special feature of the flip-chip circuit substrate facing upward, the range of heavy ions selected for the flip-chip process circuit is greater than 40μm, and it is necessary to ensure that the ion range provided by the accelerator is greater than 40μm.

[0048] To facilitate subsequent data analysis and on-orbit prediction, the LET values ​​of heavy ions selected for flip-chip process circuits cover three energy ranges:

[0049] 0~10MeV·cm 2 / mg, 30~40MeV·cm 2 / mg, 60~100MeV·cm 2 / mg.

[0050] According to the actual beam output capability of domestic heavy ion accelerators, the domestic heavy ion accelerators available include C, O, F, Al, Si, etc. (LET value is 0~10MeV·cm 2 / mg), Kr (LET value is 30~40MeV·cm 2 / mg) and Xe, Ta, Bi, etc. (LET value is 60~100MeV·cm 2 / mg).

[0051] For single particle testing of flip chip circuits, at least five heavy ions with different LET values ​​are required to accurately characterize the single particle effect characteristics. In order to ensure the effectiveness of ion injection and the effective coverage of single particle error cross sections, the appropriate irradiation ions are selected based on the actual beam output capacity of domestic heavy ion accelerators.

[0052] During the single particle test, the single particle test is carried out in the order of LET value from small to large.

[0053] In order to prevent the flip-chip integrated circuit from short-circuiting or burning out due to continuous heat generation during operation, which may affect the circuit's service life, a heat sink is usually used to dissipate heat and cool the circuit. However, when conducting single-particle tests, the substrate needs to be thinned, which will destroy the structure and the circuit's heat dissipation capacity will become poor. The Institute of Atomic Energy's tandem accelerator needs to be tested in a vacuum tank, and temperature rises become more frequent. Therefore, it is necessary to monitor the temperature of the irradiated circuit to prevent single-particle latching or circuit function abnormalities caused by high temperature and other reasons, and to ensure the accuracy of the test data.

[0054] During the single particle test, a temperature detection device is set to monitor the operating temperature of the flip chip process circuit sample in real time, and a temperature alarm threshold is set. If the operating temperature of the flip chip process circuit sample is greater than or equal to the temperature alarm threshold, the test is stopped immediately, and the test is continued after the operating temperature of the flip chip process circuit sample returns to between [T1, T2]. [T1, T2] is the rated operating temperature range of the flip chip process circuit.

[0055] S3, after the single particle test is completed, the test data is analyzed to determine the validity of the test data. If the test data is valid, the process proceeds to step S4, otherwise, the flip-chip process circuit sample is replaced and steps S1 to S3 are re-executed;

[0056] When the flip-chip process circuit is thinning the substrate, due to limited technology, there will be a certain degree of non-uniformity in the thinned surface. This situation may cause the single-particle test data to be invalid. For example, the single-particle error cross section generated at a high LET value will be lower than the single-particle error cross section at a low LET value. At least three samples are required to carry out single-particle testing. When analyzing the data at the test site, horizontal and vertical comparisons of the test data should be performed. The criterion for the validity of the test data is that the following two conditions are met at the same time, then the test data is considered valid; otherwise, the test data is considered invalid;

[0057] The first condition is that the number of single particle errors of different samples irradiated with the same ion should meet the following requirements:

[0058]

[0059] Among them, α i represents the number of single-particle errors in the ith trial;

[0060] n represents the total number of test samples;

[0061] α max Indicates the maximum single-particle error number of the test sample;

[0062] α min Indicates the minimum single particle error number of the test sample;

[0063] ε and τ are constants; according to actual engineering experience, ε is 1.5 and τ is 5.

[0064] The second condition is: when longitudinally comparing the number of single particle errors of the same sample under different ion irradiation conditions, the number of single particle errors caused by ion irradiation with a high LET value must be greater than that caused by ion data with a low LET value.

[0065] When processing single-particle data, invalid data needs to be marked, and the test should be carried out again under heavy ions of the LET value after replacing the test sample.

[0066] S4, perform thickness measurement calibration on the flip-chip process circuit samples, and select effective flip-chip process circuit samples from the experimental flip-chip process circuit samples according to the calibration results, and then perform steps S5 and S6 to obtain single-particle valid data corresponding to heavy ions, wherein the single-particle valid data includes effective LETe and single-particle error cross section σ m ;

[0067] After completing the single particle test, in order to verify the substrate thinning thickness and the incident surface uniformity of the flip-chip process circuit, it is necessary to measure and calibrate the thinning thickness of the test sample.

[0068] The method for calibrating the thickness of the flip-chip process circuit sample is as follows: the flip-chip process circuit sample is cut longitudinally along the diagonal line, and the maximum substrate thickness d of the flip-chip process circuit sample is r-max and minimum thickness d r-min , calculate the average thickness d of the flip chip process circuit sample substrate thinning r-mean , if d r-max -d r-min Greater than d r-min If the value of the flip-chip process circuit sample is less than 10%, the flip-chip process circuit sample is determined to be an invalid sample; otherwise, the flip-chip process circuit sample is determined to be a valid sample.

[0069] S5. Calculate the single particle error cross section σ of heavy ions based on the single particle test results of the effective flip chip process circuit sample m ;

[0070] The single-particle error cross section σ of the heavy ion m Obtained by the following method:

[0071] Single-event error cross section = total number of single-event errors / total irradiation dose

[0072] The total number of single-particle errors refers to the total number of single-particle errors generated by the single-particle experiments corresponding to heavy ions;

[0073] The total irradiation dose refers to the total heavy ion irradiation dose in the single particle test corresponding to heavy ions.

[0074] S6, average thickness d of the circuit sample substrate thinned according to the effective flip-chip process r-mean , the effective LETe of heavy ions is simulated using heavy ion LET calculation software (such as SRIM, etc.).

[0075] The average thickness d of the circuit sample substrate thinned by the effective flip chip process r-mean =(d r-max +d r-min ) / 2.

[0076] The effective LETe is obtained as follows:

[0077] S6.1. Substitute the surface energy Es of the ions incident on the flip-chip process circuit sample into the heavy ion LET calculation software to obtain the surface range μ of the incident ions;

[0078] S6.2. Subtract the substrate thinning thickness from the surface range μ obtained in S6.1 to obtain the effective range μ-d of the incident ion. r-mean ;

[0079] S6.3. Using the heavy ion LET calculation software, iteratively calculate the effective range to be μ-d r-mean The energy and LET value of the heavy ion corresponding to this time are the effective energy Ee, and the corresponding LET is the effective LETe.

[0080] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the protection scope of the technical solution of the present invention.

Claims

1. A method for acquiring single particle effective data of flip-chip circuits. Features The following steps are involved: S1. Thin the substrate of the flip-chip process circuit sample and record the thinning thickness; S2. Use heavy ions suitable for flip-chip process circuits to conduct single particle tests on thinned flip-chip process circuit samples to obtain the number of single particle errors of different samples under the same heavy ion irradiation and the number of single particle errors of the same sample under different heavy ion irradiations; S3, after the single particle test is completed, the test data is analyzed to determine the validity of the test data. If the test data is valid, the process proceeds to step S4, otherwise, the flip-chip process circuit sample is replaced and steps S1 to S3 are re-executed; S4, perform thickness measurement calibration on the flip-chip process circuit samples, and select effective flip-chip process circuit samples from the experimental flip-chip process circuit samples according to the calibration results, and then perform steps S5 and S6 to obtain single-particle valid data corresponding to heavy ions, wherein the single-particle valid data includes effective LETe and single-particle error cross section σ m ; S5. Calculate the single particle error cross section σ of heavy ions based on the single particle test results of the effective flip chip process circuit sample m ; S6, average thickness d of the circuit sample substrate thinned according to the effective flip-chip process r-mean The effective LETe of heavy ions is obtained by simulation using heavy ion LET calculation software.

2. The single particle effective data acquisition method of a flip chip circuit according to claim 1, It is characterized in that During the single particle test, the operating temperature of the flip chip process circuit sample is monitored in real time. If the operating temperature of the flip chip process circuit sample is greater than or equal to the temperature alarm threshold, the test is stopped immediately and the operating temperature of the flip chip process circuit sample is restored to [T 1 ,T 2 ] and then conduct the test, [T 1 ,T 2 ] is the rated operating temperature range of the flip chip process circuit.

3. The single particle effective data acquisition method of a flip chip circuit according to claim 1, It is characterized in that The thickness l of the flip-chip process circuit sample after thinning satisfies 20 μm<l<40 μm, and the uniformity of the substrate surface meets the preset conditions.

4. The single particle effective data acquisition method of a flip chip circuit according to claim 1, It is characterized in that The range of the heavy ions selected for flip-chip process circuits is greater than 40 μm.

5. The method for acquiring effective single-particle data of a flip-chip circuit according to claim 1, It is characterized in that The LET values ​​of heavy ions selected for flip-chip process circuits cover three energy ranges: 0~10MeV·cm 2 / mg、30~40MeV·cm 2 / mg、60~100MeV·cm 2 / mg。 6. The single particle effective data acquisition method of a flip chip circuit according to claim 1, It is characterized in that The validity of the test data is determined by the following two conditions being met at the same time: if the test data meets the following two conditions at the same time, the test data is considered valid; otherwise, the test data is considered invalid; The first condition is that the number of single particle errors of different samples under the same ion irradiation satisfies: Among them, α i represents the number of single-particle errors in the ith trial; n represents the total number of test samples; α max Indicates the maximum single-particle error number of the test sample; α min Indicates the minimum single particle error number of the test sample; ε and τ are constants; The second condition is that the number of single particle errors of the same sample under different ion irradiation must satisfy that the number of single particle errors caused by ion irradiation with high LET value is greater than that of ion data with low LET value.

7. The method for acquiring effective single-particle data of a flip-chip circuit according to claim 1, It is characterized in that The method for calibrating the thickness of the flip-chip process circuit sample is as follows: the flip-chip process circuit sample is cut longitudinally along the diagonal line, and the maximum substrate thickness d of the flip-chip process circuit sample is r-max and minimum thickness d r-min , calculate the average thickness d of the flip chip process circuit sample substrate thinning r-mean , if d r-max -d r-min Greater than d r-min If the value of the flip-chip process circuit sample is less than 10%, the flip-chip process circuit sample is determined to be an invalid sample; otherwise, the flip-chip process circuit sample is determined to be a valid sample.

8. The method for acquiring effective single-particle data of a flip-chip circuit according to claim 7, It is characterized in that The average thickness d of the circuit sample substrate thinned by the effective flip chip process r-mean =(d r-max +d r-min ) / 2.

9. The single particle effective data acquisition method of a flip chip circuit according to claim 1, It is characterized in that The effective LETe is obtained as follows: S6.

1. Substitute the surface energy Es of the ions incident on the flip-chip process circuit sample into the heavy ion LET calculation software to obtain the surface range μ of the incident ions; S6.

2. Subtract the substrate thinning thickness from the surface range μ obtained in S6.1 to obtain the effective range μ-d of the incident ion. r-mean ; S6.

3. Using the heavy ion LET calculation software, iteratively calculate the effective range to be μ-d r-mean The energy and LET value of the heavy ion corresponding to this time are the effective energy Ee, and the corresponding LET is the effective LETe.

10. The method for acquiring effective single-particle data of a flip-chip circuit according to claim 1, It is characterized in that The single-particle error cross section σ of the heavy ion m Obtained by the following method: Single-event error cross section = total number of single-event errors / total irradiation dose The total number of single-particle errors refers to the total number of single-particle errors generated by the single-particle experiments corresponding to heavy ions; The total irradiation dose refers to the total heavy ion irradiation dose in the single particle test corresponding to heavy ions.

Citation Information

Patent Citations

  • Chip single-event effect detection method and device

    CN106199392A

  • Pre-estimating method for single event effect cross section of anti-irradiation integrated circuit

    CN107345998A

  • Single particle evaluation method for inverted packaging device

    CN113109645A

  • Inverted packaging device single event effect test method, system, equipment and medium

    CN115356610A

  • SiC MOSFET device single event effect test method

    CN117630621A