Lead frame, packaging structure and electroplating method

By setting openings in the side ribs of the lead frame and adjusting the area of ​​the plating area, the problems of uneven current density and thickness difference of the plating layer are solved, and the process capability index of the package is improved.

CN118738009APending Publication Date: 2024-10-01JCET GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410868616.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing packaging technology, the coating area of ​​the lead frame is too large, resulting in uneven current density, resulting in poor coating thickness, thereby reducing the process capability index of the package.

Method used

Design a lead frame with openings in both the first and second side ribs, the openings are located in the sub-side rib area, and the surface area of ​​the plating area is adjusted according to the shape, line width size and number of the sub-side rib area to Reduce the area of ​​the plating area and improve the uniformity of current density.

Benefits of technology

By reducing the area of ​​the plating area, the uniformity of current density per unit area of ​​the lead frame during the electroplating process is improved, the difference in plating thickness is reduced, and the process capability index of the package is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738009A_ABST
    Figure CN118738009A_ABST
Patent Text Reader

Abstract

The invention discloses a lead frame, a packaging structure and an electroplating method. The lead frame comprises a product area; the first side rib and the second side rib are located at the two ends of the product area respectively, openings are formed in the first side rib and the second side rib, and the areas, without the openings, of the first side rib and the second side rib are coating areas. Because the first edge rib and the second edge rib are provided with the openings, compared with a scheme that the first edge rib and the second edge rib are not provided with the openings, the surface area of the plating layer area in the first edge rib and the second edge rib is reduced, so that in a packaging process, when an electroplating process is carried out on the lead frame, the surface area of the plating layer area is reduced; the current density uniformity of the unit area at the positions of the first edge rib and the second edge rib is improved, the problem that the thickness difference exists between the first edge rib and the product area and between the second edge rib and the product area is solved, and therefore the processing capability index of packaging is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a lead frame, a packaging structure and an electroplating method. Background Art

[0002] The pursuit of performance and speed in electronic devices is driving the continuous innovation of packaging technology. With the demand for miniaturization and thinness of electronic devices, surface mount technology has gradually replaced traditional direct-insertion packaging.

[0003] The lead frame structure has become a very important carrier in packaging technology. In order to meet the strength requirements in processes such as patching, wire bonding, injection molding and electroplating, the lead frame structure often also includes process ribs such as side ribs and center ribs.

[0004] However, the current packaging process capability index still needs to be improved. Summary of the invention

[0005] The problem solved by the embodiments of the present invention is to provide a lead frame, a packaging structure and an electroplating method, which are beneficial to improving the process capability index of the packaging.

[0006] To solve the above problems, an embodiment of the present invention provides a lead frame, including: a product area; a first side rib and a second side rib, respectively located at two ends of the product area, the first side rib and the second side rib both having openings, and the areas of the first side rib and the second side rib without openings are plating areas, along the arrangement direction of the first side rib and the second side rib, the first side rib and the second side rib both include multiple sub-side rib areas, and the openings are located in the multiple sub-side rib areas.

[0007] Optionally, in either the first side rib and the second side rib, the openings located in the multiple sub-side rib areas satisfy one or more of the following conditions: the shapes of the openings in the multiple sub-side rib areas are different; the line widths of the openings in the multiple sub-side rib areas are different; the numbers of the openings in the multiple sub-side rib areas are different.

[0008] Optionally, in any one of the first side rib and the second side rib, along the direction from the product area to the sub-side rib area, the total cross-sectional area of ​​the openings in a plurality of the sub-side rib areas decreases sequentially.

[0009] Optionally, in either the first side rib and the second side rib, along the direction from the product area to the sub-side rib area, the openings in the multiple sub-side rib areas satisfy one or more of the following conditions: the density of the openings in the multiple sub-side rib areas decreases successively; the number of the openings in the multiple sub-side rib areas decreases successively; the line width size of the openings in the multiple sub-side rib areas decreases successively.

[0010] Optionally, the surface area of ​​the plated region of the first side rib and the surface area of ​​the plated region of the second side rib are both smaller than 1 / 3 of the surface area of ​​the product region.

[0011] Optionally, the surface area of ​​the plated region of the first side rib is smaller than the surface area of ​​the plated region of the second side rib.

[0012] Optionally, the type of the opening includes one or both of a through hole structure and a blind hole structure; wherein the blind hole is located on any surface of the lead frame.

[0013] Optionally, the cross-sectional shape of the opening includes one or more of a circular shape, an elliptical shape and a polygonal shape.

[0014] Correspondingly, an embodiment of the present invention further provides a packaging structure, comprising: a lead frame according to any embodiment of the present invention; and a plastic encapsulation layer filling the opening and exposing the plating areas of the first side rib and the second side rib.

[0015] Optionally, the packaging structure further includes: a chip, which is arranged on one side of the lead frame and located in the product area, and the chip is electrically connected to the lead frame; and the plastic packaging layer also covers the chip in the product area.

[0016] Correspondingly, an embodiment of the present invention also provides an electroplating method, comprising: providing a packaging structure as described in any embodiment of the present invention, the packaging structure comprising a front side and a back side arranged relatively to each other, the front side of the packaging structure being used to set a chip; performing an electroplating process on the packaging structure to form a coating on the back side of the product area and on the coating areas of the first side rib and the second side rib.

[0017] Optionally, the surface area of ​​the plating area of ​​the first side rib is smaller than the surface area of ​​the plating area of ​​the second side rib; the step of performing an electroplating process on the packaging structure includes: clamping the first side rib with a plating fixture, and placing the packaging structure in an electroplating solution for electroplating.

[0018] Optionally, the step of performing an electroplating process on the packaging structure includes: providing a shielding structure at the bottom of the electroplating solution; placing the packaging structure in the electroplating solution for electroplating, with the second side rib facing the shielding structure.

[0019] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:

[0020] An embodiment of the present invention provides a lead frame, wherein both a first side rib and a second side rib have openings, and areas where the first side rib and the second side rib are not provided with openings are plating areas. Compared with a solution where the first side rib and the second side rib do not have openings, the surface areas of the plating areas in the first side rib and the second side rib are reduced, so that during the packaging process, when the lead frame is subjected to an electroplating process, the uniformity of the current density per unit area at the positions of the first side rib and the second side rib is improved, thereby improving the problem of a thickness difference of the plating layer between the first side rib and the product area, and between the second side rib and the product area, thereby improving the Complex Process Capability Index (CPK) of the packaging.

[0021] The embodiment of the present invention further provides a packaging structure, comprising: a lead frame according to any embodiment of the present invention; and a plastic layer filling the opening and exposing the plating area of ​​the first side rib and the second side rib. Since the lead frame according to the embodiment of the present invention is used, the problem of the difference in plating thickness between the first side rib, the second side rib and the product area in the packaging structure is improved, thereby improving the process capability index of the packaging structure.

[0022] The embodiment of the present invention further provides an electroplating method, comprising: providing a packaging structure according to any embodiment of the present invention, wherein the packaging structure comprises a front side and a back side arranged opposite to each other; performing an electroplating process on the packaging structure to form a plating layer on the back side of the product area and the plating area of ​​the first side rib and the second side rib. Due to the use of the packaging structure according to the embodiment of the present invention, when the packaging structure is electroplated during the packaging process, the problem of the difference in plating thickness between the first side rib, the second side rib and the product area in the packaging structure is improved, thereby improving the process capability index of the packaging structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the structure of a lead frame;

[0024] Figure 2 is a schematic structural diagram of a first embodiment of a lead frame of the present invention;

[0025] Figure 3 is a schematic structural diagram of a second embodiment of a lead frame of the present invention;

[0026] Figure 4 is a schematic structural diagram of a first embodiment of a packaging structure of the present invention;

[0027] Figure 5 is a structural schematic diagram of a second embodiment of a packaging structure of the present invention;

[0028] Figure 6 to Figure 7 It is a schematic structural diagram corresponding to each step of the electroplating method for the packaging structure of the present invention. DETAILED DESCRIPTION

[0029] At present, the process capability index of packaging still needs to be improved. Now, combined with a structural schematic diagram of a lead frame, the reasons why the process capability index of packaging needs to be improved are analyzed. Figure 1 is a schematic diagram of the structure of a lead frame, specifically, Figure 1 This is a top view.

[0030] refer to Figure 1 The lead frame includes: a product area 10; a first side rib 11 and a second side rib 12 arranged in parallel, respectively located at two ends of the product area 10, and the first side rib 11 and the second side rib 12 both have a plating area 13.

[0031] Through research, it is found that as the size of the chip increases, the area size of the lead frame also increases, and accordingly the area size of the first side rib 11 and the second side rib 12 in the lead frame also increases, which easily leads to an increase in the area of ​​the plating area 13 of the first side rib 11 and the second side rib 12. During the packaging process, when the lead frame is electroplated, the area of ​​the plating area 13 of the first side rib 11 and the second side rib 12 increases, so that the current density divided by the first side rib 11 and the second side rib 12 is greater than the current density divided by the product area 10. At the same time, when the lead frame is electroplated, the first side rib 11 is clamped by an electroplating fixture, and the corresponding electroplating fixture is Part of the current will be diverted from the first side rib 11, so that the current density per unit area of ​​the plating area 13 at the position of the first side rib 11 is less than the current density per unit area of ​​the plating area 13 at the position of the second side rib 12. Therefore, due to the above two reasons, the current density uniformity between the first side rib 11 and the product area 10, between the second side rib 12 and the product area 10, and between the first side rib 11 and the second side rib 12 is poor, resulting in a problem of thickness difference in the plating between the first side rib 11 and the product area 10, between the second side rib 12 and the product area 10, and between the first side rib 11 and the second side rib 12, which in turn affects the process capability index of the package.

[0032] In order to solve the technical problem, an embodiment of the present invention provides a lead frame, including: a product area; a first side rib and a second side rib, respectively located at two ends of the product area, the first side rib and the second side rib both having openings, and the areas of the first side rib and the second side rib without openings are plating areas, along the arrangement direction of the first side rib and the second side rib, the first side rib and the second side rib both include multiple sub-side rib areas, and the openings are located in the multiple sub-side rib areas.

[0033] In the scheme disclosed in the embodiment of the present invention, since both the first side rib and the second side rib have openings, the surface area of ​​the plating area in the first side rib and the second side rib is reduced compared with the scheme in which the first side rib and the second side rib do not have openings. Therefore, during the packaging process, when the lead frame is subjected to the electroplating process, the uniformity of the current density per unit area at the positions of the first side rib and the second side rib is improved, thereby improving the problem of thickness difference of the plating between the first side rib and the product area, and between the second side rib and the product area, thereby improving the process capability index of the packaging.

[0034] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and understandable, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0035] Figure 2 is a schematic structural diagram of a first embodiment of a lead frame of the present invention, specifically, Figure 2 This is a top view.

[0036] refer to Figure 2 The lead frame includes: a product area 100; a first side rib 101 and a second side rib 102, which are respectively located at two ends of the product area 100, and the first side rib 101 and the second side rib 102 both have openings 103, and the areas of the first side rib 101 and the second side rib 102 without openings are plating areas 104, along the arrangement direction of the first side rib 101 and the second side rib 102, the first side rib 101 and the second side rib 102 both include a plurality of sub-side rib areas 105, and the openings 103 are located in the plurality of sub-side rib areas 105.

[0037] The lead frame is used as a carrier for encapsulating subsequent chips. At the same time, after the plastic encapsulation layer is formed subsequently, the bonding strength between the plastic encapsulation layer and the lead frame is high, so that the airtightness of the subsequently formed packaging structure is better.

[0038] As an example, the lead frame is a metal lead frame. In this embodiment, the material of the lead frame includes copper or iron-nickel alloy. Specifically, copper or iron-nickel alloy has good electrical conductivity, high thermal conductivity, low thermal expansion coefficient, and good corrosion resistance and oxidation resistance.

[0039] The product area 100 is used to place the chip. It should be noted that the product area 100 refers to the area of ​​the lead frame that needs to be packaged later.

[0040] In this embodiment, along the direction from the product area 100 to the sub-side rib area 105, the product area 100 includes three sub-product areas, namely, a first sub-product area 100A located near the first side rib 101; a second sub-product area 100C located near the second side rib 102; and a third sub-product area 100B located between the first sub-product area 100A and the second sub-product area 100C. In other embodiments, along the direction from the product area to the sub-side rib area, the product area may further include more sub-product areas, that is, there may be other sub-product areas between the first sub-product area located near the first side rib and the second sub-product area located near the second side rib.

[0041] In this embodiment, along a direction perpendicular to the direction from the product area 100 to the sub-rib area 105 , the sub-product area includes a plurality of unit areas A, and the unit areas A are used to prepare a single packaging structure.

[0042] It should be noted that the unit area A includes an area for mounting chips in a subsequent packaging process (not shown) and an area for forming a pin structure (not shown).

[0043] The first side rib 101 and the second side rib 102 both play a role in supporting the lead frame. It should be noted that, since the first side rib 101 and the second side rib 102 have openings 103, the openings 103 are used to reduce the surface area of ​​the plating area 104 of the first side rib 101 and the second side rib 102. Compared with the solution in which the first side rib 101 and the second side rib 102 do not have openings, the surface area of ​​the plating area 104 in the first side rib 101 and the second side rib 102 is reduced, so that during the packaging process, when the lead frame is subjected to the electroplating process, the uniformity of the current density per unit area at the position of the first side rib 101 and the second side rib 102 is improved, thereby improving the problem of the thickness difference of the plating between the first side rib 101 and the product area 100, and between the second side rib 102 and the product area 100, thereby improving the process capability index of the packaging.

[0044] The plating area 104 is used to provide a space for forming a plating layer and also to enhance the electrical conductivity and corrosion resistance of the lead frame.

[0045] In this embodiment, the surface area of ​​the coating region 104 of the first side rib 101 and the surface area of ​​the coating region 104 of the second side rib 102 are both less than 1 / 3 of the surface area of ​​the product area 100, which is beneficial to improving the uniformity of the thickness of the coating formed in the coating region 104 between the first side rib 101 and the product area 100 and between the second side rib 102 and the product area 100.

[0046] It should be noted that, since the first side rib 101 is clamped by an electroplating fixture during the subsequent electroplating process, the electroplating fixture will divert part of the current from the first side rib 101, and accordingly the current density per unit area of ​​the plating region 104 at the position of the first side rib 101 is smaller than the current density per unit area of ​​the plating region 104 at the position of the second side rib 102. In this embodiment, the surface area of ​​the plating region 104 of the first side rib 101 is smaller than the surface area of ​​the plating region 104 of the second side rib 102, thereby improving the uniformity of the current density per unit area of ​​the plating region 104 of the first side rib 101 and the current density per unit area of ​​the plating region 104 of the second side rib 102, thereby facilitating the improvement of the uniformity of the thickness of the plating formed between the plating region 104 of the first side rib 101 and the plating region 104 of the second side rib 102, and correspondingly improving the uniformity of the thickness of the plating between the first side rib 101 and the second side rib 102.

[0047] In this embodiment, the opening 103 is a through hole that penetrates the lead frame in the thickness direction. In the subsequent plastic encapsulation process, the plastic encapsulation material fills the through hole structure. In other embodiments, the opening can also be a blind hole that is opened on any side of the lead frame.

[0048] The shape of the cross section of the opening 103 includes one or more of a circle, an ellipse and a polygon, which is conducive to flexibly adjusting the surface area of ​​the coating region 104 in the first side rib 101 and the second side rib 102; at the same time, it is conducive to reducing the process difficulty of forming the opening 103 in the first side rib 101 and the second side rib 102.

[0049] As an example, the cross-section of the opening 103 is in the shape of a triangle.

[0050] It should be noted that, during the electroplating process, the current density is different in the direction from the product area 100 to the sub-edge rib area 105. Figure 2 In the embodiment shown in the figure, along the arrangement direction of the first side rib 101 and the second side rib 102 (such as Figure 2The first side rib 101 and the second side rib 102 each include a plurality of sub-side rib areas 105, which is conducive to flexibly forming the opening 103 according to the areas of different sub-side rib areas 105, thereby facilitating improvement of the problem of thickness difference of the plating layer between the first side rib 101 and the product area 100, and between the second side rib 102 and the product area 100, thereby improving the process capability index of the package.

[0051] As an example, along the arrangement direction of the first side rib 101 and the second side rib 102, the first side rib 101 and the second side rib 102 each include three sub-side rib regions 105, and each of the three sub-side rib regions 105 has an opening 103 with a triangular cross-section. The cross-sectional areas of the openings 103 in the three sub-side rib regions 105 decrease sequentially, that is, the surface areas of the plating regions 104 in the three sub-side rib regions 105 increase sequentially.

[0052] In this embodiment, the opening 103 is located in the plurality of sub-side rib areas 105, which is beneficial to reducing the surface area of ​​the plating area 104 in the sub-side rib area 105, and correspondingly reducing the surface area of ​​the plating area 104 in the first side rib 101 and the second side rib 102. Therefore, during the packaging process, when the lead frame is subjected to the electroplating process, the uniformity of the current density per unit area at the positions of the first side rib 101 and the second side rib 102 is improved, thereby improving the problem of thickness difference of the plating between the first side rib 101 and the product area 100, and between the second side rib 102 and the product area 100, thereby improving the process capability index of the packaging.

[0053] In this embodiment, in any one of the first side rib 101 and the second side rib 102, the opening 103 located in the plurality of the sub-side rib regions 105 satisfies one or more of the following conditions: the shapes of the openings 103 in the plurality of the sub-side rib regions 105 are different (for example, among the three sub-side rib regions 105, the shape of the opening 103 in the sub-side rib region close to the first side rib 101 or the second side rib 102 may be circular, the shape of the opening 103 in the sub-side rib region 105 far away from the first side rib 101 or the second side rib 102 may be hexagonal, and the shape of the opening 103 in the middle may be hexagonal. The shape of the opening 103 in the sub-side rib area 105 is a triangle); the line widths of the openings 103 in the multiple sub-side rib areas 105 are different (for example, along the arrangement direction of the first side rib 101 and the second side rib 102, the line widths of the openings 103 in the three sub-side rib areas 105 decrease successively); the number of the openings 103 in the multiple sub-side rib areas 105 is different (for example, along the arrangement direction of the first side rib 101 and the second side rib 102, the number of the openings 103 in the three sub-side rib areas 105 decreases successively).

[0054] Specifically, by controlling the shape, line width, and number of the openings 103 in the plurality of sub-side rib areas 105, the surface area of ​​the plating area 104 in the first side rib 101 and the second side rib 102 is adjusted, so that the surface area of ​​the plating area 104 in the first side rib 101 and the second side rib 102 meets the actual process requirements.

[0055] It should be noted that, when the line width size and the number of the openings 103 are the same, the surface area of ​​the plated region 104 in the first side rib 101 and the second side rib 102 can be adjusted by changing the shape of the openings 103; when the line width size and the shape of the openings 103 are the same, the surface area of ​​the plated region 104 in the first side rib 101 and the second side rib 102 can be adjusted by changing the number of the openings 103; when the number and the shape of the openings 103 are the same, the surface area of ​​the plated region 104 in the first side rib 101 and the second side rib 102 can be adjusted by changing the line width size of the openings 103.

[0056] It should also be noted that, when the line width dimensions of the openings 103 are the same, the surface area of ​​the plated region 104 in the first side rib 101 and the second side rib 102 can be adjusted by changing the shape and number of the openings 103; when the shapes of the openings 103 are the same, the surface area of ​​the plated region 104 in the first side rib 101 and the second side rib 102 can be adjusted by changing the line width dimensions and the number of the openings 103; when the number of openings 103 is the same, the surface area of ​​the plated region 104 in the first side rib 101 and the second side rib 102 can be adjusted by changing the line width dimensions and the shape of the openings 103.

[0057] In addition, the line width, shape and number of the openings 103 may also be changed simultaneously to adjust the surface area of ​​the plated region 104 in the first side rib 101 and the second side rib 102 .

[0058] In this embodiment, in any one of the first side rib 101 and the second side rib 102, along the direction of the product area 100 pointing to the sub-side rib area 105, the total cross-sectional area of ​​the openings 103 in the plurality of sub-side rib areas 105 decreases successively.

[0059] It should be noted that, during the packaging process, when the lead frame is subjected to the electroplating process, the current density increases successively in the direction from the product area 100 to the sub-side rib area 105. Therefore, along the direction from the product area 100 to the sub-side rib area 105, the total cross-sectional area of ​​the openings 103 in the multiple sub-side rib areas 105 decreases successively, that is, along the direction from the product area 100 to the sub-side rib area 105, the surface area of ​​the plating area 104 in the multiple sub-side rib areas 105 increases successively, which is beneficial to improve the uniformity of the current density per unit area of ​​the plating area 104 of the sub-side rib area 105, and further improves the problem of thickness difference of the plating between the first side rib 101 and the product area 100, and between the second side rib 102 and the product area 100, thereby improving the process capability index of the package.

[0060] In this embodiment, in any one of the first side rib 101 and the second side rib 102, along the direction of the product area 100 pointing to the sub-side rib area 105, the openings 103 in the plurality of sub-side rib areas 105 meet one or more of the following conditions: the density of the openings 103 in the plurality of sub-side rib areas 105 decreases successively; the number of the openings 103 in the plurality of sub-side rib areas 105 decreases successively; the line width of the openings 103 in the plurality of sub-side rib areas 105 decreases successively. Specifically, through the above method, along the direction of the product area 100 pointing to the sub-side rib area 105, the total cross-sectional area of ​​the openings 103 in the plurality of sub-side rib areas 105 decreases successively.

[0061] It should be noted that the product area 100 points in the direction of the sub-side rib area 105. When the density and number of the openings 103 in the multiple sub-side rib areas 105 are the same, the line width of the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence so that the total cross-sectional area of ​​the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence; when the density and line width of the openings 103 in the multiple sub-side rib areas 105 are the same, the number of the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence so that the total cross-sectional area of ​​the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence; when the number and line width of the openings 103 in the multiple sub-side rib areas 105 are the same, the density of the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence so that the total cross-sectional area of ​​the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence.

[0062] It should also be noted that, when the product area 100 points in the direction of the sub-side rib area 105 and the densities of the openings 103 in the multiple sub-side rib areas 105 are the same, the line width and number of the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence so that the total cross-sectional area of ​​the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence; when the line widths of the openings 103 in the multiple sub-side rib areas 105 are the same, the number and density of the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence so that the total cross-sectional area of ​​the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence; when the number of the openings 103 in the multiple sub-side rib areas 105 is the same, the density and line width of the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence so that the total cross-sectional area of ​​the openings 103 in the multiple sub-side rib areas 105 can be reduced in sequence.

[0063] In addition, the density, line width and number of the openings 103 in the plurality of sub-edge rib regions 105 may be reduced simultaneously and sequentially, so that the total cross-sectional area of ​​the openings 103 in the plurality of sub-edge rib regions 105 is reduced sequentially.

[0064] It should be noted that, during the packaging process, when the lead frame is subjected to an electroplating process, under the condition of the same current, in the direction from the product area 100 to the sub-side rib area 105, since the total cross-sectional area of ​​the openings 103 in the plurality of sub-side rib areas 105 decreases successively, it means that the surface areas of the plating areas 104 in the plurality of sub-side rib areas 105 increase successively. Therefore, in the direction from the product area 100 to the sub-side rib area 105, the thickness of the plating in the plating areas 104 in the plurality of sub-side rib areas 105 decreases successively, that is, the thickness of the plating in the plating area 104 of the sub-side rib area 105 closest to the product area 100 is the largest, and the thickness of the plating in the plating area 104 of the sub-side rib area 105 far from the product area 100 is less than the thickness of the plating in the plating area 104 of the sub-side rib area 105 closest to the product area 100.

[0065] As an example, the thickness of the coating in the coating area 104 of the sub-edge rib area 105 close to the product area 100 is 10 microns to 13 microns, and the thickness of the coating in the product area 100 is 13 microns to 16 microns. Therefore, the difference in coating thickness between the two is less than 3 microns, and the process capability index of the package is greater than 1.67, which meets the actual process requirements.

[0066] Figure 3is a schematic structural diagram of a second embodiment of a lead frame of the present invention, specifically, Figure 3 This is a top view.

[0067] The similarities between this embodiment and the above embodiment are not described in detail here. The difference between this embodiment and the above embodiment is that the opening 103 is a blind hole, wherein the blind hole is located on any surface of the lead frame.

[0068] In other embodiments, the types of the openings include both through holes and blind holes, that is, two types of openings are provided on the lead frame.

[0069] As an example, the cross-section of the blind hole is in the shape of a hexagon. In other embodiments, it can also be other polygons. The blind hole can also be in the shape of a circle, an ellipse, etc.

[0070] Correspondingly, an embodiment of the present invention also provides a packaging structure.

[0071] Figure 4 is a schematic structural diagram of a first embodiment of a packaging structure of the present invention, specifically, Figure 4 This is a top view.

[0072] refer to Figure 4 The packaging structure includes: a lead frame 200 according to any embodiment of the present invention; a plastic layer 201, which fills the opening (not shown) and exposes the plating area 205 of the first side rib 203 and the second side rib 204.

[0073] It should be noted that, since the lead frame 200 described in the embodiment of the present invention is adopted, the problem of the difference in plating thickness between the first side rib 203, the second side rib 204 and the product area 206 in the packaging structure is improved, thereby improving the process capability index of the packaging structure.

[0074] The lead frame 200 is used as a carrier for packaging the chip. At the same time, after the plastic packaging layer 201 is formed, the bonding strength between the plastic packaging layer 201 and the lead frame 200 is high, so that the airtightness of the packaging structure is better.

[0075] As an example, the lead frame 200 is a metal lead frame. In this embodiment, the material of the lead frame 200 includes copper or iron-nickel alloy. Specifically, copper or iron-nickel alloy has good electrical conductivity, high thermal conductivity, low thermal expansion coefficient, and good corrosion resistance and oxidation resistance.

[0076] In this embodiment, the lead frame 200 includes a front side (not labeled) and a back side (not labeled) that are oppositely disposed.

[0077] The front side of the lead frame 200 is used to place a chip. Specifically, the lead frame 200 includes a product area 206, and the front side of the product area 206 is used to place a chip.

[0078] It should be noted that the product area 206 refers to the area where the lead frame 200 needs to be packaged.

[0079] In this embodiment, along a direction perpendicular to the direction in which the product area 206 points to the sub-rib area (not shown), the sub-product area includes a plurality of unit areas (not shown), and the unit areas are used to prepare a single packaging structure.

[0080] It should be noted that the unit area includes an area for mounting chips during packaging (not shown) and an area for forming a pin structure (not shown).

[0081] The lead frame 200 further includes a first side rib 203 and a second side rib 204, both of which play a role in supporting the lead frame 200. It should be noted that, since both the first side rib 203 and the second side rib 204 have openings (not shown), the openings are used to reduce the surface area of ​​the plating region 205 of the first side rib 203 and the second side rib 204. Compared with the solution in which the first side rib 203 and the second side rib 204 do not have openings, the surface area of ​​the plating region 205 in the first side rib 203 and the second side rib 204 is reduced, so that in the packaging process, when the lead frame 200 is subjected to the electroplating process, the uniformity of the current density per unit area at the position of the first side rib 203 and the second side rib 204 is improved, thereby improving the problem of the thickness difference of the plating layer between the first side rib 203 and the product region 206, and between the second side rib 204 and the product region 206, thereby improving the process capability index of the packaging.

[0082] The plating area 205 is used to provide a space for forming a plating layer and also to enhance the electrical conductivity and corrosion resistance of the lead frame 200 .

[0083] In this embodiment, the type of the opening is a through hole, which penetrates the lead frame 200 along the thickness direction. In the subsequent plastic encapsulation process, the plastic encapsulation material fills the through hole. In other embodiments, the opening can also be a blind hole, which is opened on any side of the lead frame.

[0084] It should be noted that the type of opening is a through hole, which penetrates the lead frame 200 along the thickness direction. Therefore, the surface area of ​​the front side of the first side rib 203 and the second side rib 204 and the surface area of ​​the plated area 205 on the back side of the first side rib 203 and the second side rib 204 can be reduced at the same time, which is beneficial to reducing the number of openings, thereby improving the mechanical strength of the first side rib 203 and the second side rib 204.

[0085] The shape of the cross section of the opening includes one or more of a circle, an ellipse and a polygon, which is conducive to flexibly adjusting the surface area of ​​the coating area 205 in the first side rib 203 and the second side rib 204; at the same time, it is conducive to reducing the process difficulty of forming the opening in the first side rib 203 and the second side rib 204.

[0086] As an example, the cross-section of the opening is in the shape of a triangle.

[0087] The plastic packaging layer 201 is used to protect the chips on the product area 206 in the lead frame 200 and is also used to achieve insulation.

[0088] In this embodiment, the plastic encapsulation layer 201 is filled in the opening, which is beneficial for evenly distributing stress on the first side rib 203 and the second side rib 204 in the subsequent process, thereby improving the problem of stress concentration and further reducing the probability of deformation of the lead frame 200.

[0089] In this embodiment, the material of the plastic encapsulation layer 201 is a plastic encapsulation material, such as epoxy resin. Epoxy resin has the advantages of low shrinkage, good adhesion, good corrosion resistance, excellent electrical properties and low cost. In other embodiments, the plastic encapsulation layer can also be made of other suitable materials.

[0090] It should be noted that, since the type of the opening is a through hole, the plastic encapsulation layer 201 is filled into the through hole accordingly.

[0091] The packaging structure further includes: a chip (not shown), which is disposed on one side of the lead frame 200 and located in the product area 206 , and the chip is electrically connected to the lead frame 200 .

[0092] As an example, the chip is disposed on one side of the front surface of the lead frame 200 .

[0093] The chip is used to be electrically connected to the lead frame 200 to form a corresponding packaging structure to achieve corresponding functions.

[0094] The plastic packaging layer 201 also covers the chips in the product area 206 to achieve insulation and protect the chips.

[0095] In this embodiment, the formed packaging structure can be packaged in the form of a quad flat no leads package (Quad Flat Noleads Package, QFN).

[0096] In other embodiments, the formed packaging structure may also adopt a SMD small power transistor package (Small Outline Transistor, SOT) and a small outline package (Small Out-Line Package, SOP).

[0097] Figure 5 is a schematic structural diagram of a second embodiment of a packaging structure of the present invention. Specifically, Figure 5 This is a top view.

[0098] The similarities between this embodiment and the above embodiment are not described in detail here. The difference between this embodiment and the above embodiment is that the type of the opening (not marked) is a blind hole.

[0099] It should be noted that, since the lead frame 200 described in the embodiment of the present invention is adopted, the problem of the difference in plating thickness between the first side rib 203, the second side rib 204 and the product area 206 in the packaging structure is improved, thereby improving the process capability index of the packaging structure.

[0100] It should also be noted that since the opening is a blind hole, that is, the opening does not need to penetrate the first side rib 203 and the second side rib 204, therefore, in the process of filling the plastic sealing layer 201 in the opening, compared with the solution of filling the plastic sealing layer into the through hole, it is beneficial to reduce the amount of material used in the plastic sealing layer 201, thereby reducing production costs; in addition, the blind hole can also improve the mechanical strength of the first side rib 203 and the second side rib 204.

[0101] It should be further explained that, since the type of the opening is a blind hole, when the plastic encapsulation layer 201 fills the opening, the plastic encapsulation layer 201 in the first side rib 203 and the second side rib 204 is only formed on the side with the blind hole.

[0102] In other embodiments, the types of the openings include both through holes and blind holes, that is, two types of openings are provided on the lead frame.

[0103] As an example, the cross-section of the blind hole is in the shape of a hexagon. In other embodiments, it can also be other polygons. The blind hole can also be in the shape of a circle, an ellipse, etc.

[0104] As an example, a flow channel is provided between adjacent blind holes, and the flow channel is a groove provided on the side rib, and the flow channel is used for filling and flowing of the plastic encapsulation material in the blind hole.

[0105] Accordingly, an embodiment of the present invention also provides an electroplating method. Figure 6 and Figure 7 , showing the structural schematic diagram corresponding to each step of the electroplating method of the packaging structure of the present invention, wherein: Figure 6is the top view of the lead frame. Figure 7 Schematic diagram of the lead frame placed in the plating solution.

[0106] refer to Figure 6 , providing a packaging structure 500 as described in any embodiment of the present invention, the packaging structure 500 includes a front side (not marked) and a back side (not marked) arranged relatively to each other, and the front side of the packaging structure 500 is used for arranging a chip.

[0107] Specifically, the packaging structure 500 includes: a lead frame 300 according to any embodiment of the present invention; and a plastic packaging layer 307 filled in the opening (not marked).

[0108] The lead frame 300 is used as a carrier for packaging the chip, and the front side of the lead frame 300 is used to place the chip.

[0109] As an example, the lead frame 300 is a metal lead frame. In this embodiment, the material of the lead frame 300 includes copper or iron-nickel alloy. Specifically, copper or iron-nickel alloy has good electrical conductivity, high thermal conductivity, low thermal expansion coefficient, and good corrosion resistance and oxidation resistance.

[0110] The lead frame 300 includes a product area 301, and the product area 301 is used to place a chip. It should be noted that the product area 301 refers to: an area of ​​the lead frame 300 that needs to be packaged.

[0111] The lead frame 300 further includes a first side rib 302 and a second side rib 303, both of which play a role in supporting the lead frame 300, and both of which have openings. The openings are used to reduce the surface area of ​​the plating region 304 of the first side rib 302 and the second side rib 303. Compared with the solution in which the first side rib 302 and the second side rib 303 do not have openings, the surface area of ​​the plating region 304 in the first side rib 302 and the second side rib 303 is reduced, so that in the packaging process, when the lead frame 300 is subjected to the electroplating process, the uniformity of the current density per unit area at the position of the first side rib 302 and the second side rib 303 is improved, thereby improving the problem of the thickness difference of the plating layer between the first side rib 302 and the product region 301, and between the second side rib 303 and the product region 301, thereby improving the process capability index of the packaging.

[0112] The type of the opening includes one or both of a through hole and a blind hole. In this embodiment, the through hole is taken as an example.

[0113] It should be noted that, since the electroplating fixture 310 is used to clamp the first side rib 302 during the electroplating process, the electroplating fixture 310 will divert part of the current from the first side rib 302, and accordingly, the current density per unit area of ​​the plating area 304 at the position of the first side rib 302 is smaller than the current density per unit area of ​​the plating area 304 at the position of the second side rib 303. In this embodiment, the surface area of ​​the plating area 304 of the first side rib 302 is smaller than the surface area of ​​the plating area 304 of the second side rib 303, thereby improving the uniformity of the current density per unit area of ​​the plating area 304 of the first side rib 302 and the plating area 304 of the second side rib 303, thereby facilitating improving the uniformity of the thickness of the plating formed between the plating area 304 of the first side rib 302 and the plating area 304 of the second side rib 303, and correspondingly improving the uniformity of the thickness of the plating between the first side rib 302 and the second side rib 303.

[0114] The plastic packaging layer 307 is used to protect the chips on the product area 301 in the lead frame 300 and is also used to achieve insulation.

[0115] It should be noted that filling the plastic encapsulation layer 307 in the opening is beneficial for evenly distributing stress on the first side rib 302 and the second side rib 303 in the subsequent process, thereby improving the problem of stress concentration and further reducing the probability of deformation of the lead frame 300.

[0116] Combined with reference Figure 6 to Figure 7 , the packaging structure 500 is subjected to an electroplating process to form a plating layer on the back side of the product area 301 and the plating area 304 of the first side rib 302 and the second side rib 303 (not shown).

[0117] Specifically, since the packaging structure 500 adopts the lead frame 300 described in the embodiment of the present invention, during the packaging process, when the lead frame 300 is subjected to the electroplating process, the problem of the difference in plating thickness between the first side rib 302, the second side rib 303 and the product area 301 in the packaging structure 500 is improved, thereby improving the process capability index of the packaging structure.

[0118] In this embodiment, the step of performing an electroplating process on the package structure 500 includes: clamping the first side rib 302 with an electroplating fixture 310, and placing the package structure 500 in an electroplating solution for electroplating.

[0119] It should be noted that, during the electroplating process, since the electroplating fixture 310 is used to clamp the first side rib 302, it is beneficial to fix the first side rib 302, and it is easy to reduce the swing of the first side rib 302 in the electroplating solution, and correspondingly reduce the swing of the packaging structure 500 in the electroplating solution, thereby reducing the probability of mechanical damage to the packaging structure 500 caused by collision, thereby providing a smooth surface for the subsequently formed coating, and improving the uniformity of the thickness of the coating formed on the packaging structure 500.

[0120] In this embodiment, the material of the electroplating fixture 310 includes stainless steel SUS304 or the like.

[0121] In this embodiment, the step of performing an electroplating process on the packaging structure 500 includes: a shielding structure 311 is provided at the bottom of the electroplating solution; and the packaging structure 500 is placed in the electroplating solution for electroplating, with the second side rib 303 facing the shielding structure 311 .

[0122] During the electroplating process, the shielding structure 311 is used to shield excess current.

[0123] In this embodiment, the material of the shielding structure 311 includes polypropylene (PP), polyvinyl chloride (PVC), etc.

[0124] In this embodiment, the shielding structure 311 is concave in shape, and has a groove 312 therein.

[0125] It should be noted that since the surface area of ​​the plating area 304 of the first side rib 302 is smaller than the surface area of ​​the plating area 304 of the second side rib 303, when the electroplating process is performed, the second side rib 303 is directed toward the shielding structure 311, which is beneficial for controlling the uniformity of the current density per unit area of ​​the plating area 304 of the second side rib 303 and the current density per unit area of ​​the plating area 304 of the first side rib 302 through the shielding structure 311, thereby improving the uniformity of the thickness of the plating area 304 of the second side rib 303 and the plating area 304 of the first side rib 302.

[0126] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A lead frame, characterized in that: include: Product area; The first side rib and the second side rib are respectively located at the two ends of the product area, and the first side rib and the second side rib both have openings, and the areas of the first side rib and the second side rib without openings are coating areas, and along the arrangement direction of the first side rib and the second side rib, the first side rib and the second side rib both include a plurality of sub-side rib areas, and the openings are located in the plurality of sub-side rib areas.

2. The lead frame according to claim 1, wherein: In any one of the first side rib and the second side rib, the opening located in the plurality of sub-side rib regions satisfies one or more of the following conditions: The shapes of the openings in the plurality of sub-side rib regions are different; The line widths of the openings in the plurality of sub-edge rib regions are different; The numbers of the openings in the plurality of sub-rib regions are different.

3. The lead frame according to claim 1, wherein: In any one of the first side rib and the second side rib, along the direction from the product area to the sub-side rib area, the total cross-sectional areas of the openings in a plurality of the sub-side rib areas decrease sequentially.

4. The lead frame according to claim 3, wherein: In any one of the first side rib and the second side rib, along the direction from the product area to the sub-side rib area, the openings in the plurality of sub-side rib areas satisfy one or more of the following conditions: The density of the openings in the plurality of sub-side rib regions decreases sequentially; The number of the openings in the plurality of sub-side rib regions decreases successively; The line widths of the openings in the plurality of sub-edge rib regions decrease in sequence.

5. The lead frame according to any one of claims 1 to 4, wherein: The surface area of ​​the plated region of the first side rib and the surface area of ​​the plated region of the second side rib are both smaller than 1 / 3 of the surface area of ​​the product region.

6. The lead frame according to any one of claims 1 to 4, wherein: The surface area of ​​the plated region of the first side rib is smaller than the surface area of ​​the plated region of the second side rib.

7. The lead frame according to any one of claims 1 to 4, characterized in that: The type of the opening includes one or both of a through hole structure and a blind hole structure; Wherein, the blind hole is located on any surface of the lead frame.

8. The lead frame according to any one of claims 1 to 4, wherein: The cross-sectional shape of the opening includes one or more of a circle, an ellipse and a polygon.

9. A packaging structure, characterized in that: include: The lead frame according to any one of claims 1 to 8; A plastic packaging layer fills the opening and exposes the plating areas of the first side rib and the second side rib.

10. The packaging structure according to claim 9, characterized in that: The packaging structure further includes: a chip, which is disposed on one side of the lead frame and located in the product area, and the chip is electrically connected to the lead frame; The plastic packaging layer also covers the chips in the product area.

11. An electroplating method, characterized in that: include: Provide a packaging structure as claimed in any one of claims 9 to 10, wherein the packaging structure comprises a front side and a back side arranged opposite to each other, and the front side of the packaging structure is used for arranging a chip; The packaging structure is subjected to an electroplating process to form a plating layer on the back side of the product area and the plating areas of the first side rib and the second side rib.

12. The electroplating method according to claim 11, characterized in that: The surface area of ​​the plated region of the first side rib is smaller than the surface area of ​​the plated region of the second side rib; The step of performing an electroplating process on the packaging structure includes: clamping the first edge rib with an electroplating fixture, and placing the packaging structure in an electroplating solution for electroplating.

13. The electroplating method according to claim 11 or 12, characterized in that: The step of performing an electroplating process on the packaging structure includes: a shielding structure is provided at the bottom of the electroplating solution; the packaging structure is placed in the electroplating solution for electroplating, and the second side rib faces the shielding structure.