High-ripple-resistant electrolyte for ox horn type product

By using a combination of organic matter, electrolyte and polymer matrix in the electrolyte of horn-type products, especially the addition of boric acid and anti-foaming agent, the problems of insufficient conductive performance and lack of high ripple resistance are solved, achieving high frequency performance. Stable operation and extended service life under environmental conditions.

CN118737706APending Publication Date: 2024-10-01ANHUI LINKEYCON ELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410895564.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing electrolytes used in horn-type products have insufficient conductivity in high-frequency environments and lack high ripple resistance, making them unable to operate stably in high-frequency working environments.

Method used

Using a combination of organic matter, electrolyte, polymer matrix and additives, including organic acids, ammonium chloride, zinc sulfate, polyacrylate, etc., through the addition of boric acid and anti-foaming agents, the viscosity and vibration resistance of the electrolyte are improved, and the metal Corrosion rate.

Benefits of technology

It effectively improves the conductivity and high ripple resistance of the electrolyte, prolongs the service life of horn-type products, and ensures stable operation in high-frequency environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of electrolyte, in particular to ox horn type product high-ripple-resistant electrolyte which comprises the following raw material components in percentage by mass: 30-60 parts of organic matter, 25-40 parts of electrolyte, 10-15 parts of polymer matrix, 5-10 parts of additive and 1-5 parts of anti-foaming agent. The organic matter comprises organic acid, an organic additive and an organic solvent, the electrolyte comprises ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride, the polymer matrix comprises polyacrylate, polyvinyl alcohol and polyurethane, and the additive comprises a main additive and a high-ripple-resistant additive. According to the invention, the viscosity and adhesiveness of the electrolyte can be improved, the stability of the surface of the electrolyte can be enhanced, the oscillation resistance of the electrolyte can be effectively improved, and the corrosion rate of the electrolyte to metal can be reduced, so that the service life of an ox horn type product is prolonged, and the ox horn type product has certain high ripple resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolytes, and in particular to an electrolyte for high ripple resistance of horn-shaped products. Background Art

[0002] Horn-shaped products usually refer to electronic devices or components that are shaped like horns, and are commonly found in some electronic products, such as wireless communication devices, antennas, etc. These products may require the use of electrolytes to achieve certain functions, such as improving conductivity, protecting the surface, and preventing corrosion.

[0003] In electronic devices or components, especially for devices that need to work stably in high-frequency environments, such as wireless communication devices, radio frequency circuits, etc., electrolytes are often required to achieve certain specific functions. Bull-horn products may require an electrolyte that is resistant to high ripple to ensure its stability and performance in high-frequency working environments. Some existing electrolyte formulations for bull-horn products may have insufficient conductivity in high-frequency environments, resulting in insufficient conductivity in bull-horn products, and also lack of certain high ripple resistance performance. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides an electrolyte for high ripple resistance of horn-type products, which can effectively solve the problems in the prior art that it cannot provide sufficient conductive performance and does not have certain high ripple resistance performance.

[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0006] The present invention provides an electrolyte for high ripple resistance of horn-shaped products, comprising the following raw material components in percentage by mass:

[0007] 30-60 parts by weight of organic matter, 25-40 parts by weight of electrolyte, 10-15 parts by weight of polymer matrix, 5-10 parts by weight of additives and 1-5 parts by weight of antifoaming agent;

[0008] The organic matter includes organic acid, organic additive and organic solvent, the electrolyte includes ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride, the polymer matrix includes polyacrylate, polyvinyl alcohol and polyurethane, and the additive includes main additive and high ripple resistance additive;

[0009] The main additives include a corrosion inhibitor, a wetting agent, a surfactant and an antioxidant, wherein the corrosion inhibitor, the wetting agent, the surfactant and the antioxidant are benzimidazole, propylene glycol, octanolphenol polyoxyethylene ether and thio-tert-butylphenol respectively;

[0010] The high ripple resistance additive is boric acid, and the ratio of the main additive to the high ripple resistance additive is 10:1;

[0011] The antifoaming agent is dimethyl silicone oil.

[0012] According to the above-mentioned high ripple resistant electrolyte for horn-type products, the electrolyte includes the following raw material components in mass percentage: 45 parts by mass of organic matter, 35 parts by mass of electrolyte, 10 parts by mass of polymer matrix, 6 parts by mass of additives and 4 parts by mass of antifoaming agent.

[0013] According to the above-mentioned high ripple resistant electrolyte for horn-shaped products, the electrolyte includes the following raw material components in mass percentage: 50 parts by mass of organic matter, 25 parts by mass of electrolyte, 12 parts by mass of polymer matrix, 8 parts by mass of additives and 5 parts by mass of antifoaming agent.

[0014] According to the above-mentioned high ripple-resistant electrolyte for horn-type products, the ratio of the organic acid, the organic additive and the organic solvent is 6:1:3.

[0015] According to the above-mentioned high ripple resistant electrolyte for horn-type products, the ratio of ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride is 4:3:2:1.

[0016] According to the above-mentioned high ripple-resistant electrolyte for horn-shaped products, the ratio of the polyacrylate, polyvinyl alcohol and polyurethane is 2:1:1:3.

[0017] According to the above-mentioned high ripple resistant electrolyte for horn-type products, the ratio of the corrosion inhibitor, the humidifier, the surfactant and the antioxidant is 5:4:3:1.

[0018] According to the above-mentioned high ripple resistant electrolyte for horn-shaped products, the preparation method includes:

[0019] S1. Gradually add the electrolyte and polymer matrix to the organic matter at a temperature of 100-115°C, and stir thoroughly for 10-40 minutes after each addition until they are completely dissolved and evenly mixed;

[0020] S2. Add the main additive, high ripple resistance additive and anti-foaming agent to the mixed electrolyte and polymer matrix one by one, and stir them thoroughly for 10 to 30 minutes to ensure that the various additives are evenly dispersed in the solution;

[0021] S3. According to actual needs, acid or alkali can be used to adjust the pH value of the electrolyte to ensure the stability and performance of the final solution.

[0022] Compared with the known prior art, the technical solution provided by the present invention has the following beneficial effects:

[0023] 1. The polymer matrix with polyacrylate, polyvinyl alcohol and polyurethane as the main materials, combined with organic matter with organic acid, organic additives and organic solvent as raw materials, can effectively improve the viscosity and adhesion of the electrolyte and enhance the stability of the electrolyte surface;

[0024] 2. By adding boric acid, main additives and anti-foaming agents to the mixture of electrolyte and polymer and mixing them again, the vibration resistance of the electrolyte can be effectively improved, and its corrosion rate to the metal can be reduced, thereby extending the service life of the bullhorn type product and having a certain high ripple resistance performance.

[0025] In summary, the present invention can improve the viscosity and adhesion of the electrolyte and enhance the stability of the electrolyte surface through the mixing of boric acid, polymer matrix and electrolyte. It can also effectively improve the vibration resistance of the electrolyte and reduce its corrosion rate to metal, thereby extending the service life of the bullhorn-type product and having a certain high ripple resistance performance. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The present invention will be further described below in conjunction with the embodiments.

[0028] Embodiment 1:

[0029] An electrolyte for high ripple resistance of horn-shaped products, comprising the following raw material components in percentage by mass:

[0030] 45 parts by mass of organic matter, 35 parts by mass of electrolyte, 10 parts by mass of polymer matrix, 6 parts by mass of additives and 4 parts by mass of antifoaming agent;

[0031] The organic matter includes organic acid, organic additive and organic solvent, the ratio of organic acid, organic additive and organic solvent is 6:1:3, and the organic acid can be citric acid or oxalic acid, which is used to adjust pH and provide electrolyte.

[0032] The electrolyte includes ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride, the ratio of ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride is 4:3:2:1, the polymer matrix includes polyacrylate, polyvinyl alcohol and polyurethane, the ratio of polyacrylate, polyvinyl alcohol and polyurethane is 2:1:1:3, the additive includes a main additive and a high ripple resistance additive, potassium carbonate is used to adjust the pH value of the electrolyte, and sodium chloride is used to increase the conductivity;

[0033] The main additives include corrosion inhibitors, wetting agents, surfactants and antioxidants. The ratio of corrosion inhibitors, wetting agents, surfactants and antioxidants is 5:4:3:1. The corrosion inhibitors, wetting agents, surfactants and antioxidants are benzimidazole, propylene glycol, octanolphenol polyoxyethylene ether and tert-butylthiophenol, respectively. The corrosion inhibitor is used to prevent metal corrosion, the wetting agent is used to improve the wettability of the electrolyte, and the surfactant is used to improve the surface tension of the liquid.

[0034] The high ripple resistance additive is boric acid. The ratio of the main additive to the high ripple resistance additive is 10:1. Boric acid can effectively improve the electrolyte's vibration resistance and reduce its corrosion rate to metals, thereby extending the service life of bullhorn products.

[0035] The anti-foaming agent is dimethyl silicone oil, which is used to reduce bubble formation.

[0036] The preparation method comprises: gradually adding electrolyte and polymer matrix into organic matter at a temperature of 100 to 115° C., and fully stirring for 10 to 40 minutes after each addition until the electrolyte and polymer matrix are completely dissolved and uniformly mixed;

[0037] Add the main additive, high ripple resistance additive and anti-foaming agent one by one to the mixed electrolyte and polymer matrix, and stir thoroughly for 10 to 30 minutes to ensure that the various additives are evenly dispersed in the solution;

[0038] According to actual needs, acid or alkali can be used to adjust the pH value of the electrolyte to ensure the stability and performance of the final solution.

[0039] Embodiment 2:

[0040] An electrolyte for high ripple resistance of horn-shaped products, comprising the following raw material components in percentage by mass:

[0041] 50 parts by mass of organic matter, 25 parts by mass of electrolyte, 12 parts by mass of polymer matrix, 8 parts by mass of additives and 5 parts by mass of antifoaming agent;

[0042] The organic matter includes organic acid, organic additive and organic solvent, the ratio of organic acid, organic additive and organic solvent is 6:1:3, and the organic acid can be citric acid or oxalic acid, which is used to adjust pH and provide electrolyte.

[0043] The electrolyte includes ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride, the ratio of ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride is 4:3:2:1, the polymer matrix includes polyacrylate, polyvinyl alcohol and polyurethane, the ratio of polyacrylate, polyvinyl alcohol and polyurethane is 2:1:1:3, the additive includes a main additive and a high ripple resistance additive, potassium carbonate is used to adjust the pH value of the electrolyte, and sodium chloride is used to increase the conductivity;

[0044] The main additives include corrosion inhibitors, wetting agents, surfactants and antioxidants. The ratio of corrosion inhibitors, wetting agents, surfactants and antioxidants is 5:4:3:1. The corrosion inhibitors, wetting agents, surfactants and antioxidants are benzimidazole, propylene glycol, octanolphenol polyoxyethylene ether and tert-butylthiophenol, respectively. The corrosion inhibitor is used to prevent metal corrosion, the wetting agent is used to improve the wettability of the electrolyte, and the surfactant is used to improve the surface tension of the liquid.

[0045] The high ripple resistance additive is boric acid. The ratio of the main additive to the high ripple resistance additive is 10:1. Boric acid can effectively improve the electrolyte's vibration resistance and reduce its corrosion rate to metals, thereby extending the service life of bullhorn products.

[0046] The anti-foaming agent is dimethyl silicone oil, which is used to reduce bubble formation.

[0047] The preparation method comprises: gradually adding electrolyte and polymer matrix into organic matter at a temperature of 100 to 115° C., and fully stirring for 10 to 40 minutes after each addition until the electrolyte and polymer matrix are completely dissolved and uniformly mixed;

[0048] Add the main additive, high ripple resistance additive and anti-foaming agent one by one to the mixed electrolyte and polymer matrix, and stir thoroughly for 10 to 30 minutes to ensure that the various additives are evenly dispersed in the solution;

[0049] According to actual needs, acid or alkali can be used to adjust the pH value of the electrolyte to ensure the stability and performance of the final solution.

[0050] Embodiment three:

[0051] An electrolyte for high ripple resistance of horn-shaped products, comprising the following raw material components in percentage by mass:

[0052] 55 parts by mass of organic matter, 30 parts by mass of electrolyte, 8 parts by mass of polymer matrix, 7 parts by mass of additives and 5 parts by mass of antifoaming agent;

[0053] The organic matter includes organic acid, organic additive and organic solvent, the ratio of organic acid, organic additive and organic solvent is 6:1:3, and the organic acid can be citric acid or oxalic acid, which is used to adjust pH and provide electrolyte.

[0054] The electrolyte includes ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride, the ratio of ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride is 4:3:2:1, the polymer matrix includes polyacrylate, polyvinyl alcohol and polyurethane, the ratio of polyacrylate, polyvinyl alcohol and polyurethane is 2:1:1:3, the additive includes a main additive and a high ripple resistance additive, potassium carbonate is used to adjust the pH value of the electrolyte, and sodium chloride is used to increase the conductivity;

[0055] The main additives include corrosion inhibitors, wetting agents, surfactants and antioxidants. The ratio of corrosion inhibitors, wetting agents, surfactants and antioxidants is 5:4:3:1. The corrosion inhibitors, wetting agents, surfactants and antioxidants are benzimidazole, propylene glycol, octanolphenol polyoxyethylene ether and tert-butylthiophenol, respectively. The corrosion inhibitor is used to prevent metal corrosion, the wetting agent is used to improve the wettability of the electrolyte, and the surfactant is used to improve the surface tension of the liquid.

[0056] The high ripple resistance additive is boric acid. The ratio of the main additive to the high ripple resistance additive is 10:1. Boric acid can effectively improve the electrolyte's vibration resistance and reduce its corrosion rate to metals, thereby extending the service life of bullhorn products.

[0057] The anti-foaming agent is dimethyl silicone oil, which is used to reduce bubble formation.

[0058] The preparation method comprises: gradually adding electrolyte and polymer matrix into organic matter at a temperature of 100 to 115° C., and fully stirring for 10 to 40 minutes after each addition until the electrolyte and polymer matrix are completely dissolved and uniformly mixed;

[0059] Add the main additive, high ripple resistance additive and anti-foaming agent one by one to the mixed electrolyte and polymer matrix, and stir thoroughly for 10 to 30 minutes to ensure that the various additives are evenly dispersed in the solution;

[0060] According to actual needs, acid or alkali can be used to adjust the pH value of the electrolyte to ensure the stability and performance of the final solution.

[0061] Embodiment 4:

[0062] An electrolyte for high ripple resistance of horn-shaped products, comprising the following raw material components in percentage by mass:

[0063] 60 parts by mass of organic matter, 28 parts by mass of electrolyte, 12 parts by mass of polymer matrix, 7 parts by mass of additives and 3 parts by mass of antifoaming agent;

[0064] The organic matter includes organic acid, organic additive and organic solvent, the ratio of organic acid, organic additive and organic solvent is 6:1:3, and the organic acid can be citric acid or oxalic acid, which is used to adjust pH and provide electrolyte.

[0065] The electrolyte includes ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride, the ratio of ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride is 4:3:2:1, the polymer matrix includes polyacrylate, polyvinyl alcohol and polyurethane, the ratio of polyacrylate, polyvinyl alcohol and polyurethane is 2:1:1:3, the additive includes a main additive and a high ripple resistance additive, potassium carbonate is used to adjust the pH value of the electrolyte, and sodium chloride is used to increase the conductivity;

[0066] The main additives include corrosion inhibitors, wetting agents, surfactants and antioxidants. The ratio of corrosion inhibitors, wetting agents, surfactants and antioxidants is 5:4:3:1. The corrosion inhibitors, wetting agents, surfactants and antioxidants are benzimidazole, propylene glycol, octanolphenol polyoxyethylene ether and tert-butylthiophenol, respectively. The corrosion inhibitor is used to prevent metal corrosion, the wetting agent is used to improve the wettability of the electrolyte, and the surfactant is used to improve the surface tension of the liquid.

[0067] The high ripple resistance additive is boric acid. The ratio of the main additive to the high ripple resistance additive is 10:1. Boric acid can effectively improve the electrolyte's vibration resistance and reduce its corrosion rate to metals, thereby extending the service life of bullhorn products.

[0068] The anti-foaming agent is dimethyl silicone oil, which is used to reduce bubble formation.

[0069] The preparation method comprises: gradually adding electrolyte and polymer matrix into organic matter at a temperature of 100 to 115° C., and fully stirring for 10 to 40 minutes after each addition until the electrolyte and polymer matrix are completely dissolved and uniformly mixed;

[0070] Add the main additive, high ripple resistance additive and anti-foaming agent one by one to the mixed electrolyte and polymer matrix, and stir thoroughly for 10 to 30 minutes to ensure that the various additives are evenly dispersed in the solution;

[0071] According to actual needs, acid or alkali can be used to adjust the pH value of the electrolyte to ensure the stability and performance of the final solution.

[0072] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the protection scope of the technical solutions of the embodiments of the present invention.

Claims

1. An electrolyte for high ripple resistance of horn-shaped products, characterized in that: The raw material components include the following mass percentages: 30-60 parts by weight of organic matter, 25-40 parts by weight of electrolyte, 10-15 parts by weight of polymer matrix, 5-10 parts by weight of additives and 1-5 parts by weight of antifoaming agent; The organic matter includes organic acid, organic additive and organic solvent, the electrolyte includes ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride, the polymer matrix includes polyacrylate, polyvinyl alcohol and polyurethane, and the additive includes main additive and high ripple resistance additive; The main additives include a corrosion inhibitor, a wetting agent, a surfactant and an antioxidant, wherein the corrosion inhibitor, the wetting agent, the surfactant and the antioxidant are benzimidazole, propylene glycol, octanolphenol polyoxyethylene ether and thio-tert-butylphenol respectively; The high ripple resistance additive is boric acid, and the ratio of the main additive to the high ripple resistance additive is 10:1; The antifoaming agent is dimethyl silicone oil.

2. The high ripple resistant electrolyte for horn-shaped products according to claim 1, characterized in that: The raw material components include the following mass percentages: 45 parts by mass of organic matter, 35 parts by mass of electrolyte, 10 parts by mass of polymer matrix, 6 parts by mass of additives and 4 parts by mass of antifoaming agent.

3. The electrolyte for high ripple resistance of horn-shaped products according to claim 1, characterized in that: The raw material components include the following mass percentages: 50 parts by mass of organic matter, 25 parts by mass of electrolyte, 12 parts by mass of polymer matrix, 8 parts by mass of additives and 5 parts by mass of antifoaming agent.

4. The high ripple resistant electrolyte for horn-shaped products according to claim 1, characterized in that: The ratio of the organic acid, the organic additive and the organic solvent is 6:1:

3.

5. The electrolyte for high ripple resistance of horn-shaped products according to claim 1, characterized in that: The ratio of ammonium chloride, zinc sulfate, potassium carbonate and sodium chloride is 4:3:2:

1.

6. The high ripple resistant electrolyte for horn-shaped products according to claim 1, characterized in that: The ratio of the polyacrylate, polyvinyl alcohol and polyurethane is 2:1:1:

3.

7. The electrolyte for high ripple resistance of horn-shaped products according to claim 1, characterized in that: The ratio of the corrosion inhibitor, the wetting agent, the surfactant and the antioxidant is 5:4:3:

1.

8. The high ripple resistant electrolyte for horn-shaped products according to claim 1, characterized in that: The preparation method comprises: S1. Gradually add the electrolyte and polymer matrix to the organic matter at a temperature of 100-115°C, and stir thoroughly for 10-40 minutes after each addition until they are completely dissolved and evenly mixed; S2. Add the main additive, high ripple resistance additive and anti-foaming agent to the mixed electrolyte and polymer matrix one by one, and stir them thoroughly for 10 to 30 minutes to ensure that the various additives are evenly dispersed in the solution; S3. According to actual needs, acid or alkali can be used to adjust the pH value of the electrolyte to ensure the stability and performance of the final solution.