Parameter optimization method for insulation repair processing of cable flexible joint
By preparing and optimizing the insulation samples of cable soft joints, combining qualitative and quantitative evaluation indicators, and adjusting process parameters, the problem of lack of targeted and systematic selection of process parameters during the processing of soft joints is solved, and the insulation interface and quality of the soft joints are improved. electrical performance, reducing experimental costs and research and development cycles.
Patent Information
- Application Number
- CN202410877294.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-02
AI Technical Summary
The selection of process parameters during the processing of existing cable flexible joints lacks purpose and systematicness, the experimental cost is high, and it is difficult to achieve accurate and efficient insulation interface performance optimization, resulting in flexible joints that are prone to failure in the submarine environment.
A parameter optimization method for cable soft joint insulation repair processing is adopted. By preparing insulation samples, performing injection molding and molding, optimizing the molding and cross-linking parameters, combined with qualitative and quantitative evaluation indicators, the process parameters are gradually adjusted until the performance requirements are met. Including the optimization of molding temperature, molding pressure, cross-linking temperature, cross-linking pressure and cross-linking time.
It realizes the simulation of the soft joint manufacturing process under laboratory conditions, reduces the cost of process parameter optimization, improves work efficiency, significantly improves the insulation interface performance and electrical performance of the soft joint, and shortens the research and development cycle.
Smart Images

Figure CN118734581A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a parameter optimization method for cable flexible joint insulation repair processing, and belongs to the field of power cable insulation design and manufacturing. Background Art
[0002] With the increasing demand for offshore wind power grid connection and cross-sea power transmission, high-voltage submarine cables have become an important part of power lines. In order to meet the needs of long-distance power transmission, intermediate joints or flexible joints are often used to connect the cable segments to extend the laying length. In addition, the environment in which submarine cables are located is very complex, and they are easily damaged by external forces such as tsunamis, ocean current changes, high-salinity seawater erosion, earthquakes, and collisions and bites of marine ecological animals. At the same time, under the influence of internal factors such as multi-stress aging, high-voltage submarine cables are very prone to breakage, damage and breakdown, which also requires a complete repair method.
[0003] Compared with the complex prefabricated intermediate joints, the flexible joints with small size, light weight, high mechanical strength and good electrical performance are more adaptable to the complex submarine environment and gradually become the main method for connecting multiple cables and repairing insulation damage of submarine cables. The basic properties of the repair insulation filled with the flexible joint are consistent with those of the main insulation, so its structural size and bending performance are only a few millimeters different from the jointless part of the cable, and the external sheath structure can be almost the same.
[0004] However, the cross-linked polyethylene insulated high-voltage submarine cable flexible joint technology is very complex, and the design and manufacture of flexible joints are extremely difficult. In the high-voltage submarine cable flexible joint, the original cable body insulation has been cross-linked, and the newly restored cross-linked polyethylene insulation is made by molding and cross-linking in sequence during the flexible joint manufacturing process. Since the molding and cross-linking processes of the body insulation and the restored insulation are asynchronous, although the same cross-linked polyethylene material is used, there is still an obvious fusion interface between the two (the interface is at a certain angle with the conductor of the cable), and the insulation strength of the interface is significantly lower than the surrounding cross-linked polyethylene insulation, which results in the flexible joint being the weakest and most prone to failure in the entire submarine cable system.
[0005] During the processing of flexible joints, changes in process parameters have a significant impact on the characteristics of the fusion interface. If appropriate process parameters can be obtained for molding and cross-linking of restored insulation, the electrical strength of the interface can be effectively improved, thereby improving the reliability of the flexible joint. The optimization of the processing parameters for restoring insulation of flexible joints faces two problems. First, the current method for testing the performance of flexible joints is not suitable for parameter optimization scenarios with large engineering volumes. Second, multiple process parameters work together during the processing of flexible joints. In the absence of effective evaluation indicators for the performance of the flexible joint insulation interface, it is difficult to design an efficient optimization process.
[0006] At present, there are two main methods for testing the performance of flexible joints. One is to first completely manufacture a small section of cable, manually cut to simulate the fault area, and then perform insulation restoration work, or weld the two sections of cable conductors, and then perform insulation restoration work, and repeat this process to obtain test data. The disadvantages of this test method are high cost, long cycle, poor repeatability of sample manufacturing, and high cost and long cycle for testing with small sections of coaxial structure cables, too demanding requirements for sites and test equipment, and unable to provide sufficient data for the optimization of process parameters. Another method is to use flat sheet samples to simulate the performance test of the fusion interface. The method is to make cross-linked polyethylene sheets and uncross-linked polyethylene sheets respectively, and then stack two samples of the same size in parallel, and then put them together under high pressure and high temperature conditions to complete a cross-linking. However, in the actual manufacturing process of high-voltage submarine cable flexible joints, in order to ensure the quality of restored insulation, the restored insulation is mostly molded by extrusion, so this method cannot simulate the process of extrusion restoration of insulation, and it is difficult to provide help for the optimization of process parameters.
[0007] At present, the evaluation indicators for the insulation interface performance of flexible joints are still imperfect. First, the current evaluation indicators are still mainly based on electrical performance, which is relatively single and difficult to fully reflect the impact of changes in various process parameters during the processing of flexible joints on the insulation interface performance of flexible joints; second, the performance of the flexible joint after manufacture is affected by multiple factors during the processing, and it is difficult to reflect the changes in a certain process parameter during the processing only through its final performance.
[0008] In summary, if the manufacturing process of flexible joints can be simulated under laboratory conditions, experimental research can be carried out using small-sized equivalent specimens, and appropriate interface performance evaluation standards can be adopted to optimize the process conditions, systematic batch experimental data can be obtained quickly and effectively, which will greatly reduce the research difficulty of high-voltage submarine cable flexible joints and shorten the R&D cycle, which is of great significance for the process improvement of submarine cable flexible joints. However, the current test methods for flexible joint performance and the evaluation indicators of insulation interface performance are difficult to support an accurate, efficient, and economical method for optimizing the key parameters of cable flexible joint insulation restoration processing. Summary of the invention
[0009] The present invention aims to solve the problems in the existing cable flexible joint processing process, such as lack of purpose and systematicness in the selection of key process parameters, high experimental cost, large experimental workload, and lack of corresponding performance as evaluation and optimization criteria, and provide a parameter optimization method for cable flexible joint insulation repair processing.
[0010] The technical solution of the present invention:
[0011] One of the purposes of the present invention is to provide a parameter optimization method for cable flexible joint insulation repair processing, the method comprising the following steps:
[0012] (1) Determine the initial process parameters and prepare an insulating sample;
[0013] (2) Performing injection molding and molding to restore the insulation of the primary insulation sample to obtain an insulation repair sample;
[0014] (3) The obtained insulation repair samples are evaluated by qualitative evaluation index I and quantitative evaluation index I in turn, and the uncross-linked composite insulation samples and the preferred process parameters of the injection molding process, the molding temperature T a and molding pressure P a ;
[0015] (4) performing secondary insulation crosslinking on the uncrosslinked composite insulation sample to obtain a crosslinked composite insulation sample;
[0016] (5) The obtained cross-linked composite insulation sample is optimized in turn with respect to qualitative evaluation index II, qualitative evaluation index I, quantitative evaluation index I and quantitative evaluation index II to obtain the secondary insulation sample and the cross-linking temperature T of the optimal process parameter of the cross-linking process. b , cross-linking pressure P b and cross-linking time t b ;
[0017] (6) Evaluate the obtained secondary insulation sample according to the quantitative evaluation index II. If the sample meets the qualitative evaluation index II, continue to evaluate the quantitative evaluation index III. If the sample does not meet the qualitative evaluation index II, repeat step (5) until the secondary insulation sample meets the qualitative evaluation index II.
[0018] (7) If the secondary insulation sample meets the evaluation of quantitative evaluation index III, the parameter number plastic temperature T for cable flexible joint insulation repair processing is obtained. a , Molding pressure P a , cross-linking temperature T b , cross-linking pressure P b and cross-linking time t b ;
[0019] If the secondary insulation sample does not meet the evaluation of quantitative evaluation index III, re-formulate qualitative evaluation index I, quantitative evaluation index I, qualitative evaluation index II and quantitative evaluation index II, and repeat steps (1) to (6) until the evaluation of quantitative evaluation index III is met.
[0020] It is further defined that the initial process parameters in (1) include the size of the primary insulation sample, the type of insulation material, and the shape and angle of the insulation interface;
[0021] The method for preparing a primary insulation sample is as follows: filling the insulation material into a mold, hot pressing it in a flat vulcanizer, and then heating and cross-linking it.
[0022] It is further defined that the method for preparing the insulation repair sample in (2) is: installing the primary insulation sample in an insulation recovery molding device to perform injection molding and molding of restored insulation to obtain the insulation repair sample.
[0023] It is further defined that the primary insulation sample and the insulation repair sample are prepared using the same insulating material to ensure the overall consistency of the composite insulation after the insulation is restored.
[0024] It is further defined that the qualitative evaluation index I is that the partial discharge is less than 5pC or the micropore size at the interface between the insulation repair specimen and the primary insulation specimen is less than 0.05mm;
[0025] In (3), when the insulation repair specimen does not meet the qualitative evaluation index I, the plastic temperature T a , until the plastic temperature reaches 120℃. If the plastic temperature reaches 120℃ and still does not meet the qualitative evaluation index I, then increase the plastic pressure P a ;
[0026] In (5), when the cross-linked composite insulation sample does not meet the qualitative evaluation index I, the cross-linking pressure P is increased. b .
[0027] It is further defined that the partial discharge quantity is tested in accordance with the reference standard GB / T-11017.1-2014.
[0028] Further defined, the statistical reference standard GB / T18890.1-2015 for the distribution of micropores of different sizes within the interface is tested.
[0029] Further defined, quantitative evaluation index I is that the micropore size at the interface between the insulation repair sample and the primary insulation sample is less than 0.05 mm, and the micropore size greater than 0.025 mm is less than 0.05 mm per 10 cm. 3 Less than 18;
[0030] In (3), when the insulation repair specimen does not meet the quantitative evaluation index I, the molding pressure P is increased. a ;
[0031] In (5), when the cross-linked composite insulation sample does not meet the quantitative evaluation index I, the cross-linking pressure P is increased. b .
[0032] Further defined, the statistical reference standard GB / T18890.1-2015 for the distribution of micropores of different sizes within the interface is tested.
[0033] It is further defined that the qualitative evaluation index II is that the thermal elongation of the cross-linked composite insulation specimen is ≤175% and the permanent elongation is ≤15%;
[0034] In (5), when the cross-linked composite insulation sample does not meet the qualitative evaluation index II, the cross-linking temperature T b .
[0035] It is further defined that the thermal elongation and permanent elongation of the material are tested with reference to the standard GB / T 2951.21-2008.
[0036] It is further defined that the quantitative evaluation index II is that the change in the carbonyl index of the primary insulation sample after injection molding and molding and cross-linking of the restored insulation is less than 80%;
[0037] In (5), when the cross-linked composite insulation sample does not meet the quantitative evaluation index II, the cross-linking time t b .
[0038] To further define, the carbonyl index CI is measured using micro-FTIR.
[0039] It is further defined that the quantitative evaluation index III is that the ratio of the AC and DC characteristic breakdown field strength of the cross-linked composite insulation sample to the AC and DC characteristic breakdown field strength of the primary insulation sample is higher than 80%, and the shape parameter of the cross-linked composite insulation sample is greater than 5.
[0040] Further defining, the AC and DC characteristic breakdown field strengths and shape parameters are measured based on cylindrical electrodes.
[0041] It is further defined that the method for performing secondary insulation cross-linking on the uncross-linked composite insulation sample in (4) is: cross-linking is performed at a certain temperature and a certain pressure, and then degassing is performed in a vacuum environment of 80°C for 12 hours after cross-linking to obtain a cross-linked composite insulation sample.
[0042] The second object of the present invention is to provide a primary insulating sample preparation mold used in the above method, specifically the mold comprises an upper mold and a lower mold, the upper mold and the lower mold are axially symmetrical solid metal structures, and when the molds are closed, the two molds are coaxially fitted through the cooperation of the positioning pins and the positioning holes to form a mold cavity;
[0043] The upper die is an integrated structure consisting of a top plate and a round table, and a material storage trough is provided on the top surface of the round table;
[0044] The lower mold is an integrated structure consisting of a bottom plate and a side plate. There is a certain inclination angle between the side plate and the bottom plate, and an overflow groove is provided on the side plate.
[0045] The third object of the present invention is to provide an insulation recovery molding device used in the above method. Specifically, the device includes an upper heating plate, a lower heating plate and a disposable insulation sample located between the upper heating plate and the lower heating plate. The upper heating plate is provided with an injection molding port.
[0046] Beneficial effects:
[0047] The present invention aims at the problem that inappropriate process parameters in the two parts of the molding and cross-linking of the cable flexible joint insulation restoration molding, which include the molding of the insulation restoration, will cause physical or chemical defects. For example, too low temperature and pressure will cause micropores to exist in the interface formed between the primary insulation and the insulation restoration, and too high cross-linking temperature and too long cross-linking time will cause the primary insulation to age. These defects will weaken the electrical performance of the flexible joint. Optimization steps and evaluation criteria are set respectively, and the cable flexible joint insulation restoration simulation is molded by preparing a mold with a self-made primary insulation sample and an insulation restoration molding device, and the key parameters of the processing process are optimized. The specific optimization parameters include the heating temperature and molding pressure in the molding stage, and the heating temperature, heating time and cross-linking pressure in the cross-linking stage. Compared with the prior art, it has the following advantages:
[0048] (1) The present invention proposes a complete and systematic optimization method for key parameters in the cable flexible joint processing process. In the optimization process, the temperature and pressure parameters of the cable flexible joint insulation recovery injection molding stage and the cross-linking stage are optimized step by step, with clear levels and high executability;
[0049] (2) The present invention realizes the simulation of the cable flexible joint manufacturing process using a small flat sample under laboratory conditions, thereby completing the optimization of key process parameters in the cable flexible joint processing process, greatly reducing the manpower and material costs of obtaining the optimal process parameters, improving work efficiency, and having important significance for the study of the insulation interface morphology and electrical properties of the cable flexible joint;
[0050] (3) The parameters to be optimized selected by the present invention correspond one-to-one to the process parameters in the manufacturing process of the cable flexible joint, and are all key process parameters. These process parameters have a direct impact on the degree of fusion of the insulation interface and the degree of aging of the primary insulation, and thus determine the insulation level of the composite insulation. The optimization of these parameters is of great significance to the processing quality of the cable flexible joint;
[0051] (4) The present invention aims at the problems that are easy to occur in the process of flexible joint processing, such as cavities at the insulation interface, the degree of primary insulation aging and unqualified thermal extension of restored insulation. It proposes to use local discharge, cavity size distribution at the interface, carbonyl index CI, thermal elongation and permanent elongation as evaluation indicators for characterization. It is targeted and can feedback and optimize the process parameters based on the results obtained from the corresponding tests. It can obtain a set of preferred values of the process parameters, and the evaluation standards can be modified according to the electrical properties of the samples corresponding to this set of parameters to obtain parameters with better performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 It is a schematic flow chart of a parameter optimization method for cable flexible joint insulation repair processing of the present invention;
[0053] Figure 2 Schematic diagram of the upper mold structure of the mold for preparing a primary insulation specimen;
[0054] Figure 3 A schematic diagram of the lower mold structure of a mold for preparing a primary insulation specimen;
[0055] Figure 4 Schematic diagram of the structure when the mold is closed for preparing a primary insulation sample;
[0056] Figure 5 A schematic diagram of the structure of the device for restoring insulation shaping;
[0057] Figure 6 It is a schematic diagram of the structure of a flat-plate composite insulation specimen;
[0058] In the figure, 1-1-top plate, 1-2-table, 1-3-storage trough, 1-4-positioning hole, 2-1-bottom plate, 2-2-side plate, 2-3-overflow trough, 3-positioning pin, 5-mold cavity, 6-upper heating plate, 6-1-injection port, 6-2-discharge port, 7-lower heating plate, 8-disposable insulation sample. DETAILED DESCRIPTION
[0059] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0060] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0061] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0062] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art. Specific implementation method one:
[0064] Reference Figure 1 As shown, a parameter optimization method for cable flexible joint insulation repair processing, the method comprises the following steps:
[0065] (1) Determine the initial process parameters and prepare an insulating sample;
[0066] (2) Performing injection molding and molding to restore the insulation of the primary insulation sample to obtain an insulation repair sample;
[0067] (3) The obtained insulation repair samples are evaluated by qualitative evaluation index I and quantitative evaluation index I in turn, and the uncross-linked composite insulation samples and the preferred process parameters of the injection molding process, the molding temperature T a and molding pressure P a ;
[0068] (4) performing secondary insulation crosslinking on the uncrosslinked composite insulation sample to obtain a crosslinked composite insulation sample;
[0069] (5) The obtained cross-linked composite insulation sample is optimized in turn with respect to qualitative evaluation index II, qualitative evaluation index I, quantitative evaluation index I and quantitative evaluation index II to obtain the secondary insulation sample and the cross-linking temperature T of the optimal process parameter of the cross-linking process. b , cross-linking pressure P b and cross-linking time t b ;
[0070] (6) Evaluate the obtained secondary insulation sample according to the quantitative evaluation index II. If the sample meets the qualitative evaluation index II, continue to evaluate the quantitative evaluation index III. If the sample does not meet the qualitative evaluation index II, repeat step (5) until the secondary insulation sample meets the qualitative evaluation index II.
[0071] (7) If the secondary insulation sample meets the evaluation of quantitative evaluation index III, the parameter number plastic temperature T for cable flexible joint insulation repair processing is obtained. a , Molding pressure P a , cross-linking temperature T b , cross-linking pressure P b and cross-linking time t b ;
[0072] If the secondary insulation sample does not meet the evaluation of quantitative evaluation index III, re-formulate qualitative evaluation index I, quantitative evaluation index I, qualitative evaluation index II and quantitative evaluation index II, and repeat steps (1) to (6) until the evaluation of quantitative evaluation index III is met.
[0073] In this way, the physical and chemical defects that lead to the degradation of the electrical performance of the flexible joint are taken as the starting point, and they are characterized, and evaluation criteria are set to optimize the factors that lead to these defects, that is, the process parameters in the processing of the flexible joint.
[0074] The flexible joint processing process can be divided into two stages: In the stage of restoring insulation molding, since the temperature of restoring insulation molding is low, it is difficult to age the primary insulation in a short time. Therefore, chemical defects caused by aging are not considered in (3), and only physical defects occurring during the molding process are optimized. During the molding process, too low molding temperature and molding pressure will cause micropores to appear on the insulation interface formed by the primary insulation and the restored insulation. These micropores in the insulator will cause local discharge inside the insulation under high electric field, accelerate the aging of the insulation, and reduce the insulation strength. Therefore, local discharge and micropore size are selected as evaluation indicators in (3), and local discharge quantity, X-ray flaw detection and computer tomography (Micro-CT) are used as characterization methods. Ideally, there should be no obvious local discharge inside the sample. The reference standard GB / T-11017.1-2014 sets the local discharge quantity standard as 5Pc. The reference standard GB / T 18890.1-2015 sets the micropore size and distribution at the insulation interface as no micropores larger than 0.05mm.
[0075] In the cross-linking stage, due to the high cross-linking temperature, the chemical defects caused by the aging of the primary insulation need to be considered at this stage. In addition, since the by-products of the cross-linking process exist in the form of gas, the influence of micropores at the interface still needs to be considered. Therefore, the cross-linking stage needs to consider parameter optimization for physical defects and chemical defects. The factors affecting the insulation interface defects in the cross-linking stage are mainly the cross-linking temperature, cross-linking pressure and cross-linking time. In the optimization process, the initial values of the three parameters are set, and the three parameters are optimized in turn. Considering that the physical defects of the interface are greatly affected by temperature and pressure, and the chemical defects are greatly affected by temperature and time, the temperature parameters should be determined first to avoid the coupling of the pressure parameters and the time parameters. After the temperature parameters are determined, the pressure parameters and time parameters can be optimized.
[0076] Considering that the cable insulation should have sufficient cross-linking degree to ensure the mechanical properties of the material, and the cross-linking degree of the insulation layer is strongly correlated with the cross-linking temperature, in order to determine the temperature parameters, thermal elongation and permanent elongation are used as evaluation indicators; after the temperature parameters are determined, the factors that cause physical defects in the insulation interface, namely the cross-linking pressure, are optimized, and the evaluation criteria used are the same as those in the molding stage; then the time parameters are optimized. In the cross-linking stage, in order to ensure that the material has sufficient cross-linking degree, the cross-linking temperature is high. If the cross-linking time is too long, it will cause excessive aging of the primary insulation to form chemical defects and reduce the insulation capacity. The aging of cross-linked polyethylene will produce C=O, so the carbonyl index CI is used as the evaluation standard.
[0077] In addition, after all three parameters are determined, a thermal extension test is still required to determine whether the sample prepared under this set of parameter conditions has sufficient cross-linking degree. If so, the electrical properties test can be carried out. Otherwise, this set of parameters should be used as the initial value and the cross-linking temperature, cross-linking pressure and cross-linking time should be optimized again.
[0078] The electrical performance of the flexible joint is the most important factor in determining whether it can operate stably. Therefore, after completing the parameter optimization, it is still necessary to determine whether the sample produced under the process conditions of this set of parameters has sufficient insulation performance. Therefore, the two-parameter Weibull distribution parameters of the AC and DC breakdown field strengths, namely the characteristic breakdown field strength and the shape parameter, are selected as the evaluation criteria. The specific value of the characteristic breakdown field strength should be determined according to the application voltage level of the flexible joint corresponding to the optimized parameters. The shape parameter represents the dispersion of the breakdown field strength. The larger the shape parameter, the more concentrated the breakdown field strength, which means the more uniform the material. Therefore, the shape parameter should be as large as possible, and its minimum value should not be less than 5 to ensure the reliability of the experimental results. Specific implementation method 2:
[0080] The initial process parameters in (1) include the size of the primary insulation sample, the type of insulation material, the shape and angle of the insulation interface; the method for preparing the primary insulation sample is: filling the insulation material into the mold, hot pressing it in a flat vulcanizer, and then heating it for cross-linking. The other process steps and parameter settings are the same as those in the specific method 1. Specific implementation method three:
[0082] (2) The preparation method of the insulation repair sample is as follows: the primary insulation sample is installed in the insulation recovery molding device for injection molding and molding of the insulation recovery to obtain the insulation repair sample. The other process steps and parameter settings are the same as those of the specific method 1. Specific implementation method four:
[0084] Qualitative evaluation index I is that the partial discharge is less than 5pC or the micropore size at the interface between the insulation repair sample and the primary insulation sample is less than 0.05mm. The other process steps and parameter settings are the same as the specific method 1. Qualitative evaluation index I can choose partial discharge test, refer to the standard GB / T-11017.1-2014, the partial discharge standard is 5Pc. If the test result meets the requirement of partial discharge <5pC, then enter the quantitative evaluation standard I, otherwise the mold heating temperature should be increased in the insulation recovery molding stage, and the test should be repeated. In order to avoid pre-crosslinking, the insulation recovery molding temperature cannot exceed 120℃. When the molding temperature T a If it cannot be increased, the molding pressure P can be increased. a Qualitative evaluation index I can also be tested by X-ray flaw detection technology, and the statistical reference standard GB / T 18890.1-2015 of the distribution of micropores of different sizes in the interface is tested.
[0085] In (3), when the insulation repair specimen does not meet the qualitative evaluation index I, the plastic temperature T a , until the plastic temperature reaches 120℃. If the plastic temperature reaches 120℃ and still does not meet the qualitative evaluation index I, then increase the plastic pressure P a ;
[0086] In (5), when the cross-linked composite insulation sample does not meet the qualitative evaluation index I, the cross-linking pressure P is increased. b . Specific implementation method five:
[0088] Quantitative evaluation index I is the number of micropores with a size less than 0.05 mm at the interface between the insulation repair specimen and the primary insulation specimen, and the number of micropores with a size greater than 0.025 mm per 10 cm. 3 The number of cavities in the interface is less than 18, and the other process steps and parameter settings are the same as those in the specific method 1. The quantitative evaluation index I is the distribution of cavity size at the interface between the insulation repair sample and the primary insulation sample. The prepared insulation repair sample is subjected to computer tomography (Micro-CT), the insulation interface morphology is observed, and the distribution of cavities of different sizes in the interface is statistically analyzed. With reference to GB / T 18890.1-2015, if the test results meet the following requirements: the size of the micropores at the interface between the insulation repair sample and the primary insulation sample is less than 0.05 mm, and the micropores with a size greater than 0.025 mm are located in every 10 cm 3 If the number of crosslinks is less than 18, the insulation restoration crosslinking stage is entered. Otherwise, when the insulation repair specimen does not meet the quantitative evaluation index I in (3), the molding pressure P is increased. a In (5), when the cross-linked composite insulation sample does not meet the quantitative evaluation index I, the cross-linking pressure P is increased. b . Specific implementation method six:
[0090] Qualitative evaluation index II is that the thermal elongation of the cross-linked composite insulation sample is ≤175% and the permanent elongation is ≤15%. The other process steps and parameter settings are the same as the specific method one. Qualitative evaluation index II is the thermal elongation test result of the cross-linked composite insulation sample, that is, the thermal elongation and permanent elongation of the material; the test is carried out with reference to the standard GB / T 2951.21-2008. If the test results meet the following requirements: the maximum elongation under load is ≤175%, and the maximum permanent elongation after cooling is ≤15%, then enter the next stage. Otherwise, in (5), when the cross-linked composite insulation sample does not meet the qualitative evaluation index II, increase the cross-linking temperature T b . Specific implementation method seven:
[0092] Quantitative evaluation index II is that the change in the carbonyl index of the primary insulation sample after injection molding, forming and cross-linking of restored insulation is less than 80% (it is generally believed that the carbonyl index of XLPE is less than 0.8 for no aging, 0.8-1.5 for mild aging, and greater than 1.5 for severe aging. During the process of restoring the insulation of the flexible joint, the primary insulation should not be obviously aged. The change in the carbonyl index here refers to mild aging and is set to 80%. When the final result cannot meet the electrical performance test, the change in the carbonyl index in this standard should be further reduced). Other process steps and parameter settings are the same as specific method one. Quantitative evaluation index II is the change in the carbonyl index of the primary insulation sample after injection molding and cross-linking of the restored insulation. The cross-linked composite insulation sample is subjected to a micro-infrared spectroscopy test (Micro-FTIR) to calculate the carbonyl index CI. Before the experiment, the primary insulation sample prepared in step (1) is subjected to a micro-infrared spectroscopy test and the carbonyl index CI-a is calculated. The degree of change in the carbonyl index of the primary insulation sample during the restoration of insulation cross-linking is used to characterize the aging degree of the primary insulation. The change in the carbonyl index of the primary insulation sample should be less than the set standard value. If the test result meets the requirements, proceed to the next stage. Otherwise, in (5), when the cross-linked composite insulation sample does not meet the quantitative evaluation index II, reduce the cross-linking time t b . Specific implementation eight:
[0094] The quantitative evaluation index III is that the ratio of the AC and DC characteristic breakdown field strength of the cross-linked composite insulation sample to the AC and DC characteristic breakdown field strength of the primary insulation sample is higher than 80%, and the shape parameter of the cross-linked composite insulation sample is greater than 5, and the other process steps and parameter settings are the same as the specific method 1. The quantitative evaluation index III is the two-parameter Weibull distribution parameter of the AC and DC breakdown field strength of the cross-linked composite insulation sample measured based on the cylindrical electrode, that is, the characteristic breakdown field strength and the shape parameter; before the test, the AC and DC breakdown field strength of the insulating material used for the primary insulation after cross-linking should be tested and statistically analyzed, and the sample should be evaluated with the characteristic breakdown field strength and shape parameter as evaluation indicators. Under ideal conditions, the characteristic breakdown strength and shape parameters of the cross-linked composite insulation sample should be similar to those of the primary insulation sample. Taking into account that the high temperature during the process of restoring the insulation cross-linking will cause a certain degree of aging of the primary insulation sample in the cross-linked composite insulation sample, the AC and DC characteristic breakdown field strength of the cross-linked composite insulation sample should not be less than 80% of the AC and DC characteristic breakdown field strength of the primary insulation, and the shape parameter should be greater than 5 to ensure the reliability of the test results. According to the above indicators, if the test results of the cross-linked composite insulation sample meet the requirements, the preferred process parameters are obtained, otherwise it means that the evaluation indicators for the restoration of insulation cross-linking parameters are too loose, and the evaluation standards should be appropriately improved to select samples with better performance for testing. Specific implementation method nine:
[0096] The primary insulation sample preparation mold includes an upper mold and a lower mold. The upper mold and the lower mold are axisymmetric solid metal structures. When the molds are closed, the two molds are coaxially fitted through the cooperation of the positioning pins and the positioning holes to form a mold cavity.
[0097] The upper die is an integrated structure consisting of a top plate and a round table, and a material storage trough is provided on the top surface of the round table;
[0098] The lower mold is an integrated structure consisting of a bottom plate and a side plate. There is a certain inclination angle between the side plate and the bottom plate, and an overflow groove is provided on the side plate. Specific implementation method ten:
[0100] The insulation recovery molding device comprises an upper heating plate, a lower heating plate and a disposable insulation sample located between the upper heating plate and the lower heating plate; the upper heating plate is provided with an injection molding port.
[0101] Example 1
[0102] Step 1:
[0103] Select the required cross-linkable polyethylene granules, determine the shape and angle of the simulated interface, and select the mold of the corresponding size to prepare the primary insulation sample. The specific preparation process is to fill the cross-linkable polyethylene granules into the mold, hot press molding in a flat vulcanizer at 110°C, and then cross-link for 30 minutes at 175°C and 15MPa to obtain the primary insulation sample. Subsequently, the primary insulation sample was subjected to microscopic infrared spectroscopy test and breakdown field strength test, and the carbonyl index CI of the primary insulation sample and the Weibull distribution parameters of the breakdown field strength were analyzed.
[0104] The mold used for preparing the primary insulation sample includes an upper mold and a lower mold. The upper mold and the lower mold are axially symmetrical solid metal structures. When the molds are closed, the two molds are coaxially fitted through the cooperation of the positioning pins 3 and the positioning holes 1-4 to form a mold cavity 5. Figure 4 As shown. Figure 2 As shown, the upper mold is an integrated structure consisting of a top plate 1-1 and a truncated cone 1-2. A material storage trough 1-3 is provided on the top surface of the truncated cone 1-2, and a positioning hole 1-4 is provided on the diagonal of the top plate 1-1. The truncated cone 1-2 is a standard truncated cone with different radii or a quasi-truncated cone with a curved generatrix according to the shape and angle of the required simulated interface. Figure 3 As shown, the lower mold is an integrated structure consisting of a bottom plate 2-1 and a side plate 2-2. There is a certain inclination angle between the side plate 2-2 and the bottom plate 2-1, and a semicircular overflow groove 2-3 is provided on the side plate. A positioning hole 1-4 is opened on the diagonal of the bottom plate 2-1.
[0105] Step 2:
[0106] The insulation repair specimens are prepared by using an insulation extrusion device and an insulation recovery molding device, such as Figure 5As shown, the recovery insulation molding mold includes an upper heating plate 6, a lower heating plate 7 and a disposable insulation sample 8 located between the upper heating plate and the lower heating plate. The upper heating plate 6 is provided with an injection port 6-1. An insulation extrusion mechanism is used to inject the viscous recovery insulation material into the recovery insulation molding mold through the injection port 6-1. Specifically, the insulation extrusion device and the recovery insulation molding device are preheated first. When the minimum temperature of the cone surface of the disposable insulation sample exceeds 110°C and the maximum temperature is less than 120°C, the mold heating temperature T is recorded at this time. a , the same cross-linkable polyethylene granules as those used to prepare the disposable insulation sample are filled into the insulation extrusion device for injection molding; after the injection molding is completed, nitrogen is introduced through the injection port 6-1 opened on the upper heating plate 6 and in conjunction with the air pipe quick connector 6-3 to provide air pressure to help molding. In order to maintain air tightness and not damage the primary insulation, the nitrogen pressure here should be less than the pressure provided by the flat vulcanizer, and the pressure provided by the flat vulcanizer should be less than the yield strength of the primary insulation sample at this temperature. At this time, the nitrogen pressure is recorded as P a ; A flat composite insulation specimen is obtained which is formed but not cross-linked, such as Figure 6 shown.
[0107] Step 3:
[0108] The flat plate-shaped composite insulation specimen obtained in step 2 above, which was molded but not cross-linked, was evaluated.
[0109] First, the qualitative evaluation index I is used for evaluation. The qualitative evaluation index I is the partial discharge amount or X-ray flaw detection. In the recovery insulation molding stage, due to the low temperature or pressure, the melt viscosity of the recovery insulation will be low, resulting in large micropores on the insulation interface formed by the primary insulation and the recovery insulation, resulting in defects at the interface. The partial discharge or micropore size caused by the micropores can be observed by using partial discharge or X-ray detection. Based on this, the temperature of the recovery insulation molding stage is optimized until the partial discharge amount or micropore size meets the qualitative evaluation index I, and then enter the next stage. The recovery insulation molding temperature T is recorded at this time. a is the preferred value.
[0110] Then, quantitative evaluation index I is used for evaluation. Quantitative evaluation index I is the cavity size distribution at the interface between primary insulation and recovery insulation in the flat composite insulation specimen. Tiny cavities will be generated at the interface between recovery insulation and primary insulation. In the recovery insulation stage, the formation of cavities is mainly related to the material molding temperature and pressure. Referring to GB / T 18890.1-2015, the cavity size distribution at the interface formed by primary insulation and recovery insulation should meet the following requirements: no micropores larger than 0.05 mm, and micropores larger than 0.025 mm per 10 cm 3There should be no more than 18 in the insulation. If the test results meet the requirements, proceed to the next stage. If the test results do not meet the requirements, increase the gas pressure P during the molding process by 0.1MPa as a unit pressure. a , until the cavity size distribution at the insulation interface meets the requirements, and the mold pressure at this time is recorded as P a is the preferred value.
[0111] Step 4:
[0112] The molded but uncrosslinked flat composite insulation specimen was subjected to crosslinking treatment using the insulation recovery molding device. The crosslinking heating temperature was set to 120°C and recorded as T b , the mold pressure is the same as the mold pressure P selected in step 3 a Same, denoted as P b Under this condition, the cross-linking time is recorded as t b , t b A larger value should be selected within the acceptable range. The cooled composite sample is degassed in a vacuum environment at 80°C for 12 hours, and the obtained cross-linked composite insulation sample is optimized in turn through subsequent indicators.
[0113] Step 5:
[0114] The cross-linked composite insulation sample obtained in step 2 is optimized in turn with respect to qualitative evaluation index II, qualitative evaluation index I, quantitative evaluation index I and quantitative evaluation index II to obtain a secondary insulation sample and the cross-linking temperature T of the cross-linking process. b , cross-linking pressure P b and cross-linking time t b .
[0115] The specific process is as follows:
[0116] Qualitative evaluation index II is the result of the insulation recovery heat extension test after cross-linking, that is, the thermal elongation and permanent elongation of the material; refer to the standard GB / T 2951.21-2008 for testing. If the test results meet the following requirements: the maximum elongation under load is ≤175%, and the maximum permanent elongation after cooling is ≤15%, then enter the next stage, otherwise the insulation recovery cross-linking temperature T should be increased. b , retest until the thermal elongation meets the standard.
[0117] Qualitative evaluation index I is partial discharge or X-ray flaw detection. In the stage of restoring insulation cross-linking, AC reaction will produce gas, which may cause micropores to appear on the insulation interface formed by primary insulation and restored insulation, resulting in defects at the interface. By using partial discharge or X-ray detection, the partial discharge or micropore size caused by the micropores can be observed. Based on this, the pressure in the stage of restoring insulation cross-linking is optimized until the partial discharge or micropore size meets the qualitative evaluation standard I and enters the next stage.
[0118] Quantitative evaluation index I is the cavity size distribution at the interface between the primary insulation and the restored insulation in the cross-linked composite insulation sample; tiny cavities will be generated at the interface between the restored insulation and the primary insulation. During the restoration insulation stage, the formation of cavities is mainly related to the material molding temperature and pressure. Referring to GB / T 18890.1-2015, the cavity size distribution at the interface formed by the primary insulation and the restored insulation should meet the following requirements: no micropores larger than 0.05 mm, and micropores larger than 0.025 mm per 10 cm 3 There should be no more than 18 in the insulation. If the test results meet the requirements, the quantitative evaluation index II is carried out. If the test results do not meet the requirements, the mold pressure P during the cross-linking process is increased by 0.1MPa as a unit pressure. b (The nitrogen pressure is kept equal to the mold pressure) until the cavity size distribution at the insulation interface meets the requirements. The mold pressure at this time is recorded as P b is the preferred value.
[0119] The quantitative evaluation index II is the change of the primary insulation carbonyl index CI. In the stage of restoring insulation crosslinking, high temperature will cause a certain degree of aging of the primary insulation. The present invention uses the change of the primary insulation carbonyl index CI to evaluate the aging degree of the primary insulation. If the composite insulation sample does not meet the evaluation standard, the crosslinking time is reduced by 5 minutes as a unit time. When the composite insulation sample meets the quantitative evaluation index II, a set of preferred T b , P b ,t b The composite insulation molded under this parameter is evaluated by qualitative evaluation index II. If the test passes, it will enter the next stage. Otherwise, the cross-linking temperature should be increased by 5℃ as a unit temperature, and T b , P b ,t b Make optimizations.
[0120] Quantitative evaluation index III is the two-parameter Weibull distribution parameter of the AC and DC breakdown field strength measured based on the cylindrical electrode, namely, the characteristic breakdown field strength and the shape parameter; the composite specimens that meet the qualitative evaluation index II are subjected to AC and DC breakdown field strength tests. Considering that the high temperature during the insulation restoration molding and cross-linking process will cause a certain degree of aging of the primary insulation in the composite specimen, the AC and DC characteristic breakdown field strength of the composite specimen should meet the requirements of the cable insulation layer breakdown field strength under the working voltage level of the flexible joint, and the shape parameter should be greater than 5. According to the above indicators, if the test results of the composite specimens meet the requirements, a set of preferred process parameters is obtained. Otherwise, it means that the evaluation indicators for the insulation restoration cross-linking parameters are too loose, and the evaluation standards should be appropriately improved to select specimens with better performance for testing.
[0121] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A parameter optimization method for cable flexible joint insulation repair processing, It is characterized in that include: (1) Determine the initial process parameters and prepare an insulating sample; (2) Performing injection molding and molding to restore the insulation of the primary insulation sample to obtain an insulation repair sample; (3) The obtained insulation repair samples are evaluated by qualitative evaluation index I and quantitative evaluation index I in turn, and the uncross-linked composite insulation samples and the optimal process parameters of the injection molding process, the molding temperature T a and molding pressure P a ; (4) performing secondary insulation crosslinking on the uncrosslinked composite insulation sample to obtain a crosslinked composite insulation sample; (5) The obtained cross-linked composite insulation sample is optimized in turn with respect to qualitative evaluation index II, qualitative evaluation index I, quantitative evaluation index I and quantitative evaluation index II to obtain the secondary insulation sample and the cross-linking temperature T of the optimal process parameter of the cross-linking process. b , cross-linking pressure P b and cross-linking time t b ; (6) Evaluate the obtained secondary insulation sample according to the quantitative evaluation index II. If the sample meets the qualitative evaluation index II, continue to evaluate the quantitative evaluation index III. If the sample does not meet the qualitative evaluation index II, repeat step (5) until the secondary insulation sample meets the qualitative evaluation index II. (7) If the secondary insulation sample meets the evaluation of quantitative evaluation index III, the parameter number plastic temperature T for cable flexible joint insulation repair processing is obtained. a , Molding pressure P a , cross-linking temperature T b , cross-linking pressure P b and cross-linking time t b ; If the secondary insulation sample does not meet the evaluation of quantitative evaluation index III, re-formulate qualitative evaluation index I, quantitative evaluation index I, qualitative evaluation index II and quantitative evaluation index II, and repeat steps (1) to (6) until the evaluation of quantitative evaluation index III is met.
2. The method according to claim 1, It is characterized in that (1) The initial process parameters include the size of the primary insulation sample, the type of insulation material, and the shape and angle of the insulation interface; The method for preparing a primary insulation sample is as follows: filling the insulation material into a mold, hot pressing it in a flat vulcanizer, and then heating and cross-linking it.
3. The method according to claim 1, It is characterized in that (2) The preparation method of the insulation repair sample is as follows: the primary insulation sample is installed in an insulation recovery molding device for injection molding and molding of insulation recovery to obtain the insulation repair sample.
4. The method according to claim 1, It is characterized in that Qualitative evaluation index I is that the partial discharge is less than 5pC or the micropore size at the interface between the insulation repair sample and the primary insulation sample is less than 0.05mm; In (3), when the insulation repair specimen does not meet the qualitative evaluation index I, the plastic temperature T a , until the plastic temperature reaches 120℃. If the plastic temperature reaches 120℃ and still does not meet the qualitative evaluation index I, then increase the plastic pressure P a ; In (5), when the cross-linked composite insulation sample does not meet the qualitative evaluation index I, the cross-linking pressure P is increased. b .
5. The method according to claim 1, It is characterized in that Quantitative evaluation index I is the number of micropores with a size less than 0.05 mm at the interface between the insulation repair specimen and the primary insulation specimen, and the number of micropores with a size greater than 0.025 mm per 10 cm. 3 Less than 18; In (3), when the insulation repair specimen does not meet the quantitative evaluation index I, the molding pressure P is increased. a ; In (5), when the cross-linked composite insulation sample does not meet the quantitative evaluation index I, the cross-linking pressure P is increased. b .
6. The method according to claim 1, It is characterized in that Qualitative evaluation index II is that the thermal elongation of the cross-linked composite insulation sample is ≤175% and the permanent elongation is ≤15%; In (5), when the cross-linked composite insulation sample does not meet the qualitative evaluation index II, the cross-linking temperature T b .
7. The method according to claim 1, It is characterized in that Quantitative evaluation index II is that the change in carbonyl index of the primary insulation sample after injection molding and cross-linking of restored insulation is less than 80%; In (5), when the cross-linked composite insulation sample does not meet the quantitative evaluation index II, the cross-linking time t b .
8. The method according to claim 1, It is characterized in that The quantitative evaluation index III is that the ratio of the AC and DC characteristic breakdown field strength of the cross-linked composite insulation sample to the AC and DC characteristic breakdown field strength of the primary insulation sample is higher than 80%, and the shape parameter of the cross-linked composite insulation sample is greater than 5.
9. A primary insulation sample preparation mold used in the method according to claim 1, It is characterized in that It includes an upper mold and a lower mold, the upper mold and the lower mold are axially symmetrical solid metal structures, and when the mold is closed, the two molds are coaxially fitted through the cooperation of the positioning pins and the positioning holes to form a mold cavity; The upper die is an integrated structure consisting of a top plate and a round table, and a material storage trough is provided on the top surface of the round table; The lower die is an integrated structure consisting of a bottom plate and a side plate. There is a certain inclination angle between the side plate and the bottom plate, and an overflow groove is provided on the side plate.
10. A recovery insulation molding device used in the method of claim 1, It is characterized in that The invention comprises an upper heating plate, a lower heating plate and a disposable insulating sample located between the upper heating plate and the lower heating plate. The upper heating plate is provided with an injection molding port.
Citation Information
Patent Citations
Experimental high-voltage XLPE cable flexible joint insulating layer interface simulation device and method
CN113146932A
Method for optimizing field intensity concentration of XLPE cable factory joint stress cone
CN113255095A
Method and device for evaluating and optimizing continuous extrusion processing characteristics of high-voltage cable insulating material
CN115718040A
Formula design and optimization method for crosslinked polyethylene insulating material of high-voltage alternating-current cable
CN116625427A
End determination method and device of cable joint, storage medium and electronic device
CN118153379A