Polarizing plate and polarizing plate
By adding boron, iodine and zinc elements to the polyvinyl alcohol-based resin film, and processing it through specific processes, a polarizing plate with stable performance at high temperatures is prepared, which solves the problem of the rapid color change of the polyvinyl alcohol-based resin film at high temperatures. problem, achieving improved durability in high-temperature environments such as vehicle-mounted display devices.
Patent Information
- Application Number
- CN202410365913.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
Polarizing plates formed of polyvinyl alcohol-based resin films are prone to polyene in high-temperature environments, resulting in drastic changes in color tone. It is difficult to effectively suppress this change with existing technology, especially in high-temperature environments encountered in automotive applications.
Add an appropriate amount of boron, iodine and zinc elements to the polyvinyl alcohol resin film, and control their content ratio to suppress color tone changes. Through specific processes such as swelling, dyeing, cross-linking and stretching processes, a film that can be used in Polarizer with stable performance at high temperatures.
It effectively suppresses the sharp change in hue of the polarizer at a high temperature of 115°C, improves its durability, and is suitable for use in high-temperature environments such as automotive display devices.
Smart Images

Figure CN118732129A_ABST
Abstract
Description
Technical Field The present invention relates to a polarizing plate and a polarizing film. Background Art In the past, it is known that there is a polaroid formed by a film containing a polyvinyl alcohol resin and iodine (for example, Patent Document 1). The image display device containing the polaroid is also used as an image display device for vehicle use such as a navigation device and a rear-view monitor, and its use is expanding. With the expansion of uses, for the image display device and the polaroid as a part of the image display device, compared with the previous requirements, high durability in a more severe environment (for example, a high temperature environment) is expected. Prior art literature Patent Literature Patent Document 1: Japanese Patent Application Publication No. 2020-71241 Summary of the invention Problems to be solved by the invention When a polarizer formed of a polyvinyl alcohol-based resin film is exposed to a high temperature environment, the polyeneization of polyvinyl alcohol is promoted, so there is a problem of color change of the polarizer due to polyeneization. In particular, in a high temperature environment such as the above-mentioned vehicle-mounted use (e.g., 115°C), the color change due to polyeneization does not proceed slowly, but changes rapidly after a certain period of time, and there is a tendency for the color change to become more significant. However, with regard to conventional polarizers, it is not necessarily possible to fully suppress such color change at high temperatures. The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a polarizing plate capable of suppressing a rapid change in the color tone of the polarizing plate when the polarizing plate is exposed to a high temperature of 115°C. Means for solving problems
[0001] A polarizing plate, wherein a polyvinyl alcohol resin film contains boron, iodine and zinc. The polarizing plate satisfies the following formula (A). 0.001≤[Zn] / ([I]×[B])≤0.025(A) [In formula (A), [Zn] represents the content (mass %) of zinc in the polyvinyl alcohol resin film, [I] represents the content (mass %) of iodine in the polyvinyl alcohol resin film, and [B] represents the content (mass %) of boron in the polyvinyl alcohol resin film.]
[0002] The polarizing plate according to [1], wherein the [Zn] content is 0.01 mass % or more and 1.0 mass % or less.
[0003] The polarizing plate according to [1] or [2], wherein [B] is 3.5 mass % or more and 6.0 mass % or less.
[0004] The polarizing plate according to any one of [1] to [3], wherein [I] is 2.0 mass % or more and 4.0 mass % or less.
[0005] A polarizing plate comprising the polarizer according to any one of [1] to [4], an adhesive layer, and a protective film in this order. Effects of the Invention According to the present invention, it is possible to provide a polarizing plate or the like capable of suppressing a rapid change in the color tone of the polarizing plate when the polarizing plate is exposed to a high temperature of 115°C. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 It is a cross-sectional view showing a polarizing plate according to one embodiment. Description of Reference Numerals 100 polarizing plate, 101 first protective film, 102 polarizing plate, 103 second protective film. DETAILED DESCRIPTION <Polarizing Plate> The polarizing plate according to one embodiment contains a boron element, an iodine element, and a zinc element in a polyvinyl alcohol-based resin film. (Polyvinyl alcohol resin) As the polyvinyl alcohol resin of the polyvinyl alcohol resin film, a resin obtained by saponifying a polyvinyl acetate resin can be used. As the polyvinyl acetate resin, in addition to polyvinyl acetate as a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers copolymerizable therewith can also be exemplified. As other monomers copolymerizable with vinyl acetate, for example, unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, (meth) acrylamides having an ammonium group, etc. can be cited. The saponification degree of the polyvinyl alcohol resin is usually about 85 mol% or more, preferably about 90 mol% or more, and more preferably about 99 mol% or more. The so-called "(meth) acrylic acid" in this specification means at least one selected from acrylic acid and methacrylic acid. The same is true for "(meth) acryloyl". The polyvinyl alcohol-based resin may be modified. For example, polyvinyl formal, polyvinyl acetal, polyvinyl butyral, etc. modified with aldehydes may be used. The average degree of polymerization of the polyvinyl alcohol resin is preferably 100 or more and 10,000 or less, more preferably 1,500 or more and 8,000 or less, and further preferably 2,000 or more and 5,000 or less. The average degree of polymerization of the polyvinyl alcohol resin can be obtained in accordance with JIS K 6726 (1994). If the average degree of polymerization is less than 100, it is difficult to obtain the preferred polarization performance, and if it is greater than 10,000, there is a case where the film processability is poor. The polyvinyl alcohol resin film can be a single film formed by polyvinyl alcohol resin, or a laminated film laminated with a substrate film and a polyvinyl alcohol resin film. In the case of a laminated film, for example, a coating solution containing polyvinyl alcohol resin is applied to at least one side of the substrate film and dried to produce the laminated film. As the substrate film, for example, a thermoplastic resin film can be cited. As the thermoplastic resin film, it is preferably a film composed of an optically transparent thermoplastic resin, and can be a transparent resin film including a polyolefin resin such as a chain polyolefin resin (polypropylene resin, etc.) and a cyclic polyolefin resin (norbornene resin, etc.); a cellulose ester resin such as triacetyl cellulose and diacetyl cellulose; a polyester resin such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; a polycarbonate resin; a (meth) acrylic resin such as a polymethyl methacrylate resin; or a mixture or copolymer thereof. The thickness of the polarizer, i.e., the polyvinyl alcohol-based resin film, can be, for example, 30 μm or less, preferably 25 μm or less, more preferably 20 μm or less, further preferably 15 μm or less, further preferably 14 μm or less, particularly preferably 13 μm or less, and more particularly preferably 12 μm or less. When the thickness of the polarizer is 30 μm or less, there is a tendency to easily suppress light leakage. In addition, thinning the thickness of the polarizer is conducive to the thin filmization of the polarizing plate. The thickness of the polarizer is usually 2 μm or more, for example, 5 μm or more. The polyvinyl alcohol-based resin film is preferably uniaxially stretched. A dichroic dye such as iodine may be adsorbed and oriented in the uniaxially stretched polyvinyl alcohol-based resin film. (Parameter A) The polarizing plate of the present embodiment satisfies the following formula (A) from the viewpoint of suppressing the degree of change in the color tone of the polarizing plate from increasing over time in a state where the polarizing plate is exposed to high temperature. 0.001≤[Zn] / ([I]×[B])≤0.025(A) Here, in formula (A), [Zn] represents the content (mass %) of zinc element in the polyvinyl alcohol resin film, [I] represents the content (mass %) of iodine element in the polyvinyl alcohol resin film, and [B] represents the content (mass %) of boron element in the polyvinyl alcohol resin film. [Zn] / ([I]×[B]) may be 0.002 or more, may be 0.003 or more, may be 0.004 or more, or may be 0.005 or more. [Zn] / ([I]×[B]) may be 0.020 or less, may be 0.018 or less, may be 0.015 or less, may be 0.014 or less, may be 0.013 or less, and may be 0.010 or less. (Mechanism of Action) It is believed that the zinc, iodine, and boron elements in the polarizer are the factors that affect the color change. For example, it is believed that the content of zinc in the polarizer has an influence on the color change of I5 - If the content of zinc in the polarizer is relatively high, it is easy to maintain I5 even after being exposed to a high temperature of 115°C. - . If it is exposed to a high temperature of 115°C, it can also maintain I5 - If the content of iodine in the polarizer is a certain amount, the polyeneization of polyvinyl alcohol will slowly advance, and the polyene chain will be long enough to absorb light in the visible light region, and it is speculated that there is a tendency for a sharp color change to occur. In addition, it is believed that the content of iodine in the polarizer has a certain influence on the initial (i.e., before exposure to a high temperature environment) I5 - If the iodine content is relatively high, it is considered that I5 - The content of I5 is also high, and it is believed that even after exposure to a high temperature of 115°C, I5 - The content is maintained at a certain amount. Therefore, the polyeneization of polyvinyl alcohol is slowly advanced, and the polyene chain becomes longer to be able to absorb light in the visible light region, and it is speculated that a sharp change in color tone is prone to occur. It is believed that the content of boron in the polarizer affects the number of crosslinking points between the polyvinyl alcohol chains. If the content of boron in the polarizer becomes relatively more, the number of crosslinking points between the polyvinyl alcohol chains increases. Therefore, even if the dehydration reaction of polyvinyl alcohol is promoted by exposure to a high temperature of 115°C, the polyene chain will not become longer to be able to absorb light in the visible light region, and it is speculated that it should be easy to suppress the sharp change in color tone. Therefore, when suppressing the sharp change in color tone, it becomes important to contain boron, iodine and zinc elements in a well-balanced manner. The polarizer of this embodiment contains boron, iodine and zinc in a ratio satisfying the above-mentioned parameter A in the polyvinyl alcohol resin film, and thus contains boron, iodine and zinc in a well-balanced manner. Therefore, it is believed that even when exposed to a high temperature of 115°C, a sharp change in color tone can be suppressed. (Boron) The boron content in the polyvinyl alcohol resin film is not particularly limited, and may be 3.5% by mass or more and 6.0% by mass or less. The boron element may crosslink the polyvinyl alcohol resin in the polyvinyl alcohol resin film. From the viewpoint of crosslinking between the polyvinyl alcohol chains, the boron content in the polyvinyl alcohol resin film may be 5.5% by mass or less, 5.0% by mass or less, or 4.7% by mass or less. (Iodine) The content of the iodine element in the polyvinyl alcohol-based resin film is not particularly limited, and may be 2.0% by mass or more and 4.0% by mass or less. Iodine is a dichroic dye, and can exhibit polarization performance by being adsorbed and oriented in the polyvinyl alcohol-based resin film. The content of iodine in the polyvinyl alcohol resin film may be 2.1% by mass or more, 2.2% by mass or more, or 2.3% by mass or more. The content of iodine in the polyvinyl alcohol resin film may be 3.5% by mass or less, 3.2% by mass or less, 3.0% by mass or less, 2.9% by mass or less, or 2.7% by mass or less. (Zinc) The polyvinyl alcohol resin film further includes zinc. The zinc content in the polyvinyl alcohol resin film is not particularly limited, and may be 0.01% by mass or more and 1.0% by mass or less. The zinc content in the polyvinyl alcohol resin film may also be 0.02% by mass or more, 0.03% by mass or more, or 0.05% by mass or more. The zinc content in the polyvinyl alcohol resin film may also be 0.9% by mass or less, 0.7% by mass or less, 0.5% by mass or less, 0.3% by mass or less, 0.2% by mass or less, or 0.15% by mass or less. (Potassium) The polyvinyl alcohol type resin film may further contain potassium element. The potassium content in the polyvinyl alcohol resin film is not particularly limited and may be 0.40% by mass or more and 1.0% by mass or less. If the potassium content in the polyvinyl alcohol resin film is within the above range, there is a tendency to easily suppress the yellowing caused by polyeneization of the polyvinyl alcohol resin film. If the potassium content in the polarizer is within the above range, the potassium element is easy to act as a protective group for the hydroxyl group contained in the polyvinyl alcohol, and the dehydration reaction of the polyvinyl alcohol can be suppressed even when exposed to a high temperature of 115°C. The polyene chain will not be elongated to the extent that it can absorb light in the visible light region, and it is believed that there is a tendency to easily suppress the yellowing caused by polyeneization. The potassium content in the polyvinyl alcohol resin film may be 0.90 mass % or less, 0.80 mass % or less, 0.70 mass % or less, 0.65 mass % or less, 0.60 mass % or less, 0.55 mass % or less, or 0.50 mass % or less. The polarizing plate of this embodiment is a so-called absorption-type polarizing plate having the property of absorbing linearly polarized light having a vibration plane parallel to its absorption axis and transmitting linearly polarized light having a vibration plane orthogonal to the absorption axis (parallel to the transmission axis). (Parameter C) From the viewpoint of further suppressing yellowing after exposure to high temperatures, the polarizing plate of the present embodiment may satisfy the following formula (C). 0.001≤[Zn] / ([I]×[B]×[K])≤0.070(C) [In formula (C), [Zn] represents the content (mass %) of zinc element in the polyvinyl alcohol resin film, [I] represents the content (mass %) of iodine element in the polyvinyl alcohol resin film, [B] represents the content (mass %) of boron element in the polyvinyl alcohol resin film, and [K] represents the content (mass %) of potassium element in the polyvinyl alcohol resin film. [Zn] / ([I]×[B]×[K]) may be 0.003 or more, 0.005 or more, or 0.010 or more. [Zn] / ([I]×[B]×[K]) may be 0.060 or less, may be 0.050 or less, may be 0.040 or less, may be 0.030 or less, or may be 0.025 or less. (Parameter S) From the viewpoint of suppressing the change in color tone when exposed to high temperature, the area S[h] of the above-mentioned polarizer calculated as follows can satisfy a value greater than 0.1 and less than 45. The above-mentioned area S[h] is calculated by integrating the function f(t) related to absorbance in which the coefficients a to e obtained by the following steps (1) to (2) are substituted at t = 0 to 72 hours. Step (1): While the polarizing plates are exposed to an environment at 115° C., the absorbance at 780 nm of a pair of polarizing plates at crossed Nicol prisms is measured at 0 hours, 24 hours, 48 hours, 120 hours, 240 hours, and 500 hours. Step (2): Based on the seven combinations of time and absorbance obtained in (1) and the following function f(t), curve fitting based on the least squares method is performed to determine coefficients a to e. f(t)=a·Exp(-b·t)+c·Exp(-d·t)+e t: time [h] a~e:coefficient The optimization method for curve fitting is not particularly limited, but the GRG method (Generalized Reduced Gradient method) is suitable. <Polarizing Plate Manufacturing Method> The production method according to one embodiment includes a swelling step, a dyeing step, a cross-linking step, an optional washing step, an optional drying step, and a stretching step. (1) Swelling process The swelling treatment in this process is a treatment implemented as needed for the purpose of removing foreign matter, removing plasticizers, imparting easy dyeing properties, and plasticizing the film of the polyvinyl alcohol-based resin film as the original material film. Specifically, it can be a treatment of immersing the polyvinyl alcohol-based resin film in a treatment solution (swelling solution) containing water. The polyvinyl alcohol-based resin film as the original material film can appropriately utilize the resin film exemplified in the description column of the polarizer. The resin film can be immersed in one swelling solution, or can be immersed in two or more swelling solutions in sequence. The film can be subjected to uniaxial stretching treatment before the swelling treatment, during the swelling treatment, or before and during the swelling treatment. The thickness of the polyvinyl alcohol-based resin film as the raw material film is, for example, about 10 μm or more and 80 μm or less. From the viewpoint of making the thickness of the polarizer 15 μm or less, it is preferably 40 μm or less, and more preferably 30 μm or less. The polyvinyl alcohol-based resin film as the raw material film can be prepared in the form of a roll (rolled product) of a long unstretched or stretched polyvinyl alcohol-based resin film, for example. In this case, the polarizing plate is also obtained in the form of a long article. The swelling liquid may be water (for example, pure water) or an aqueous solution to which a water-soluble organic solvent such as alcohol is added. The temperature of the swelling solution when the original film is immersed is usually about 10 to 70° C., preferably about 15 to 50° C., and the immersion time of the film is usually about 10 to 600 seconds, preferably about 20 to 300 seconds. (2) Dyeing process The dyeing process in this process is a process for adsorbing iodine on the polyvinyl alcohol resin film and orienting it. Specifically, it can be a process of dipping the polyvinyl alcohol resin film in a treatment solution (dyeing solution) containing iodine. The film can be immersed in one dyeing solution, or in two or more dyeing solutions in sequence. In order to improve the dyeability of iodine, the film provided to the dyeing process can be subjected to at least a certain degree of uniaxial stretching. The uniaxial stretching process before the dyeing process can be replaced or, on the basis of the uniaxial stretching process before the dyeing process, the uniaxial stretching process can be carried out during the dyeing process. In addition, a dichroic organic dye may also be used while using iodine. When using a dichroic organic dye, the dichroic organic dye may also be used in combination with iodine in one dyeing solution, or in a dyeing solution different from the dyeing solution using iodine when using more than two dyeing tanks. Specific examples of the dichroic organic dye include Red BR, Red LR, Red R, Pink LB, Rubine BL, Bordeaux GS, Sky Blue LG, Lemon Yellow, Blue BR, Blue 2R, Navy RY, Green LG, Violet LB, Violet B, Black H, Black B, Black GSP, Yellow 3G, Yellow R, Orange LR, Orange 3R, Scarlet GL, Scarlet KGL, Congo Red, Brilliant Violet BK, Supra Blue G, Supra Blue GL, Supra Orange GL, Direct Sky Blue, and more. Blue), Direct Fast Orange S, and Fast Black. The dichroic dye may be used alone or in combination of two or more. As the dyeing solution containing iodine, an aqueous solution containing iodine and potassium iodide can be used. Other iodides such as zinc iodide can be used instead of potassium iodide, and potassium iodide and other iodides can also be used in combination. In addition, compounds other than iodides, such as boric acid, zinc chloride, cobalt chloride, etc., can also coexist. When adding boric acid, it is different from the cross-linking treatment described later in that it contains iodine. The content of iodine in the above-mentioned aqueous solution is usually 0.01 mass parts and less than 1 mass parts per 100 mass parts of water. In addition, the content of iodides such as potassium iodide is usually 0.01 mass parts and less than 20 mass parts per 100 mass parts of water. The concentration of boric acid in the above-mentioned aqueous solution can be set to be 0.1 mass parts and less than 5 mass parts per 100 mass parts of water. The temperature of the dyeing solution when the film is immersed is usually 10°C to 45°C, preferably 10°C to 40°C, more preferably 20°C to 35°C, and the immersion time of the film is usually 30 seconds to 600 seconds, preferably 60 seconds to 300 seconds. When a dichroic organic dye is used, an aqueous solution containing the dichroic organic dye can be used as the dyeing liquid. The content of the dichroic organic dye in the aqueous solution is usually 1×10 -4 parts by mass or more and 10 parts by mass or less, preferably 1×10 -3 The dyeing liquid may contain at least 1 part by mass and less than 1 part by mass. Dyeing aids may coexist in the dyeing liquid, for example, inorganic salts such as sodium sulfate, surfactants, etc. The dichroic organic dye may be used alone or in combination of two or more. The temperature of the dyeing liquid during the immersion of the film is, for example, 20°C to 80°C, preferably 30°C to 70°C, and the immersion time of the film is usually 30 seconds to 600 seconds, preferably 60 seconds to 300 seconds. (3) Cross-linking process The cross-linking treatment of the polyvinyl alcohol-based resin film after the dyeing process with a cross-linking agent is a treatment performed for the purpose of water resistance and color tone adjustment due to cross-linking. Specifically, it can be a treatment of immersing the film after the dyeing process in a treatment solution (cross-linking solution) containing a cross-linking agent. The film can be immersed in one cross-linking solution, or in two or more cross-linking solutions in sequence. During the cross-linking treatment, a uniaxial stretching treatment can be performed. (Crosslinking agent) As the cross-linking agent, boric acid, glyoxal, glutaraldehyde, etc. can be cited, preferably boric acid. It is also possible to use two or more cross-linking agents. The content of boric acid in the cross-linking solution is usually 0.1 mass parts or more and 15 mass parts or less per 100 mass parts of water, preferably 1 mass parts or more and 10 mass parts or less. (Iodide) When the dichroic pigment is iodine, the crosslinking liquid preferably contains an iodide in addition to boric acid. The content of iodide in the crosslinking liquid is usually 0.1 parts by mass or more and 15 parts by mass or less per 100 parts by mass of water, preferably 1 part by mass or more and 12 parts by mass or less. Examples of the iodide include potassium iodide, zinc iodide, and the like. (zinc sulfate and potassium sulfate) The cross-linking solution further comprises zinc sulfate and potassium sulfate. The content of zinc sulfate (ZnSO 4 ) in the crosslinking liquid may be 0.0005 to 30 parts by mass, preferably 0.001 to 25 parts by mass, and more preferably 0.1 to 10 parts by mass, per 100 parts by mass of water. The content of potassium sulfate (K2SO4) in the crosslinking liquid can usually be 0.1 to 30 parts by mass, preferably 0.2 to 25 parts by mass, and more preferably 0.3 to 20 parts by mass per 100 parts by mass of water. (Other ingredients) The cross-linking liquid may contain other components in addition to the cross-linking agent, iodide, zinc sulfate and potassium sulfate. Examples of other components contained in the crosslinking liquid include zinc salts other than zinc sulfate and potassium sulfate. Examples of zinc salts other than zinc sulfate and potassium sulfate contained in the crosslinking liquid include zinc halides such as zinc chloride and zinc iodide, zinc acetate, and zinc nitrate. Other examples of other components contained in the cross-linking liquid include cobalt chloride, zirconium chloride, sodium thiosulfate, and potassium sulfite. When the polyvinyl alcohol-based resin film is immersed in a plurality of cross-linking liquids, the concentrations of zinc sulfate and potassium sulfate in the cross-linking liquids may be different in the respective cross-linking liquids. By immersing the polyvinyl alcohol-based resin film in a crosslinking solution containing zinc sulfate and potassium sulfate, the contents of boron, iodine, and zinc in the resulting polarizer can be adjusted to fall within the range satisfying the above parameter A, and the above polarizer can be obtained. The temperature of the crosslinking solution during immersion of the film is usually 50° C. to 85° C., preferably 50° C. to 70° C., and the immersion time of the film is usually 10 seconds to 600 seconds, preferably 20 seconds to 300 seconds. In the cross-linking step, the polyvinyl alcohol-based resin film may be immersed in two or more cross-linking liquids. In this case, the composition and temperature of each cross-linking liquid may be the same or different. When the polyvinyl alcohol-based resin film is immersed in two or more cross-linking liquids, at least one cross-linking liquid contains zinc sulfate and potassium sulfate. The crosslinking solution may have a concentration and temperature of a crosslinking agent and iodide corresponding to the purpose of immersing the polyvinyl alcohol-based resin film. The crosslinking treatment for water resistance by crosslinking and the crosslinking treatment for color adjustment (color correction) may be performed in multiple steps (e.g., multiple tanks containing treatment solutions). In general, when both the cross-linking treatment for water resistance by cross-linking and the cross-linking treatment for color tone adjustment (color correction) are performed, the cross-linking liquid (color correction liquid) for the cross-linking treatment for color tone adjustment (color correction) is arranged in the latter stage. The temperature of the color correction liquid is, for example, 10° C. to 55° C., preferably 20° C. to 50° C. The immersion time of the membrane in the color correction liquid is usually 5 seconds to 600 seconds, preferably 10 seconds to 300 seconds. The content of the cross-linking agent in the color-replenishing solution is, for example, more than 1 mass part and less than 5 mass parts per 100 mass parts of water. The content of the iodide in the color-replenishing solution is, for example, more than 1 mass part and less than 30 mass parts per 100 mass parts of water. As shown above, the color-replenishing solution may contain zinc salts and other components. In the case where the color-replenishing solution contains zinc sulfate, the content of zinc sulfate may be more than 0.1 mass part and less than 20 mass parts per 100 mass parts of water, preferably more than 1 mass part and less than 10 mass parts. In the case where the color-replenishing solution contains potassium sulfate, the content of potassium sulfate may be more than 0.1 mass part and less than 20 mass parts per 100 mass parts of water, preferably more than 1 mass part and less than 10 mass parts. In the manufacture method of the polarizer of this mode, the polyvinyl alcohol-based resin film is suitable for being uniaxially stretched (stretching process) in any one or more stages from the swelling process to the cross-linking process. From the viewpoint of improving the dyeability of the dichroic pigment, the film provided to the dyeing process is preferably a film that has been uniaxially stretched to a certain extent, or preferably replaces the uniaxial stretching before the dyeing process or performs uniaxial stretching on the basis of the uniaxial stretching before the dyeing process during the dyeing process. The uniaxial stretching process can be any one of dry stretching for stretching in the air and wet stretching for stretching in liquid, or both of them can be performed. The uniaxial stretching process can be roller-to-roll stretching, hot roller stretching, stenter stretching, etc. for longitudinal uniaxial stretching by setting a circumferential speed difference between two clamping rollers, but preferably includes roller-to-roll stretching. The stretching ratio based on the original film (the cumulative stretching ratio thereof in the case of stretching treatment in more than two stages) is more than 3 times and about 8 times or less. In order to give good polarization characteristics, the stretching ratio is preferably set to more than 4 times, and more preferably set to more than 5 times. (4) Cleaning process The cleaning process in this process is a process implemented as needed for the purpose of removing excess cross-linking agents, dichroic pigments and other chemicals attached to the polyvinyl alcohol resin film, and is a process of using a cleaning solution containing water to clean the polyvinyl alcohol resin film after the cross-linking process. Specifically, it can be a process of immersing the polyvinyl alcohol resin film after the cross-linking process in a cleaning solution. The film can be immersed in one cleaning solution, or it can be immersed in two or more cleaning solutions in sequence. Alternatively, the cleaning process can also be a process of spraying the cleaning solution on the polyvinyl alcohol resin film after the cross-linking process in the form of a spray liquid, or the above-mentioned immersion and spraying can be combined. The cleaning liquid may be water (eg, pure water) or an aqueous solution to which a water-soluble organic solvent such as alcohol is added. The temperature of the cleaning liquid may be, for example, about 5° C. or higher and 40° C. or lower. The washing step is an optional step and may be omitted, or the washing treatment may be performed in the drying step as described later. It is preferred that the film after the washing step is subjected to a drying step. (5) Drying process The drying step is a step for drying the polyvinyl alcohol-based resin film after the cross-linking step or the washing step. The polarizing plate can be obtained by subjecting the polyvinyl alcohol-based resin film after the cross-linking step or the washing step to drying treatment. The drying treatment is carried out using a drying mechanism (heating mechanism) of the film. A suitable example of the drying mechanism is a drying furnace. The drying furnace is preferably a drying furnace capable of controlling the temperature in the furnace. The drying furnace is, for example, a hot air oven capable of increasing the temperature in the furnace by supplying hot air, etc. In addition, the drying treatment based on the drying mechanism can be a treatment in which the polyvinyl alcohol-based resin film after the crosslinking process or the cleaning process is closely attached to one or more heating bodies having a convex curved surface, or a treatment in which the film is heated using a heater. The heating body includes a roller (e.g., a guide roller also serving as a heating roller) that has a heat source (e.g., a heat medium such as warm water, an infrared heater) inside and can increase the surface temperature. The heater includes an infrared heater, a halogen heater, a plate heater, and the like. The drying temperature (eg, the temperature inside the drying furnace, the surface temperature of the heat roll, etc.) is usually 30° C. to 100° C., preferably 50° C. to 90° C. The drying time is not particularly limited, but is, for example, 30 seconds to 600 seconds. Through the above steps, a polarizing plate in which a dichroic dye is adsorbed and oriented on a uniaxially stretched polyvinyl alcohol-based resin film can be obtained. <Polarizing plate> like Figure 1 As shown, a polarizing plate 100 according to one embodiment of the present invention includes the polarizer 102 described above, a first protective film 101 provided on one surface thereof, and a second protective film 103 provided on the other surface thereof. The polarizing plate may not include the second protective film 103 . The first and second protective films may be transparent resin films containing thermoplastic resins, for example, polyolefin resins such as chain polyolefin resins (polypropylene resins, etc.), cyclic polyolefin resins (norbornene resins, etc.); cellulose ester resins such as triacetyl cellulose and diacetyl cellulose; polyester resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polycarbonate resins; (meth) acrylic resins such as polymethyl methacrylate resins; or mixtures and copolymers thereof. The first and second protective films may be made of the same material or different materials. Either or both of the first protective film and the second protective film may be protective films having optical functions such as a phase difference film and a brightness enhancement film. For example, a transparent resin film containing the above materials is stretched (uniaxially stretched or biaxially stretched, etc.), or a liquid crystal layer is formed on the film, thereby making a phase difference film with an arbitrary phase difference value. A surface treatment layer (coating layer) such as a hard coat layer, an antiglare layer, an antireflection layer, an antistatic layer, or an antifouling layer may be formed on the surface of the first protective film 101 and / or the second protective film 103 opposite to the polarizing plate 102 . From the viewpoint of reducing the thickness of the polarizing plate 100 , the thickness of the first and second protective films is preferably thin. However, if too thin, the strength decreases and processability tends to be poor. Therefore, the thickness is preferably 5 to 150 μm, more preferably 5 to 100 μm, and further preferably 10 to 50 μm. The polarizing plate 100 can be obtained by laminating (stacking) the first protective film 101 and the second protective film 103 on both sides of the polarizer 102 via an adhesive. As the adhesive used in laminating the polarizer and the protective film, active energy ray-curable adhesives such as ultraviolet curable adhesives, aqueous solutions of polyvinyl alcohol resins or aqueous solutions in which a crosslinking agent is formulated, and water-based adhesives such as urethane emulsion adhesives can be cited. In the case of laminating the protective film on both sides of the polarizer 102, the adhesives forming the two adhesive layers can be of the same type or of different types. For example, in the case of laminating the protective film on both sides of the polarizer, one side can be laminated with a water-based adhesive and the other side can be laminated with an active energy ray-curable adhesive. The ultraviolet curable adhesive can be a mixture of a free radical polymerizable (meth) acrylic compound and a photoradical polymerization initiator, a mixture of a cationic polymerizable epoxy compound and a photocationic polymerization initiator, etc. Moreover, you may use together a cationically polymerizable epoxy compound and a radically polymerizable (meth)acrylic compound, and you may use together a photocationic polymerization initiator and a photoradical polymerization initiator as an initiator. When an active energy ray-curable adhesive is used, the adhesive is cured by irradiating the active energy ray after lamination. The light source of the active energy ray is not particularly limited, but preferably an active energy ray (ultraviolet ray) having a luminous distribution below a wavelength of 400 nm, specifically, a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, a metal halide lamp, etc. are preferably used. In order to improve the adhesion between the polarizer and the protective film, the bonding surface of the polarizer and / or the protective film may be subjected to surface treatment such as corona treatment, flame treatment, plasma treatment, ultraviolet irradiation treatment, primer coating treatment, saponification treatment, etc. before bonding the polarizer and the thermoplastic resin film. When the polarizing plate 102 has protective films laminated on both sides of the polarizing plate, the method further includes a second laminating step of laminating a second protective film to the polarizing plate surface having the first protective film on one side thereof using an adhesive. (use) The polarizing plate can be used in a display device. The display device can be any display device such as a liquid crystal display device, an organic EL display device, but preferably a liquid crystal display device. The liquid crystal display device has a liquid crystal panel having a liquid crystal unit as an image display element and a backlight. When constructing a liquid crystal display device, the polarizing plate can be used for a polarizing plate configured on the visible side, can also be used for a polarizing plate configured on the backlight side, and can also be used for a polarizing plate on both the visible side and the backlight side. The above-mentioned polarizing plate is particularly suitable for a vehicle-mounted display device. For example, in a vehicle-mounted display device, the polarizing plate is bonded to an image display unit with an adhesive or bonding agent, and a light-transmitting member such as a glass plate or a touch panel is bonded to the surface opposite to the surface bonded to the image display unit with an adhesive or bonding agent. The polarizing plate of a vehicle-mounted display device is sometimes used for a long time at a relatively high temperature, and in such a case, it tends to turn yellow easily, and the polarizing plate of this embodiment has a high effect. The polarizing plate is suitable for an in-vehicle display device including a polarizing plate, a light-transmitting member disposed on the first protective film side of the polarizing plate, and a display device disposed on the second protective film side of the polarizing plate. The light-transmitting member may be a glass plate, a light-transmitting resin film, or the like. Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples. Example <Example 1> (Manufacturing of Polarizing Plate) A transparent unstretched polyvinyl alcohol film (TS4500, manufactured by Kuraray Co., Ltd.) having a thickness of 45 μm and a saponification degree of 99.9% or more was immersed in water (deionized water) at 30° C. for 86 seconds to swell, and then immersed in a dyeing solution having a mass ratio of iodine / potassium iodide / water of 1.0 / 2.0 / 7.0 and a mass ratio of boric acid to water of 0.4 / 2.0 / 97.6 at a temperature of 30° C. for 160 seconds to dye. At this time, the film was stretched at a stretch ratio of 2.00 times and 1.51 times in the swelling and dyeing stages, respectively, and stretched in such a way that the cumulative stretch ratio until the dyeing tank was 3.02 times. Next, the film was immersed in a crosslinking solution (crosslinking stage) of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water in a mass ratio of 2.2 / 3.5 / 2.1 / 2.6 / 89.6 and heated to 60°C for 76 seconds to crosslink the film and stretched at a stretch ratio of 1.86. Then, an aqueous solution of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water with a mass ratio of 2.6 / 4.4 / 2.3 / 2.7 / 88.0 was heated to 45°C and immersed in a crosslinking solution for 12 seconds (color correction stage) to crosslink, and then stretched by 1.04 times. At this time, the total cumulative stretching ratio of the swelling, dyeing, crosslinking, and color correction stages was 5.83 times. After the crosslinking was completed, the polyvinyl alcohol film stretched 5.83 times was dried in an oven at 60° C. for 200 seconds to produce a polarizing plate. The thickness of the polarizing plate was about 20 μm. <Example 2> (Manufacturing of Polarizing Plate) A transparent unstretched polyvinyl alcohol film (TS4500, manufactured by Kuraray Co., Ltd.) having a thickness of 45 μm and a saponification degree of 99.9% or more was immersed in water (deionized water) at 30° C. for 86 seconds to swell, and then immersed in a dyeing solution having a mass ratio of iodine / potassium iodide / water of 1.0 / 2.0 / 7.0 and a mass ratio of boric acid to water of 0.4 / 2.0 / 97.6 at a temperature of 30° C. for 160 seconds to dye. At this time, the film was stretched at a stretch ratio of 2.00 times and 1.51 times in the swelling and dyeing stages, respectively, and stretched in such a way that the cumulative stretch ratio until the dyeing tank was 3.02 times. Next, the film was immersed in a crosslinking solution (crosslinking stage) of an aqueous solution of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water in a mass ratio of 2.4 / 3.9 / 4.8 / 5.7 / 100 heated to 60°C for 76 seconds to crosslink the film and stretched at a stretch ratio of 1.86. Then, an aqueous solution of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water in a mass ratio of 2.9 / 5.0 / 4.8 / 6.2 / 100 was heated to 45°C and immersed in a crosslinking solution for 12 seconds (color correction stage) to crosslink, and then stretched by 1.04 times. At this time, the total cumulative stretching ratio of the swelling, dyeing, crosslinking, and color correction stages was 5.83 times. After the crosslinking was completed, the polyvinyl alcohol film stretched 5.83 times was dried in an oven at 60° C. for 200 seconds to produce a polarizing plate. The thickness of the polarizing plate was about 20 μm. <Comparative Example 1> (Manufacturing of Polarizing Plate) A transparent unstretched polyvinyl alcohol film (TS4500, manufactured by Kuraray Co., Ltd.) having a thickness of 45 μm and a saponification degree of 99.9% or more was immersed in water (deionized water) at 30° C. for 86 seconds to swell, and then immersed in a dyeing solution having a mass ratio of iodine / potassium iodide / water of 1.0 / 2.0 / 7.0 and a mass ratio of boric acid to water of 0.4 / 2.0 / 97.6 at a temperature of 30° C. for 160 seconds to dye. At this time, the film was stretched at a stretch ratio of 2.00 times and 1.51 times in the swelling and dyeing stages, respectively, and stretched in such a way that the cumulative stretch ratio until the dyeing tank was 3.02 times. Next, the film was immersed in a crosslinking solution (crosslinking stage) of an aqueous solution of potassium iodide / boric acid / water at a mass ratio of 1.2 / 3.7 / 95.1 heated to 60° C. for 76 seconds to crosslink the film, and was stretched at a stretch ratio of 1.86. Then, the film was immersed in a crosslinking solution heated to 45°C in a mass ratio of potassium iodide / boric acid / water of 1.4 / 4.7 / 93.9 for 12 seconds (color correction stage) to crosslink the film, and then stretched by 1.04 times. At this time, the total cumulative stretching ratio of the swelling, dyeing, crosslinking, and color correction stages was 5.83 times. After the crosslinking was completed, the polyvinyl alcohol film was dried in an oven at 60° C. for 200 seconds to produce a polarizing plate. The thickness of the polarizing plate was about 20 μm. <Comparative Example 2> (Manufacturing of Polarizing Plate) A transparent unstretched polyvinyl alcohol film (TS4500, manufactured by Kuraray Co., Ltd.) having a thickness of 45 μm and a saponification degree of 99.9% or more was immersed in water (deionized water) at 30° C. for 86 seconds to swell, and then immersed in a dyeing solution having a mass ratio of iodine / potassium iodide / water of 1.0 / 2.0 / 7.0 and a mass ratio of boric acid to water of 0.4 / 2.0 / 97.6 at a temperature of 30° C. for 160 seconds to dye. At this time, the film was stretched at a stretch ratio of 2.00 times and 1.51 times in the swelling and dyeing stages, respectively, and stretched in such a way that the cumulative stretch ratio until the dyeing tank was 3.02 times. Next, the film was immersed in a crosslinking solution (crosslinking stage) of an aqueous solution of potassium iodide / boric acid / zinc nitrate hexahydrate / water at a mass ratio of 2.3 / 3.6 / 2.0 / 92.1 heated to 60°C for 76 seconds to crosslink the film and stretched at a stretch ratio of 1.86. Then, an aqueous solution of potassium iodide / boric acid / zinc nitrate 6 hydrate / water in a mass ratio of 2.7 / 4.5 / 2.4 / 90.4 was heated to 45°C and immersed in a crosslinking solution for 12 seconds (color correction stage) to crosslink, and then stretched by 1.04 times. At this time, the total cumulative stretching ratio of the swelling, dyeing, crosslinking, and color correction stages was 5.83 times. After the crosslinking was completed, the polyvinyl alcohol film stretched 5.83 times was dried in an oven at 60° C. for 200 seconds to produce a polarizing plate. The thickness of the polarizing plate was about 20 μm. [Durability test for yellow index evaluation] The polarizers of the examples and comparative examples were cut into 30 mm in the MD direction (absorption axis direction of the polarizer) and 25 mm in the TD direction (transmission axis direction of the polarizer). The polarizers were clamped by two metal plates with a length of 40 mm, a width of 40 mm, a thickness of 2 mm and a hole with a diameter of 20 mm in the center, and the four sides were fixed with a polyimide tape (Kapton tape). The evaluation sample fixed to the metal plate was placed in a 115° C. heating oven in an upright state, taken out after 500 hours, and evaluated. [Yellowness Index Evaluation] The initial yellowness index of the polarizing plate sample before the durability test was measured using a spectrophotometer (U4100, manufactured by Hitachi, Ltd.) in accordance with JIS K 7373 (2006). Then, the yellowness index of the sample after the durability test was similarly determined using a spectrophotometer (U4100 manufactured by Hitachi, Ltd.) in accordance with JIS K 7373 (2006). Based on the obtained yellowness index, the difference ΔYI between the yellowness index before and after the durability test was calculated by the following formula. ΔYI = (yellow index after durability test) - (initial yellow index) When the obtained yellow index difference was less than 30 at 115° C. after 500 hours, it was evaluated as good, and when it was 30 or more, it was evaluated as poor. <Durability test for single Δab evaluation> The evaluation samples were cut into 50 mm × 40 mm in a manner that the absorption axis of the polarizer was parallel to the long side. The evaluation samples obtained in this manner were subjected to spectral measurement (measurement wavelength: 280 to 900 nm) before the durability test using a spectrophotometer U-4100 manufactured by Hitachi High-Technologies. Thereafter, the monomer transmittance of the same sample was measured at regular intervals in an environment of 115°C to obtain the hue (a, b). The measurement time was set to after a 24-hour durability test, after 48 hours, after 120 hours, after 240 hours, and after 500 hours. Single Δab is calculated using the following calculation formula. Single Δab=√{(a after durability test - a before durability test) 2 +(b after durability test - b before durability test) 2} [Changes in Single Δab from 240h to 500h] The rapid change of Single Δab from 240h to 500h was calculated using the following calculation formula. The rapid change of Single Δab during 240h to 500h = (SΔab after 500h - SΔab after 240h) If the change in Single Δab during 240 h to 500 h is small, it can be considered that a sudden change in the color tone of the polarizing plate can be suppressed. [Curve fitting and area S] Based on the results of the Single Δab evaluation durability test, coefficients a to e were obtained based on the combined data of time and absorbance and function f(t) using the Generalized Reduced Gradient method using Excel 2016 Solver. It should be noted that the initial values of coefficients a to e in formula (A) are 0. Function f(t) = a·Exp(-b·t)+c·Exp(-d·t)+e It should be noted that the results of curve fitting show that the coefficients a to e obtained from the polarizing plate obtained in Example 1 are coefficient a=1.1, coefficient b=0.36, coefficient c=0.40, coefficient d=0.0084, and coefficient e=0.21. The area S of the polarizing plate obtained in Example 1 is 39.8. The coefficients a to e obtained from the polarizing plate obtained in Example 2 were: coefficient a=1.0, coefficient b=0.36, coefficient c=0.39, coefficient d=0.0075, and coefficient e=0.22. The coefficients a to e obtained from the fitting curve were substituted into the function f(t), and the function f(t) was integrated over t=0 to 72 hours to determine the area S. The area S of the polarizing plate obtained in Example 2 was 40.7. [Elemental analysis and measurement method in polarizing film] The boron and zinc contents of the polarizing plates of Examples and Comparative Examples were determined by microwave decomposition / ICP-AES, the potassium content was determined by microwave decomposition / atomic absorption spectrometry, and the iodine content was determined by oxygen combustion / ion chromatography. [Measurement of thickness of polarizing plate] The measurement was performed using a digital altimeter "MH-15M" manufactured by Nikon Corporation. Table 1 shows the components of the obtained polarizing plate and the properties of the polarizing plate. [Table 1] <Example 3> A polarizing plate was manufactured in the same manner as in Example 1 except that the dyeing liquid was an aqueous solution having a mass ratio of iodine / potassium iodide / water of 1.0 / 2.0 / 7.0 and a mass ratio of boric acid to water of 0.4 / 2.8 / 96.8, the crosslinking liquid was an aqueous solution having a mass ratio of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water of 2.4 / 5.5 / 2.4 / 2.6 / 100 and a temperature of 66° C., and the color correction liquid was an aqueous solution having a mass ratio of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water of 2.5 / 6.1 / 2.5 / 2.7 / 100 and a temperature of 47° C. The thickness of the polarizing plate was about 20 μm. <Example 4> A polarizing plate was manufactured in the same manner as in Example 1 except that the dyeing solution was an aqueous solution having a mass ratio of iodine / potassium iodide / water of 1.0 / 2.0 / 7.0 and a mass ratio of boric acid to water of 0.4 / 2.0 / 97.6, the crosslinking solution was an aqueous solution having a mass ratio of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water of 2.8 / 5.5 / 2.4 / 2.6 / 100 and a temperature of 62° C., and the color correction solution was an aqueous solution having a mass ratio of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water of 2.9 / 6.1 / 2.5 / 2.7 / 100 and a temperature of 47° C. The thickness of the polarizing plate was about 20 μm. <Example 5> A polarizing plate was produced in the same manner as in Example 1 except that the dyeing liquid was an aqueous solution having a mass ratio of iodine / potassium iodide / water of 1.0 / 2.0 / 7.0 and the mass ratio of boric acid to water was 0.2 / 2.0 / 97.8, the temperature of the crosslinking liquid in the crosslinking stage was set to 62° C., and the temperature of the liquid in the color correction stage was set to 47° C. The thickness of the polarizing plate was about 20 μm. <Example 6> A polarizing plate was produced in the same manner as in Example 1 except that the dyeing liquid was an aqueous solution having a mass ratio of iodine / potassium iodide / water of 1.0 / 2.0 / 7.0 and the mass ratio of boric acid to water was 0.3 / 2.0 / 97.7, the temperature of the crosslinking liquid in the crosslinking stage was set to 64° C., and the temperature of the liquid in the color correction stage was set to 47° C. The thickness of the polarizing plate was about 20 μm. [Durability test for yellow index evaluation] The polarizers of the examples and comparative examples were cut into 30 mm in the MD direction (absorption axis direction of the polarizer) and 25 mm in the TD direction (transmission axis direction of the polarizer). The polarizers were clamped by two metal plates with a length of 40 mm, a width of 40 mm, a thickness of 2 mm and a hole of 20 mm in the center, and the four sides were fixed with polyimide tape. The evaluation sample fixed to the metal plate was placed in a 115° C. heating oven in an upright state, taken out after 500 hours, and evaluated. [Yellowness Index Evaluation] The initial yellowness index of the polarizing plate sample before the durability test was measured using a spectrophotometer (U4100, manufactured by Hitachi, Ltd.) in accordance with JIS K 7373 (2006). Then, the yellowness index of the sample after the durability test was similarly determined using a spectrophotometer (U4100 manufactured by Hitachi, Ltd.) in accordance with JIS K 7373 (2006). Based on the obtained yellowness index, the difference ΔYI between the yellowness index before and after the durability test was calculated by the following formula. ΔYI = (yellow index after durability test) - (initial yellow index) When the obtained yellow index difference was less than 30 at 115° C. after 500 hours, it was evaluated as good, and when it was 30 or more, it was evaluated as poor. <Durability test for single Δab evaluation> The evaluation samples were cut into 50 mm × 40 mm in a manner that the absorption axis of the polarizer was parallel to the long side. The evaluation samples obtained in this manner were subjected to spectral measurement (measurement wavelength: 280 to 900 nm) before the durability test using a spectrophotometer U-4100 manufactured by Hitachi High-Technologies. Thereafter, the monomer transmittance of the same sample was measured at regular intervals in an environment of 115°C to obtain the hue (a, b). The measurement time was set to after a 24-hour durability test, after 48 hours, after 120 hours, after 240 hours, and after 500 hours. Single Δab is calculated using the following calculation formula. Single Δab=√{(a after durability test - a before durability test) 2 +(b after durability test - b before durability test) 2} [Changes in Single Δab from 240h to 500h] The rapid change of Single Δab from 240h to 500h was calculated using the following calculation formula. The rapid change of Single Δab during 240h to 500h = (SΔab after 500h - SΔab after 240h) If the change in Single Δab during 240 h to 500 h is small, it can be considered that a sudden change in the color tone of the polarizing plate can be suppressed. [Elemental analysis and measurement method in polarizing film] The boron and zinc contents of the polarizing plates of Examples and Comparative Examples were determined by microwave decomposition / ICP-AES, the potassium content was determined by microwave decomposition / atomic absorption spectrometry, and the iodine content was determined by oxygen combustion / ion chromatography. Table 2 shows the components in the polarizing plates of Examples 3-7 and the properties of the polarizing plates.
Table 2
Claims
1. A polarizing plate, The polyvinyl alcohol resin film contains boron, iodine and zinc. The polarizer satisfies the following formula (A): 0.001≤[Zn] / ([I]×[B])≤0.025(A) In formula (A), [Zn] represents the content of zinc element in the polyvinyl alcohol resin film, [I] represents the content of iodine element in the polyvinyl alcohol resin film, and [B] represents the content of boron element in the polyvinyl alcohol resin film, and the units of the contents are mass %.
2. The polarizing plate according to claim 1, wherein [Zn] is 0.01 mass % or more and 1.0 mass % or less.
3. The polarizing plate according to claim 1 or 2, wherein: [B] is 3.5 mass % or more and 6.0 mass % or less.
4. The polarizing plate according to claim 1 or 2, wherein: [I] is 2.0 mass % or more and 4.0 mass % or less. 5 . A polarizing plate comprising the polarizer according to claim 1 or 2 , an adhesive layer, and a protective film in this order.