Light-transmitting conductive layer and light-transmitting conductive sheet
By controlling the grain diameter and the structure of the base material layer in the translucent conductive layer, the problem of poor flexibility in the prior art is solved, and a translucent conductive layer with low resistance and excellent flexibility is achieved, which is suitable for optical applications. device.
Patent Information
- Application Number
- CN202410371852.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
When the existing transparent conductive film is bent, due to the large average diameter of the crystal grains, stress concentration causes cracks and poor bending properties, making it difficult to meet the requirements for low resistance and excellent bending properties.
A translucent conductive layer is designed, the average diameter of the crystal grains is 105nm or less, and the content of crystal grains with a maximum diameter of 110nm or more is less than 70%. By forming an optical adjustment layer and a hardening layer in the thickness direction of the base material layer, The coating combines sputtering and heat treatment to form a light-transmitting conductive layer with low resistance and excellent flexibility.
A light-transmitting conductive layer with low resistance and excellent flexibility is realized, which is suitable for applications such as touch panels in optical devices, and improves the mechanical strength and transparency of the conductive layer.
Smart Images

Figure CN118737527A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a light-transmitting conductive layer and a light-transmitting conductive sheet. Background Art
[0002] Translucent conductive sheets having a transparent substrate and a transparent conductive layer in this order in the thickness direction have long been known. The translucent conductive layer formed of indium tin oxide (ITO) can be used as a conductor film for patterning transparent electrodes in various devices such as liquid crystal displays, touch panels, and optical sensors.
[0003] On the other hand, from the viewpoint of improving the response speed of the touch panel, the demand for a light-transmitting conductive sheet having a light-transmitting conductive layer (ITO layer) with low resistance is increasing. Therefore, it is proposed to increase the average grain diameter of the grains contained in the light-transmitting conductive layer and reduce the resistance thereof (for example, refer to the following patent document 1).
[0004] Existing patent literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2013-152827 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] On the other hand, in recent years, transparent conductive films are required to have low resistance and excellent bendability.
[0009] However, in the light-transmitting conductive layer of Patent Document 1, since the average grain diameter of the crystal grains included is large, when the light-transmitting conductive layer is bent, a large stress is applied to the bent portion, thereby generating cracks. In other words, there is a problem of low bendability.
[0010] The present invention provides a light-transmitting conductive layer and a light-transmitting conductive sheet having low resistance and excellent bendability.
[0011] Solutions for solving problems
[0012] The present invention [1] comprises a translucent conductive layer, which comprises a first main surface and a second main surface opposite to the first main surface in the thickness direction, wherein the thickness of the translucent conductive layer exceeds 50 nm, the translucent conductive layer comprises crystal grains, and the average grain diameter of the crystal grains is less than 105 nm.
[0013] The present invention [2] comprises the light-transmitting conductive layer described in the above [1], wherein the crystal grains include crystal grains having a maximum crystal grain diameter of 110 nm or more.
[0014] The present invention [3] comprises the light-transmitting conductive layer described in [1] or [2] above, wherein the content ratio of crystal grains having a crystal grain diameter of 100 nm or more is 70% or less relative to the total number of the crystal grains.
[0015] The present invention [4] includes a translucent conductive sheet comprising: the translucent conductive layer according to any one of [1] to [3] above, and a substrate layer on the first main surface and / or the second main surface side of the translucent conductive layer.
[0016] Effects of the Invention
[0017] The present invention is a light-transmitting conductive layer having a first main surface and a second main surface opposite to the first main surface in the thickness direction, wherein the thickness of the light-transmitting conductive layer exceeds 50 nm, and the light-transmitting conductive layer has crystal grains, and the average crystal grain diameter of the crystal grains is less than 105 nm. Therefore, the light-transmitting conductive layer has low resistance and excellent bendability.
[0018] The light-transmitting conductive sheet of the present invention includes the light-transmitting conductive layer of the present invention, and therefore has low resistance and excellent bendability. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A cross-sectional view showing one embodiment of the light-transmitting conductive sheet of the present invention.
[0020] Figure 2 This is a schematic diagram showing one embodiment of a method for producing a light-transmitting conductive layer and a light-transmitting conductive sheet of the present invention. Figure 2 A in the figure represents a step of preparing a transparent substrate in the first step. Figure 2 B represents a step of forming an optical adjustment layer on one surface in the thickness direction of the transparent substrate in the first step. Figure 2 C represents a step of forming a hard coating layer on the other surface in the thickness direction of the transparent substrate in the first step. Figure 2 D represents a second step of disposing a light-transmitting conductive layer on one surface in the thickness direction of the base layer. Figure 2 E represents a third step of heating the light-transmitting conductive layer.
[0021] Description of Reference Numerals
[0022] 1Transparent conductive sheet
[0023] 2Transparent conductive layer
[0024] 3. Base material layer
[0025] 21 First main surface
[0026] 22 Second main surface DETAILED DESCRIPTION
[0027] refer to Figure 1, describing an embodiment of the light-transmitting conductive layer and the light-transmitting conductive sheet of the present invention.
[0028] Figure 1 In the figure, the up-down direction on the paper is the up-down direction (thickness direction, first direction). The upper side on the paper is the upper side (one side in the thickness direction, one side in the first direction). In addition, the lower side on the paper is the lower side (the other side in the thickness direction, the other side in the first direction). In addition, the left-right direction and the depth direction on the paper are the plane directions orthogonal to the up-down direction. Specifically, the directions of the figures are based on the arrows.
[0029] <Light-transmitting conductive sheet>
[0030] like Figure 1 As shown, the light-transmitting conductive sheet 1 is formed into a sheet shape (including a film shape) with a specified thickness, extends in a specified direction (front-back direction and left-right direction, i.e., surface direction) orthogonal to the up-down direction (thickness direction), and has a flat upper surface (one side in the thickness direction) and a flat lower surface (the other side in the thickness direction). The light-transmitting conductive sheet 1 is, for example, a component of a touch panel and a dimming panel included in an optical device, i.e., it is not an optical device. That is, the light-transmitting conductive sheet 1 is a component for making an optical device, etc., and does not include an image display element such as an LCD module, a light source such as an LED, etc. It is a component that circulates independently and is an industrially usable device.
[0031] In addition, the light-transmitting conductive sheet 1 includes a light-transmitting conductive layer 2 and a substrate layer 3. It should be noted that the light-transmitting conductive layer 2 includes a first principal surface 21 and a second principal surface 22 opposite to the first principal surface 21 in the thickness direction. That is, the light-transmitting conductive sheet 1 includes the light-transmitting conductive layer 2 and the substrate layer 3 on the first principal surface 21 and / or second principal surface 22 side of the light-transmitting conductive layer 2. Specifically, the light-transmitting conductive sheet 1 includes the light-transmitting conductive layer 2 and the substrate layer 3 on the second principal surface 22 side (the other side in the thickness direction) of the light-transmitting conductive layer 2.
[0032] The thickness of the light-transmitting conductive sheet 1 is, for example, 300 μm or less, preferably 200 μm or less, more preferably 150 μm or less, and, for example, 20 μm or more, preferably 40 μm or more, more preferably 60 μm or more, further preferably 80 μm or more.
[0033] <Base material layer>
[0034] The base material layer 3 ensures the mechanical strength of the light-transmitting conductive sheet 1 .
[0035] The base material layer 3 has a sheet shape (including a film shape).
[0036] The substrate layer 3 is arranged on the first principal surface 21 and / or the second principal surface 22 side of the translucent conductive layer 2. The substrate layer 3 is preferably arranged on the second principal surface 22 side (the other side in the thickness direction) of the translucent conductive layer 2. Specifically, the substrate layer 3 is arranged on the entire surface of the second principal surface 22 of the translucent conductive layer 2 in a manner that contacts the second principal surface 22 of the translucent conductive layer 2.
[0037] The substrate layer 3 includes, for example, a transparent substrate 31 and, if necessary, a functional layer 32. The substrate layer 3 preferably includes a transparent substrate 31 and a functional layer 32 on one side in the thickness direction and / or the other side in the thickness direction of the transparent substrate 31. The substrate layer 3 more preferably includes a transparent substrate 31 and a functional layer 32 on one side in the thickness direction and the other side in the thickness direction of the transparent substrate 31.
[0038] The thickness of the base material layer 3 is, for example, 300 μm or less, preferably 200 μm or less, more preferably 150 μm or less, and, for example, 20 μm or more, preferably 40 μm or more, more preferably 60 μm or more, further preferably 80 μm or more.
[0039] [Transparent substrate]
[0040] The transparent base material 31 has flexibility and supports the light-transmitting conductive layer 2 .
[0041] The transparent base material 31 has a sheet shape (including a film shape).
[0042] The transparent base material 31 is formed of, for example, a polymer film, and therefore has excellent flexibility. In addition, when the transparent base material 31 is formed of a polymer film, the production efficiency of the light-transmitting conductive sheet 1 is excellent.
[0043] In addition, if the transparent substrate 31 is formed of a polymer film, it is sometimes necessary to reheat the translucent conductive sheet 1 (crystalline translucent conductive layer 2) from the perspective of providing the translucent conductive sheet 1 with dimensional stability, but the translucent conductive sheet 1 has excellent heating stability.
[0044] As the material of the polymer film, for example, polyester resin, (meth) acrylic resin, olefin resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin, polystyrene resin and norbornene resin can be listed. From the viewpoints of flexibility, heat resistance, mechanical strength, etc., the transparent substrate 31 preferably includes a polymer film formed of a polyester resin.
[0045] Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate, and preferably polyethylene terephthalate is used.
[0046] As a (meth)acrylic resin, polymethacrylate is mentioned, for example.
[0047] Examples of the olefin resin include polyethylene, polypropylene, and cycloolefin polymers.
[0048] The polymer films may be used alone or in combination of two or more.
[0049] The total light transmittance (JIS K 7375-2008) of the transparent base material 31 is, for example, 60% or more, preferably 80% or more, and more preferably 85% or more.
[0050] When the total light transmittance of the transparent base material 31 is equal to or greater than the above lower limit, the transparency of the transparent base material 31 is excellent.
[0051] The thickness of the transparent substrate 31 is, for example, 1 μm or more, preferably 10 μm or more, more preferably 50 μm or more, further preferably 80 μm or more, particularly preferably 100 μm or more, and is, for example, 300 μm or less, preferably 200 μm or less, more preferably 150 μm or less.
[0052] When the thickness of the transparent base material 31 is within the above range, the light-transmitting conductive sheet 1 can be made thinner and has excellent mechanical strength.
[0053] The thickness of the transparent base material 31 can be measured using, for example, a film thickness meter.
[0054] [Functional layer]
[0055] The functional layer 32 is disposed on one surface in the thickness direction and / or the other surface in the thickness direction of the transparent substrate 31. The functional layer 32 is preferably disposed on one surface in the thickness direction and the other surface in the thickness direction of the transparent substrate 31.
[0056] The functional layer 32 has a sheet shape (including a film shape).
[0057] Examples of the functional layer 32 include an anti-adhesion layer, an optical adjustment layer, and a hard coat layer, and preferably include an optical adjustment layer and a hard coat layer.
[0058] When the functional layer 32 is an optical adjustment layer and a hard coating layer, the substrate layer 3 includes, for example, a transparent substrate 31, a hard coating layer 33 on the other side in the thickness direction of the transparent substrate 31, and an optical adjustment layer on one side in the thickness direction of the transparent substrate 31. In other words, the substrate layer 3 includes the hard coating layer 33, the transparent substrate 31, and the optical adjustment layer 34 in this order toward one side in the thickness direction.
[0059] {Hard Coat Layer} The hard coat layer 33 is a scratch protection layer for making the light-transmitting conductive sheet 1 less susceptible to scratches.
[0060] The hard coating layer 33 is disposed on the other side in the thickness direction of the transparent substrate 31. Specifically, the hard coating layer 33 is disposed on the entire lower surface (the other side in the thickness direction) of the transparent substrate 31 in a manner that contacts the other side in the thickness direction of the transparent substrate 31. It should be noted that the hard coating layer 33 is the bottom layer of the light-transmitting conductive sheet.
[0061] It should be noted that Figure 1 In the embodiment, the hard coating layer 33 is disposed on the other side in the thickness direction of the transparent substrate 31, but it is not limited thereto. That is, the hard coating layer 33 may be disposed on one side in the thickness direction of the transparent substrate 31, or may be disposed in multiple layers. In addition, when the substrate layer 3 includes the hard coating layer 33 and the optical adjustment layer 34 described later in the same direction on one side or the other side in the thickness direction of the transparent substrate 31, the stacking order is not particularly limited.
[0062] The hard coating layer 33 is formed of, for example, a hard coating composition.
[0063] The hard coating composition contains, for example, a resin and contains particles as needed. That is, the hard coating layer 33 contains, for example, a resin and contains particles as needed.
[0064] Examples of the resin include thermoplastic resins and curable resins.
[0065] Examples of the thermoplastic resin include polyolefin resins.
[0066] Examples of the curable resin include acrylic resins, polyurethane resins, amide resins, silicone resins, epoxy resins, melamine resins, alkyd resins, siloxane polymers, and organosilane condensates, and preferably acrylic resins are used.
[0067] Examples of the curable resin include active energy ray-curable resins that are cured by irradiation with active energy rays (eg, ultraviolet rays and electron beams) and thermosetting resins that are cured by heating.
[0068] The resins may be used alone or in combination of two or more.
[0069] Examples of the particles include metal oxide fine particles and organic fine particles.
[0070] Examples of the material of the metal oxide fine particles include silicon dioxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide.
[0071] Examples of the material of the organic fine particles include polymethyl methacrylate, silicone, polystyrene, polyurethane, acrylic-styrene copolymer, benzoguanamine, melamine, and polycarbonate.
[0072] The particles may be used alone or in combination of two or more.
[0073] The hard coating composition contains, for example, a resin, preferably a curable resin, and more preferably an active energy ray-curable resin. Specifically, the hard coating composition contains an acrylic resin.
[0074] In addition, the hard coating composition may contain, for example, a thixotropy-imparting agent, a photopolymerization initiator, a filler (eg, organoclay), and a leveling agent at an appropriate ratio. The hard coating composition may also be diluted with a known solvent.
[0075] The formation of the hard coat layer 33 will be described in detail later. A diluted hard coat composition is applied to the other surface in the thickness direction of the transparent substrate 31 and dried as necessary. After drying, the hard coat composition is cured by, for example, irradiation with active energy rays.
[0076] Thus, the hard coating layer 33 is formed.
[0077] The thickness of the hard coating layer 33 is, for example, 0.1 μm or more, preferably 0.5 μm or more, more preferably 1 μm or more, and, for example, 10 μm or less, preferably 5 μm or less, more preferably 3 μm or less.
[0078] The thickness of the hard coating layer 33 can be determined by observing a cross section of the hard coating layer 33 using a scanning electron microscope (SEM), for example.
[0079] {Optical Adjustment Layer}
[0080] The optical adjustment layer 34 suppresses pattern visibility of the translucent conductive layer 2 and also suppresses reflection at the interface within the translucent conductive sheet 1 , and adjusts the optical properties (eg, refractive index) of the translucent conductive sheet 1 in order to ensure excellent transparency in the translucent conductive sheet 1 .
[0081] The optical adjustment layer 34 is disposed on one surface in the thickness direction of the transparent substrate 31. Specifically, the optical adjustment layer 34 is disposed on the entire upper surface (one surface in the thickness direction) of the transparent substrate 31 in a manner that contacts one surface in the thickness direction of the transparent substrate 31. It should be noted that the optical adjustment layer 34 contacts the second main surface 22 of the translucent conductive layer 2.
[0082] It should be noted that Figure 1 In the embodiment, the optical adjustment layer 34 is disposed on one side of the transparent substrate 31 in the thickness direction, but it is not limited thereto. That is, the optical adjustment layer 34 may be disposed on the other side of the transparent substrate 31 in the thickness direction, or may be disposed in multiple layers. In addition, when the substrate layer 3 has the hard coating layer 33 and the optical adjustment layer 34 in the same direction on one side or the other side of the transparent substrate 31 in the thickness direction, the stacking order is not particularly limited.
[0083] The optical adjustment layer 34 is formed of, for example, an optical adjustment composition.
[0084] The optical adjustment composition contains, for example, a resin and contains particles as needed. That is, the optical adjustment layer 34 contains, for example, a resin and contains particles as needed.
[0085] Examples of the resin include the resins listed above for the hard coating composition, and preferably include melamine resins, alkyd resins, and organosilane condensates.
[0086] Examples of the particles include the particles exemplified above for the hard coating composition.
[0087] The optical adjustment composition contains, for example, a resin, preferably a curable resin, and more preferably a thermosetting resin. Specifically, the optical adjustment composition contains a melamine resin, an alkyd resin, and an organic silane condensate.
[0088] The optical adjustment composition may be mixed with, for example, a thixotropy-imparting agent, a photopolymerization initiator, a filler (eg, organoclay), and a leveling agent at an appropriate ratio. The optical adjustment composition may be diluted with a known solvent.
[0089] The formation of the optical adjustment layer 34 will be described in detail later. A diluted optical adjustment composition is applied to one surface in the thickness direction of the transparent substrate 31 and dried as necessary. After drying, the optical adjustment composition is cured by, for example, heating.
[0090] Thus, the optical adjustment layer 34 is formed.
[0091] The thickness of the optical adjustment layer 34 is, for example, greater than 1 nm, preferably greater than 5 nm, more preferably greater than 10 nm, further preferably greater than 20 nm, particularly preferably greater than 30 nm, and is, for example, less than 1000 nm, preferably less than 500 nm, more preferably less than 100 nm, further preferably less than 50 nm.
[0092] The thickness of the optical adjustment layer 34 can be calculated based on the wavelength of the interference spectrum observed using a transient multi-channel photometry system, for example. Alternatively, the thickness can be determined by observing a cross section of the optical adjustment layer 34 using a field emission transmission electron microscope (FE-TEM).
[0093] <Light-transmitting conductive layer>
[0094] The light-transmitting conductive layer 2 is a transparent layer having excellent conductivity.
[0095] The light-transmitting conductive layer 2 includes a first main surface 21 and a second main surface 22 opposite to the first main surface 21 in the thickness direction. In addition, a base material layer 3 is arranged on the first main surface 21 and / or the second main surface 22 side of the light-transmitting conductive layer 2. Preferably, the base material layer 3 is arranged on the second main surface 22 side (the other side in the thickness direction) of the light-transmitting conductive layer 2. Specifically, the light-transmitting conductive layer 2 includes an optical adjustment layer 34, a transparent base material 31, and a hard coating layer 33 in sequence from the second main surface 22 side (the other side in the thickness direction) toward the other side in the thickness direction. That is, the light-transmitting conductive layer 2 is arranged on the entire upper surface (one side in the thickness direction) of the optical adjustment layer 34 in a manner that contacts one side in the thickness direction of the optical adjustment layer 34. It should be noted that the light-transmitting conductive layer 2 is the uppermost layer of the light-transmitting conductive sheet.
[0096] The first main surface 21 is exposed on one side in the thickness direction. The first main surface 21 is a flat surface.
[0097] The second main surface 22 is disposed opposite to the first main surface 21 at a distance from the other side in the thickness direction. The second main surface 22 is a flat surface parallel to the first main surface 21. In this embodiment, the light-transmitting conductive layer 2 includes an optical adjustment layer 34, a transparent substrate 31, and a hard coating layer 33 in this order on the second main surface 22 side (the other side in the thickness direction).
[0098] It should be noted that the flat surface means that both the first main surface 21 and the second main surface 22 are substantially parallel planes. For example, minute irregularities and ripples to an extent that cannot be observed are permitted.
[0099] Examples of the material of the light-transmitting conductive layer 2 include metal oxides containing at least one metal and / or semimetal selected from the group consisting of In, Sn, Zn, Ga, Sb, Ti, Si, Zr, Mg, Al, Au, Ag, Cu, Pd, and W. The metal oxides may be doped with metal atoms listed in the above group as needed.
[0100] As the light-transmitting conductive layer 2, specifically, for example, indium-containing oxides such as indium tin oxide (ITO), indium gallium oxide (IGO), indium zinc oxide (IZO), indium gallium zinc oxide (IGZO), and antimony-containing oxides such as antimony tin oxide (ATO) can be listed. Preferably, indium-containing oxides can be listed, and more preferably, indium tin oxide (ITO) can be listed.
[0101] When the light-transmitting conductive layer 2 contains indium tin composite oxide, the resistance can be reduced.
[0102] When ITO is used as the material of the light-transmitting conductive layer 2, the content ratio of tin oxide relative to the total amount of tin oxide and indium oxide is, for example, 0.5 mass % or more, preferably 3 mass % or more, more preferably 5 mass % or more, further preferably 8 mass % or more, and, for example, 20 mass % or less, preferably 15 mass % or less, more preferably 12 mass % or less.
[0103] When the content of tin oxide is not less than the above lower limit, the resistance can be reduced. When the content of tin oxide is not more than the above upper limit, the heat stability of the light-transmitting conductive layer 2 is excellent.
[0104] The tin oxide concentration in the light-transmitting conductive layer 2 can be measured by X-ray photoelectron spectroscopy to calculate the tin oxide content. Alternatively, the tin oxide content can be estimated from the (known) composition of the target used when forming the light-transmitting conductive layer 2 by sputtering.
[0105] The light-transmitting conductive layer 2 has crystal grains, and preferably has a plurality of types of crystal grains. Crystal grains are sometimes referred to as crystalline particles.
[0106] Furthermore, the light-transmitting conductive layer 2 has a plurality of types of crystal grains and thus has a crystal grain boundary. It should be noted that the crystal grain boundary refers to a boundary between a plurality of adjacent crystal grains.
[0107] It should be noted that the grain size of the crystal grains described below is a circle equivalent diameter.
[0108] The average grain diameter of the crystal grains is 105 nm or less, preferably 100 nm or less, more preferably 95 nm or less, and, for example, is 20 nm or more, preferably 40 nm or more, more preferably 60 nm or more, and further preferably 80 nm or more.
[0109] When the average grain size of the crystal grains is less than the above upper limit, the bendability is excellent because the crystal grains are small. On the other hand, when the average grain size of the crystal grains is more than the above lower limit, the resistance can be reduced.
[0110] It should be noted that the average grain size of the crystal grains can be determined by photographing the crystal grains using a field emission transmission electron microscope (FE-TEM) and subjecting the photographed image to image analysis processing. Specifically, the measurement is performed by the method described in the Examples below.
[0111] The crystal grains include crystal grains having a maximum crystal grain diameter of, for example, 100 nm or more, preferably 110 nm or more, more preferably 130 nm or more, further preferably 150 nm or more, and particularly preferably 170 nm or more.
[0112] When crystal grains having a maximum crystal grain size equal to or larger than the above lower limit are included, the resistance can be reduced.
[0113] Furthermore, the maximum grain diameter of the crystal grains is, for example, 300 nm or less, preferably 250 nm or less, and more preferably 220 nm or less.
[0114] When the maximum crystal grain size is equal to or less than the above upper limit, there are no excessively large crystal grains, and the bendability is excellent.
[0115] It should be noted that the maximum grain size of the crystal grains can be determined by photographing the crystal grains using a field emission transmission electron microscope (FE-TEM) and subjecting the photographed image to image analysis processing. Specifically, the maximum grain size can be measured by the method described in the examples below.
[0116] In the light-transmitting conductive layer 2, the content ratio of grains with a grain diameter of 100 nm or more relative to the total number of grains is, for example, 80% or less, preferably 70% or less, more preferably 60% or less, further preferably 50% or less, and particularly preferably 40% or less, and, for example, exceeds 0%, preferably 5% or more, more preferably 10% or more, further preferably 20% or more, and particularly preferably 30% or more.
[0117] If the content ratio of crystal grains with a crystal grain diameter of 100 nm or more relative to the total number of crystal grains is below the upper limit, the bendability is excellent. In addition, if the content ratio of crystal grains with a crystal grain diameter of 100 nm or more relative to the total number of crystal grains is above the lower limit, the resistance can be reduced.
[0118] In the light-transmitting conductive layer 2 , the content ratio of crystal grains having a crystal grain diameter of 150 nm or more relative to the total number of crystal grains is, for example, 50% or less, preferably 30% or less, more preferably 20% or less, further preferably 10% or less, and particularly preferably 5% or less.
[0119] When the content ratio of crystal grains having a crystal grain diameter of 150 nm or more relative to the total number of crystal grains is equal to or less than the above upper limit, the bendability is excellent.
[0120] It should be noted that the content ratio of crystal grains with a specific crystal grain diameter or larger relative to the total number of crystal grains can be obtained by photographing the crystal grains using a field emission transmission electron microscope (FE-TEM) and performing image analysis on the photographed image. The measurement is specifically performed by the method described in the examples below.
[0121] In addition, the light-transmitting conductive layer 2 is crystalline because it has crystal grains. That is, the light-transmitting conductive layer 2 preferably does not include an amorphous region in the surface direction, and only includes a crystalline region. It should be noted that the transparent conductive layer including an amorphous region can be identified by observing the crystal grains in the surface direction of the transparent conductive layer using a transmission electron microscope (TEM), for example.
[0122] When the light-transmitting conductive layer 2 is crystalline, for example, after the light-transmitting conductive layer 2 is immersed in a 5 mass % hydrochloric acid aqueous solution for 15 minutes, it is washed with water and dried, and the resistance between the two terminals between about 15 mm on the first main surface 21 is measured, and the resistance between the two terminals is 10 kΩ or less. On the other hand, if the resistance between the two terminals exceeds 10 kΩ, the light-transmitting conductive layer 2 is amorphous.
[0123] The total light transmittance (JIS K 7375-2008) of the light-transmitting conductive layer 2 is, for example, 60% or more, preferably 80% or more, and more preferably 85% or more.
[0124] When the total light transmittance of the light-transmitting conductive layer 2 is not less than the above lower limit, the light-transmitting conductive layer 2 has excellent transparency.
[0125] The thickness of the light-transmitting conductive layer 2 exceeds 50 nm, preferably is 55 nm or more, more preferably is 60 nm or more, further preferably is 80 nm or more, particularly preferably is 100 nm or more, and most preferably is 120 nm or more. In addition, for example, it is 1000 nm or less, preferably 300 nm or less, more preferably 250 nm or less, further preferably 200 nm or less, particularly preferably 150 nm or less, and most preferably 130 nm or less.
[0126] When the thickness of the light-transmitting conductive layer 2 is not less than the above lower limit, the resistance can be reduced. On the other hand, when the thickness of the light-transmitting conductive layer 2 is not more than the above upper limit, the bendability is excellent.
[0127] In addition, the thickness of the light-transmitting conductive layer 2 can be measured by observing the cross section of the light-transmitting conductive sheet 1 using a field emission transmission electron microscope (FE-TEM), for example.
[0128] The resistivity of the light-transmitting conductive layer 2 is, for example, 5.0×10 -4 Ω·cm or less, preferably 3.0×10 -4 Ω·cm or less, more preferably 2.8×10 -4 Ω·cm or less, more preferably 2.6×10 -4 Ω·cm or less, and for example, 0.1×10 -4 Ω·cm or more, preferably 0.5×10 -4 Ω·cm or more, more preferably 1.0×10 -4 Ω·cm or more.
[0129] In addition, the resistivity can be measured by the four-probe method according to JIS K7194.
[0130] The surface resistance value of the light-transmitting conductive layer 2 is, for example, 200Ω / □ or less, preferably 80Ω / □ or less, more preferably 50Ω / □ or less, further preferably 40Ω / □ or less, particularly preferably 30Ω / □ or less, most preferably 25Ω / □ or less, and usually exceeds 0Ω / □, and is 1Ω / □ or more.
[0131] In addition, the surface resistance value can be measured by the four-terminal method based on JIS K7194.
[0132] The number of the light-transmitting conductive layers 2 in the light-transmitting conductive sheet 1 is not particularly limited, and is, for example, 1. Specifically, the number of the light-transmitting conductive layers 2 is, for example, 1 per 1 layer of the base material layer 3 .
[0133] <Method for producing light-transmitting conductive sheet>
[0134] refer to Figure 2 , a method for manufacturing the light-transmitting conductive sheet 1 is described.
[0135] The method for manufacturing the light-transmitting conductive sheet 1 comprises a first step of preparing a substrate layer 3, a second step of stacking (arranging) a light-transmitting conductive layer 2 on one surface in the thickness direction of the substrate layer 3, and a third step of heating and crystallizing the light-transmitting conductive layer 2. In addition, in the manufacturing method, each layer is sequentially arranged, for example, in a roll-to-roll manner.
[0136] [1st step]
[0137] In the first step, the base material layer 3 is prepared.
[0138] In making the substrate layer 3, Figure 2 As shown in A, first, a transparent substrate 31 is prepared.
[0139] Then, if Figure 2 As shown in FIG. 1B , a diluted solution of the optical adjustment composition is applied to one side of the transparent substrate 31 in the thickness direction, and after drying, the optical adjustment composition is cured by ultraviolet irradiation or heating. Thus, an optical adjustment layer 34 is formed on one side of the transparent substrate 31 in the thickness direction.
[0140] Further, if Figure 2 As shown in FIG. 3 , a diluted solution of a hard coating composition is applied to the other side of the transparent substrate 31 in the thickness direction, and after drying, the hard coating composition is cured by ultraviolet irradiation or heating. Thus, a hard coating layer 33 is formed on the other side of the transparent substrate 31 in the thickness direction. Thus, a substrate layer 3 is produced.
[0141] [Step 2]
[0142] In the second step, Figure 2As shown in D in FIG. 1 , the light-transmitting conductive layer 2 is stacked (arranged) on one surface in the thickness direction of the base material layer 3 (optical adjustment layer 34 ).
[0143] Examples of a method for laminating the light-transmitting conductive layer 2 include vacuum deposition, sputtering, and ion plating. Preferably, sputtering is used. That is, the light-transmitting conductive layer 2 is preferably a sputtered layer.
[0144] In the sputtering method, in a chamber of a vacuum device, one side of the adherend (base layer 3) in the thickness direction is opposed to a target formed of the material of the light-transmitting conductive layer 2, and gas is supplied and a voltage is applied to accelerate and irradiate the gas ions to eject the target material from the target surface, thereby laminating the target material on the adherend surface. In addition, the base layer 3 is closely attached along the circumferential direction of the film-forming roller.
[0145] Examples of the sputtering method include a dipole sputtering method, an ECR (electron cyclotron resonance) sputtering method, a magnetron sputtering method, and an ion beam sputtering method. Preferably, the magnetron sputtering method is used.
[0146] Examples of the power source used in the sputtering method include a direct current (DC) power source, an alternating current medium frequency (AC / MF) power source, a high frequency (RF) power source, and a high frequency power source superimposed with a direct current power source. Preferably, a DC power source is used.
[0147] That is, in the second step, a DC magnetron sputtering device is preferably used.
[0148] As the target, for example, there can be mentioned the above-mentioned metal oxides constituting the light-transmitting conductive layer 2. Specifically, when ITO is used as the material of the light-transmitting conductive layer 2, a target formed of ITO is used.
[0149] The horizontal magnetic field intensity on the target is, for example, 10 mT or more, preferably 60 mT or more, and, for example, 300 mT or less.
[0150] By setting the horizontal magnetic field intensity on the target to the above range, the resistance of the light-transmitting conductive layer 2 can be reduced.
[0151] The film formation temperature during sputtering (specifically, the temperature of the base material layer 3 ) is, for example, 100° C. or less, preferably 50° C. or less, more preferably 0° C. or less, further preferably -5° C. or less, and, for example, -20° C. or more.
[0152] If the film forming temperature during sputtering is within the above range, the substrate layer 3 can be sufficiently cooled, and the crystal growth of the translucent conductive layer 2 during film formation (especially the crystal growth in the thickness direction of the translucent conductive layer 2) can be suppressed, so that it is easy to obtain grains in the translucent conductive layer 2 after the third step described later.
[0153] The gas pressure in the sputtering film forming apparatus is, for example, 1.0 Pa or less, preferably 0.5 Pa or less, and, for example, 0.01 Pa or more, preferably 0.1 Pa or more.
[0154] As the gas (sputtering gas) to be introduced, for example, an inert gas is mentioned, and argon gas is preferred. In addition, a reactive gas (for example, oxygen gas) may be used in combination.
[0155] The ratio of the amount of reactive gas introduced to the total amount of sputtering gas and reactive gas introduced is, for example, 0.1 flow % or more, preferably 1.0 flow % or more, more preferably 2.0 flow % or more, and, for example, 10.0 flow % or less, preferably 8.0 flow % or less, more preferably 5.0 flow % or less.
[0156] By adjusting the ratio of the amount of the reactive gas introduced to the total amount of the sputtering gas and the reactive gas introduced, the grain size of the crystal grains 6 in the light-transmitting conductive layer 2 can be adjusted.
[0157] Thus, the amorphous light-transmitting conductive sheet 1 including the amorphous light-transmitting conductive layer 2 and the base material layer 3 is obtained.
[0158] [Step 3]
[0159] In the third step, the amorphous light-transmitting conductive layer 2 is heated. For example, the amorphous light-transmitting conductive layer 2 is heated by a heating device (for example, an infrared heater or a hot air oven).
[0160] The heating temperature is, for example, 80° C. or more, preferably 110° C. or more, and, for example, less than 200° C., preferably 180° C. or less. The heating time is, for example, 1 minute or more, preferably 10 minutes or more, more preferably 20 minutes or more, and, for example, 24 hours or less, preferably 4 hours or less, more preferably 1 hour or less.
[0161] Therefore, if Figure 2 As shown in E, the amorphous light-transmitting conductive layer 2 is crystallized to form a crystalline light-transmitting conductive layer 2 .
[0162] In this way, the light-transmitting conductive layer 2 is obtained, and the light-transmitting conductive sheet 1 including the light-transmitting conductive layer 2 and the base material layer 3 is obtained.
[0163] Then, the light-transmitting conductive layer 2 may be patterned. For example, the patterning is performed by etching.
[0164] <Effects>
[0165] The present invention is a light-transmitting conductive layer having a first main surface and a second main surface opposite to the first main surface in the thickness direction, wherein the thickness of the light-transmitting conductive layer exceeds 50 nm, and the light-transmitting conductive layer has crystal grains, and the average crystal grain diameter of the crystal grains is less than 105 nm. Therefore, the light-transmitting conductive layer has low resistance and excellent bendability.
[0166] Specifically, the light-transmitting conductive layer has a thickness exceeding 50 nm and thus has low resistance, and has excellent bendability because it has crystal grains and the average crystal grain diameter is 105 nm or less.
[0167] Furthermore, the light-transmitting conductive sheet including the light-transmitting conductive layer of the present invention has low resistance and excellent bendability.
[0168] Example
[0169] Embodiment and comparative example are shown below, and the present invention is further specifically described.It should be noted that the present invention is not limited to any embodiment and comparative example.In addition, the specific numerical values such as the blending ratio (containing ratio), physical property value, parameter used in the following description can replace the upper limit (as the numerical value defined as "below", "not enough") or the lower limit (as the numerical value defined as "above", "exceeding") of the blending ratio (containing ratio), physical property value, parameter, etc. recorded in the above-mentioned "specific embodiments", corresponding thereto.
[0170] Example 1
[0171] <Manufacturing of light-transmitting conductive sheet>
[0172] [1st step]
[0173] As a long transparent substrate, a roll of polyethylene terephthalate (PET) film (thickness 100μm, manufactured by Mitsubishi Chemical Corporation) is prepared, and a thermosetting resin composition C1 is applied on one side of the PET film in the thickness direction to form a coating. The coating of the resin composition C1 is heated at 185°C for 1 minute to cure it. Thus, an optical adjustment layer with a thickness of 35nm is formed. It should be noted that the resin composition C1 is a resin composition comprising 100 parts by mass of a melamine resin, 100 parts by mass of an alkyd resin, and 50 parts by mass of an organic silane condensate. Then, a UV-curable resin composition C2 is applied on the other side of the PET film in the thickness direction to form a coating. The coating of the resin composition C2 is cured by ultraviolet irradiation. Thus, a hard coating layer with a thickness of 2μm is formed. It should be noted that the resin composition C2 is a resin composition comprising an acrylic resin.
[0174] In this way, a base material layer (comprising a hard coat layer, a transparent base material, and an optical adjustment layer in this order toward one side in the thickness direction) was prepared.
[0175] [Step 2]
[0176] An amorphous light-transmitting conductive layer with a thickness of 125 nm was stacked (arranged) on one side of the substrate layer (optical adjustment layer) in the thickness direction by reactive sputtering. In the reactive sputtering, a sputtering film forming apparatus (DC magnetron sputtering apparatus) capable of performing film forming process by roll-to-roll method was used.
[0177] Specifically, a sintered body of indium oxide and tin oxide (tin oxide concentration of 10 mass%) was used as a target. A DC power supply was used as a power source for applying voltage to the target. The horizontal magnetic field intensity on the target was set to 90 mT. The conveying speed of the substrate layer was set to 2.0 m / min. The film forming temperature (temperature of the substrate layer) was set to -8°C.
[0178] In addition, the sputtering film forming apparatus was evacuated to a vacuum level of 0.8×10 -4 After 0.04 Pa, argon as a sputtering gas and oxygen as a reactive gas were introduced into the sputtering film forming apparatus, and the gas pressure in the sputtering film forming apparatus was set to 0.4 Pa. It should be noted that the ratio of the oxygen introduction amount to the total introduction amount of argon and oxygen introduced into the sputtering film forming apparatus was approximately 3.4 flow %.
[0179] In this way, a light-transmitting conductive sheet including an amorphous light-transmitting conductive layer having a thickness of 125 nm was obtained.
[0180] [Step 3]
[0181] The light-transmitting conductive sheet having the amorphous light-transmitting conductive layer was heated in a hot air oven at 155° C. for 30 minutes to crystallize the light-transmitting conductive layer.
[0182] Thus, the light-transmitting conductive sheet of Example 1 including the light-transmitting conductive layer and the base material layer on the second main surface side (the other side in the thickness direction) of the light-transmitting conductive layer was obtained.
[0183] Comparative Example 1
[0184] A light-transmitting conductive sheet was obtained in the same manner as in Example 1 except that krypton gas was used as the sputtering gas in the second step.
[0185] Comparative Example 2
[0186] A light-transmitting conductive sheet was obtained in the same manner as in Example 1, except that the light-transmitting conductive sheet was not heated in the third step so as not to crystallize the amorphous light-transmitting conductive layer.
[0187] <Evaluation>
[0188] [Thickness of light-transmitting conductive layer]
[0189] The thickness of the light-transmitting conductive layer of Example 1 and each comparative example was measured by observation (cross-sectional observation) using a field emission transmission electron microscope (FE-TEM). Specifically, first, samples for cross-sectional observation of the light-transmitting conductive layer of Example 1 and each comparative example were prepared by a focused ion beam (FIB) microsampling method. A FIB device (trade name "FB2200", manufactured by Hitachi) was used in the FIB microsampling method, and the acceleration voltage was set to 10 kV. Then, the thickness of the light-transmitting conductive layer in the sample for cross-sectional observation was measured by FE-TEM observation. A FE-TEM device (trade name "JEM-2800", manufactured by JEOL) was used in the FE-TEM observation, and the acceleration voltage was set to 200 kV. The results are shown in Table 1.
[0190] [Resistance value]
[0191] The resistance values (R0) of the light-transmitting conductive sheets of Example 1 and Comparative Example were measured by a four-terminal method. The resistance values were evaluated based on the following criteria. The results are shown in Table 1.
[0192] {Benchmark}
[0193] ○: 40Ω / □ or less
[0194] ×: more than 40Ω / □
[0195] [Grain diameter (top view)]
[0196] The light-transmitting conductive sheets of Example 1 and Comparative Example 1 were cut and fixed on the sample holder of the ultrathin slicer. Then, the slicer was set at an extremely acute angle relative to the light-transmitting conductive layer surface, and the cross section was cut in a manner that was roughly parallel to the light-transmitting conductive layer, thereby obtaining an observation sample. The observation sample was photographed using a FE-TEM device (trade name "JEM-2800", manufactured by JEOL) at an accelerating voltage of 200 kV to photograph the grains of the light-transmitting conductive layer from a top view (direct magnification: 100,000 times). It should be noted that the photographing range was set to approximately 1400 nm × 1400 nm. Then, by performing image analysis processing on the photographed image, the area of each grain boundary region was calculated based on the number of pixels existing in the region specified by the grain boundary (the region within each grain boundary), and the diameter of a circle having the same area as that of the circle was calculated as the grain diameter (equivalent circle diameter), and the average grain diameter and the maximum grain diameter were calculated. In addition, the number of crystal grains with a crystal grain diameter of 100 nm or more among the crystal grains observed (photographed) by FE-TEM was calculated, and the content ratio of crystal grains of 100 nm or more relative to the total number of observed crystal grains was calculated. In addition, the content ratio of crystal grains of 150 nm or more was also calculated. The results are shown in Table 1. It should be noted that the light-transmitting conductive sheet of Comparative Example 2 is amorphous and therefore has no crystal grains.
[0197] [Flexibility]
[0198] The light-transmitting conductive sheet of each embodiment and each comparative example was cut into a width of 10 mm and a length of 150 mm. The cut light-transmitting conductive sheet was placed on a core rod so that the light-transmitting conductive layer was on the outside and the other side (hard coating) of the substrate layer in the thickness direction was in contact with the core rod. Then, the two ends of the light-transmitting conductive sheet in the length direction were clamped with a clamp, and a weight of 1000 g was placed in the center of the clamp. That is, a load of 100 g / mm relative to the width of the light-transmitting conductive sheet was applied to the lower side to bend the light-transmitting conductive sheet. This bending state lasted for 10 seconds. In this bending state, after the bent portion was coated with a marker pen, the bending state was released and the marked portion was observed under a microscope. The diameter of the core rod was changed from a large diameter to a small diameter by 1 mm each time, and the minimum diameter in which cracks could not be confirmed in the observation of the pen-coated portion was shown in Table 1. The smaller the diameter in which cracks could not be confirmed, the better the bending resistance. It should be noted that a new light-transmitting conductive sheet was used each time the diameter of the core rod was changed.
[0199] [Table 1]
[0200] Table 1
[0201]
[0202] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, but it is merely an illustration and should not be interpreted as limiting. Modifications of the present invention that are obvious to those skilled in the art are within the scope of the above claims.
[0203] Industrial Applicability
[0204] The light-transmitting conductive sheet 1 including the light-transmitting conductive layer 2 of the present invention is suitably used for a touch panel or a dimming panel included in an optical device.
Claims
1. A light-transmitting conductive layer comprising a first main surface and a second main surface opposite to the first main surface in a thickness direction, The thickness of the light-transmitting conductive layer exceeds 50 nm, The light-transmitting conductive layer has crystal grains, The average grain diameter of the crystal grains is less than 105 nm.
2. The light-transmitting conductive layer according to claim 1, wherein The crystal grains include crystal grains having a maximum crystal grain diameter of 110 nm or more.
3. The light-transmitting conductive layer according to claim 1, wherein The content ratio of the crystal grains having a crystal grain diameter of 100 nm or more is 70% or less relative to the total number of the crystal grains.
4. A light-transmitting conductive sheet comprising: The light-transmitting conductive layer according to any one of claims 1 to 3, and A base material layer is provided on the first main surface and / or the second main surface side of the light-transmitting conductive layer.