Positive pole piece and preparation method thereof, battery and power utilization device

By designing sodium-containing cathode sheets in lithium-ion batteries, utilizing the cathode active material layer of layered oxides and polyanionic compounds, combined with sodium-supplementing additives, the low energy density and cycle performance of the cathode sheets of lithium-ion batteries are solved. problem, achieving structural stability and alleviating expansion stress.

CN118738263APending Publication Date: 2024-10-01CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310322609.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode plates and their preparation methods suffer from insufficient sodium resources and structural instability, resulting in low energy density and cycle performance.

Method used

A cathode electrode sheet is designed, which includes a cathode current collector and a cathode active material layer. The cathode active material layer is composed of a sodium-containing layered oxide and a polyanionic compound, with a porosity of 25%-50%, and performs during charge and discharge. During the process, the thickness changes are used to adapt to the expansion stress of the negative electrode piece and reduce the volume expansion of the battery.

Benefits of technology

It improves the structural stability and energy density of the battery, extends the service life of the battery, and compensates for the sodium consumption during the cycle through sodium supplementation additives, improving the cycle performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738263A_ABST
    Figure CN118738263A_ABST
Patent Text Reader

Abstract

The invention discloses a positive pole piece, a preparation method of the positive pole piece, a battery and a power utilization device. The positive electrode active material layer is arranged on the surface of at least one side of the positive electrode current collector, the positive electrode active material layer comprises a positive electrode active material, the positive electrode active material comprises a sodium-containing positive electrode active material, the thickness of the positive electrode plate meets the condition that Dmax / Dmin is 104.5%-300%, and after the positive electrode plate and the negative electrode plate are assembled into the battery, the thickness of the positive electrode plate is smaller than that of the negative electrode plate. The thickness of the positive pole piece is Dmax when the battery is in 0% SOC, the thickness of the positive pole piece is Dmin when the battery is in 100% SOC, the negative pole piece comprises a negative current collector, and at least one side surface of the negative current collector is provided with a sodium metal layer when the battery is in 100% SOC. The positive pole piece can relieve the stress change caused by the volume change of the negative pole piece in the charging and discharging process, so that the volume expansion of the battery in the working process is reduced, and the structural stability of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and in particular, to a positive electrode plate and a preparation method thereof, a battery and an electrical device. Background Art

[0002] As the application of lithium-ion battery technology in consumer electronics, electric vehicles, energy storage and other markets gradually expands, the problem of insufficient lithium resources has also begun to become prominent. Sodium-based batteries have gradually attracted attention because the earth has a sufficiently high abundance of sodium, and they have an important strategic position in cost-sensitive application fields such as energy storage. With the development and progress of electrolyte and its additive technology and surface modification technology, the problem of sodium dendrite growth caused by uneven deposition on metal surfaces that has long plagued the academic community has been significantly improved, allowing high-energy-density sodium metal negative electrodes to re-enter people's field of vision.

[0003] Therefore, the current positive electrode plates and preparation methods thereof, batteries and electrical devices still need to be improved. Summary of the invention

[0004] The present application aims to alleviate or solve at least one of the above-mentioned problems to at least some extent.

[0005] In one aspect of the present application, the present application proposes a positive electrode sheet, comprising: a positive electrode current collector; a positive electrode active material layer, wherein the positive electrode active material layer is disposed on at least one side surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, wherein the positive electrode active material comprises a sodium-containing positive electrode active material, and wherein the thickness of the positive electrode sheet satisfies D max / D min 104.5%-300%, wherein after the positive electrode sheet and the negative electrode sheet are assembled into a battery, the thickness of the positive electrode sheet when the battery is at 0% SOC is D max When the battery is at 100% SOC, the thickness of the positive electrode sheet is D min , wherein the negative electrode plate includes a negative electrode current collector, and when the battery is at 100% SOC, at least one side of the surface of the negative electrode current collector has a sodium metal layer. The positive electrode plate in the present application can alleviate the stress change caused by the volume change of the negative electrode plate during the charging and discharging process, thereby reducing the volume expansion of the battery during operation and improving the structural stability of the battery.

[0006] According to an embodiment of the present application, the porosity of the positive electrode active material layer is 25%-50%. Thus, the stress change caused by the expansion and contraction of the negative electrode sheet can be alleviated by the pore structure of the positive electrode sheet.

[0007] According to an embodiment of the present application, the positive electrode active material includes a layered oxide, and the layered oxide satisfies the chemical formula Na x My O2, wherein 0<x≤4.5, 0<y≤1, and M element includes at least one of Ti, V, Cr, Fe, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La and Ce; preferably, the M element includes at least one of Ti, V, Cr, Fe, Co, Mn, Ni, Cu and Zn. Thus, the manufacturing cost of the positive electrode sheet can be reduced and the energy density of the positive electrode sheet can be improved.

[0008] According to an embodiment of the present application, the positive electrode active material includes a polyanionic compound, the cationic element of the polyanionic compound includes at least one of Ni, V, Co, Fe, Mn and Cu, and the anion of the polyanionic compound includes F - PO4 3- 、P2O7 4- and (PO4)2P2O7 10- At least one of; Preferably, the anion of the polyanionic compound includes F - Thus, the manufacturing cost of the positive electrode sheet can be reduced and the energy density of the positive electrode sheet can be increased.

[0009] According to an embodiment of the present application, the anion of the polyanionic compound includes PO4 3- and P2O7 4- , the P2O7 in the polyanionic compound 4- With the PO4 3- The molar ratio of P2O7 is 0.1-5; preferably, the P2O7 4- With the PO4 3- The molar ratio of is 0.1-3. Thus, the manufacturing cost of the positive electrode sheet can be further reduced and the energy density of the positive electrode sheet can be increased.

[0010] According to an embodiment of the present application, the positive electrode active material layer further includes a sodium supplement additive, the mass fraction of the positive electrode active material in the positive electrode active material layer is 50wt%-98wt%, and the mass fraction of the sodium supplement additive in the positive electrode active material layer is 2wt%-50wt%. Thus, the energy density of the battery can be improved by the sodium supplement additive; on the other hand, the lithium supplement additive can also be used to compensate for the sodium consumption during the cycle and improve the cycle performance of the battery.

[0011] According to an embodiment of the present application, the sodium supplement additive includes at least one of Na2S, NaN3, Na2NiO2, NaC6H5O7, Na2O, Na2O2, Na6CoO4, Na5FeO4, Na2C2O4, Na2C4O4, Na2C3O5, Na2C4O6 and Na2C6O6. Thus, the energy density and cycle performance of the battery can be further improved.

[0012] According to an embodiment of the present application, the thickness of the negative electrode sheet satisfies d max / d min is 100%-700%, wherein the d max is the thickness of the negative electrode sheet when the battery is at 100% SOC, and the d min is the thickness of the negative electrode sheet when the battery is at 0% SOC. Thus, the aforementioned positive electrode sheet can meet the use of negative electrode sheets with a larger thickness variation rate in the battery.

[0013] In another aspect of the present application, the present application proposes a method for preparing the aforementioned positive electrode sheet, comprising: providing a positive electrode current collector; providing a positive electrode slurry, and coating the positive electrode slurry on at least one side of the positive electrode current collector to form a positive electrode active material layer. Therefore, the method has all the features and advantages of the aforementioned positive electrode sheet, which will not be described in detail here.

[0014] According to an embodiment of the present application, providing the positive electrode slurry includes: uniformly mixing the positive electrode active material and the sodium supplement additive in a solvent; and after forming the positive electrode active material layer, further includes: assembling the positive electrode plate and the negative electrode plate into a battery, and performing a formation treatment. Thus, the porosity of the positive electrode active material layer can be further improved.

[0015] According to an embodiment of the present application, before coating the positive electrode slurry on at least one side of the positive electrode current collector, the method further includes: arranging a sodium foil on the surface of the positive electrode current collector for coating the positive electrode slurry. Thus, a positive electrode sheet with a higher energy density can be prepared.

[0016] In another aspect of the present application, the present application proposes a battery, comprising: a positive electrode sheet, a negative electrode sheet, and a separator located between the positive electrode sheet and the negative electrode sheet, wherein the positive electrode sheet is the aforementioned positive electrode sheet, and / or the positive electrode sheet prepared by the aforementioned method, the negative electrode sheet includes a negative electrode current collector, and the thickness of the negative electrode sheet satisfies d max / d min is 100%-700%, wherein the d max is the thickness of the negative electrode sheet when the battery is at 100% SOC, and the d minis the thickness of the negative electrode sheet when the battery is at 0% SOC. Therefore, the battery has all the features and advantages of the positive electrode sheet and the method for preparing the positive electrode sheet, which will not be described in detail here.

[0017] In another aspect of the present application, the present application proposes an electrical device, comprising: the aforementioned positive electrode sheet, and / or, the positive electrode sheet prepared by the aforementioned method, and / or, the aforementioned battery. Therefore, the electrical device has all the features and advantages of the aforementioned positive electrode sheet, the method for preparing the positive electrode sheet, and the aforementioned battery, which will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0019] Figure 1 A schematic diagram showing the structure of a battery at 0% SOC according to an embodiment of the present application is shown;

[0020] Figure 2 A schematic diagram showing the structure of a battery at 100% SOC according to an embodiment of the present application is shown;

[0021] Figure 3 A schematic diagram showing the structure of a battery at 60% SOC according to an embodiment of the present application is shown;

[0022] Figure 4 A schematic diagram of a battery according to an embodiment of the present application is shown;

[0023] Figure 5 Shows Figure 4 An exploded view of a battery according to an embodiment of the present application is shown;

[0024] Figure 6 A schematic diagram of a battery module according to an embodiment of the present application is shown;

[0025] Figure 7 A schematic diagram of a battery pack according to an embodiment of the present application is shown;

[0026] Figure 8 Shows Figure 7 An exploded view of a battery pack according to an embodiment of the present application is shown;

[0027] Fig. 9 A schematic diagram of an electric device using a battery as a power source according to an embodiment of the present application is shown.

[0028] Description of reference numerals:

[0029] 1: battery pack; 2: upper case; 3: lower case; 4: battery module; 5: battery; 11: negative electrode current collector; 12: sodium metal layer; 21: positive electrode current collector; 22: positive electrode active material layer; 30: isolation membrane; 40: electrolyte; 51: shell; 52: electrode assembly; 53: top cover assembly. DETAILED DESCRIPTION

[0030] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.

[0031] In the description of this application, SOC refers to the state of charge of the battery, which can reflect the remaining capacity of the battery. It is numerically defined as the ratio of the remaining capacity to the battery capacity, usually expressed as a percentage, with a value range of 0%-100%. "100% SOC" refers to the state when the battery is charged to the maximum design voltage at a constant current of 1C and then switched to constant voltage charging to 0.05C, including the state after standing (generally standing for 10 minutes), which are all considered to be 100% SOC state, that is, fully charged state. "60% SOC" refers to the state when the electrochemical device is charged to 60% state of charge at a constant current. The battery can be adjusted to 60% SOC state by referring to the following method: first fully charge the battery, and then discharge it at a constant current of 1C for 12 minutes. At this time, the battery is in a 60% SOC state, and includes the state after standing (generally standing for 10 minutes). "0% SOC" refers to the state when the remaining capacity of the battery is zero, that is, fully discharged state.

[0032] In the description of this application, a "negative electrode-free" metal battery refers to a battery that does not add negative electrode active materials during the manufacturing process, and only uses a negative electrode current collector as a nominal negative electrode plate. However, the negative electrode current collector does not have the function of a negative electrode plate. Only after charging is completed, the metal in the positive electrode active material layer migrates to the surface of the negative electrode current collector and deposits on the surface of the negative electrode current collector to form a sodium metal layer. Only then does the battery have a true negative electrode plate.

[0033] In some embodiments, a "negative electrode-free" sodium battery refers to a battery in which a negative electrode active material layer is not actively provided on the negative electrode plate side during the manufacturing process of the battery. For example, a negative electrode active material layer is not provided at the negative electrode current collector through coating or deposition processes during the manufacturing process of the battery. During the first charge, the sodium ions obtain electrons on the anode side and metallic sodium is deposited on the surface of the negative electrode current collector to form a sodium metal phase. During discharge, the metallic sodium can be converted into sodium ions and return to the positive electrode plate to achieve cyclic charge and discharge. Compared with other sodium batteries, "negative electrode-free" sodium batteries can achieve higher energy density due to the lack of a negative electrode active material layer.

[0034] As an example, in a "negative electrode-free" sodium battery, a functional coating can be provided on the surface of the negative electrode current collector of the negative electrode plate. The functional coating can improve battery performance.

[0035] In some embodiments, in order to improve battery performance, the negative electrode plate may include a negative electrode current collector and a functional coating arranged on the surface of at least one side of the negative electrode current collector. The functional coating may include a carbon material coating (including single-arm conductive carbon tubes, multi-arm conductive carbon tubes, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers, soft carbon and hard carbon, etc.), a lithium-philic / sodium-philic metal composite coating, etc.

[0036] In one aspect of the present application, the present application proposes a positive electrode sheet, comprising: a positive electrode current collector; a positive electrode active material layer, the positive electrode active material layer is arranged on at least one side surface of the positive electrode current collector, the positive electrode active material layer includes a positive electrode active material, the positive electrode active material includes a sodium-containing positive electrode active material, and the thickness of the positive electrode sheet meets D max / D min 104.5%-300%, wherein, after the positive electrode sheet and the negative electrode sheet are assembled into a battery, the thickness of the positive electrode sheet when the battery is at 0% SOC is D max , when the battery is at 100% SOC, the thickness of the positive electrode sheet is D min , wherein the negative electrode sheet includes a negative electrode current collector, and when the battery is at 100% SOC, at least one side of the negative electrode current collector has a sodium metal layer. When the thickness D of the positive electrode sheet max / D min When the volume change rate of the positive electrode active material layer is greater than 300%, the positive electrode active material layer is too large, and the positive electrode active material layer is easy to pulverize during the charge and discharge process, and then fall off from the surface of the positive electrode current collector; when the thickness of the positive electrode sheet D max / D min Less than 4.5%, the volume change rate of the positive electrode active material layer is too small to alleviate the volume change of the negative electrode sheet. max / D min When it is 104.5%-300%, the positive electrode plate can effectively alleviate the expansion stress of the negative electrode plate caused by the volume change during the battery charging and discharging process, so that the structural stability of the battery is significantly improved, thereby increasing the battery life.

[0037] For ease of understanding, the principle of the positive electrode sheet in this application having the above beneficial effects is explained below:

[0038] In this application, taking the "negative electrode-free" sodium metal battery as an example, during the charging process of the battery, see Figure 1-Figure 3When the battery is in a fully discharged state, the negative electrode plate only includes the negative electrode current collector 11. As the sodium ions in the positive electrode active material layer 22 gradually escape and deposit on the surface of the negative electrode current collector 11 during the charging process, a sodium metal layer 12 will gradually form on the surface of the negative electrode current collector 11, that is, the thickness of the negative electrode plate will gradually increase, and the thickness of the negative electrode plate will reach a maximum value when the battery is fully charged. Furthermore, when the volume of other structures in the battery except the negative electrode plate remains unchanged, as the thickness of the negative electrode plate gradually increases during the charging process, the utilization rate of the internal space of the battery will become higher and higher, and the pressure exerted by the internal structure of the battery on the battery shell will become greater and greater, eventually causing the battery shell to deform and fail to meet the surface flatness requirements, thereby affecting the assembly of the battery module, and at the same time significantly increasing the fatigue strength of the functional components; and the large volume expansion will cause the glue layer between adjacent batteries to fall off and peel off, thereby causing the structure of the battery module to be damaged.

[0039] For "negative electrode-free" sodium metal batteries, the maximum value of the change in the thickness of the negative electrode sheet caused by the sodium deposition or release on the surface of the negative electrode current collector can reach several times the initial thickness value. On this basis, by selecting a positive electrode sheet with a thickness change law opposite to that of the negative electrode sheet of the "negative electrode-free" metal battery, the stress caused by the expansion and contraction of the negative electrode sheet can be effectively alleviated. Specifically, when the battery is in a fully charged state, the thickness of the positive electrode sheet proposed in the present application is its minimum thickness, and when the battery is in a fully discharged state, the thickness of the positive electrode sheet is its maximum thickness, and the thickness of the positive electrode sheet gradually increases during the transition of the battery from a fully charged state to a fully discharged state, and the thickness of the positive electrode sheet gradually decreases during the transition of the battery from a fully discharged state to a fully charged state; on the contrary, when the battery is in a fully charged state, the thickness of the negative electrode sheet is its maximum thickness, and when the battery is in a fully discharged state, the thickness of the negative electrode sheet is its minimum thickness, and the thickness of the negative electrode sheet gradually increases during the transition of the battery from a fully discharged state to a fully charged state, and the thickness of the negative electrode sheet gradually decreases during the transition of the battery from a fully charged state to a fully discharged state. By selecting the positive electrode sheets in the present application to assemble a "negative electrode-free" metal battery, the thickness of the negative electrode sheet will continue to increase during the charging process, and the thickness of the positive electrode sheet will continue to decrease adaptively; during the discharging process, the thickness of the negative electrode sheet will continue to decrease, and the thickness of the positive electrode sheet will continue to increase adaptively, thereby achieving an effect of increasing and decreasing the thickness of the electrode sheets and matching each other, thereby effectively alleviating the volume change of the negative electrode sheet during the charging and discharging process, so that the internal stress of the battery is always in a relatively stable state during the charging and discharging process, the structural stability of the battery is significantly improved, and the battery life is improved.

[0040] According to some embodiments of the present application, when the positive electrode sheet has a pore structure, for example, when the positive electrode active material layer has a pore structure, the pore structure provides a compressible space for the positive electrode active material layer, and the compressible space can rebound after the external force is removed. When the positive electrode active material layer is squeezed by an external force, it can be compressed, so that the thickness of the positive electrode active material layer is reduced, and then the thickness of the entire positive electrode sheet is reduced. As a result, the thickness of the positive electrode sheet can be reduced when it is squeezed by the negative electrode sheet during charging, thereby alleviating the expansion stress generated by the negative electrode sheet during charging. The porosity of the positive electrode active material layer is not particularly limited. For example, the porosity of the positive electrode active material layer can be 25%-50%. When the porosity of the positive electrode active material layer is less than 25%, the compressibility of the positive electrode active material layer is poor and it cannot effectively alleviate the expansion stress of the negative electrode plate; when the porosity of the positive electrode active material layer is greater than 50%, the positive electrode active material layer has too many pores and too large pore sizes, which leads to poor contact of the positive electrode active material particles, and then increases the contact resistance, resulting in deterioration of the performance of the positive electrode plate. At the same time, there will also be problems such as low energy density of the positive electrode plate.

[0041] The porosity of the positive electrode active material layer can be determined by a gas replacement method, and the percentage of the pore volume in the positive electrode active material layer to the total volume of the positive electrode active material layer is the porosity of the positive electrode active material layer. Specifically, according to some embodiments of the present application, it can be determined by referring to GB / T 24586-2009 through the following steps: the positive electrode sheet is immersed in ethyl methyl carbonate (EMC) for cleaning, and the gas replacement method is used to measure the porosity of the positive electrode sheet using an AccuPycⅡ1340 device. The calculation formula is as follows: The porosity ρ of the positive electrode sheet 总 =(V-V0) / V 总 × 100%, where V0 is the true volume, V is the apparent volume, and the porosity of the positive electrode active material layer is ρ = ρ 总 ×V / (VV 集流体 ) Among them, V 集流体 is the current collector volume.

[0042] According to some embodiments of the present application, the type of positive electrode active material is not particularly limited. For example, the positive electrode active material may include a layered oxide, and the layered oxide may satisfy the chemical formula Na x M yO2, wherein 0<x≤4.5, 0<y≤1, and M element includes at least one of Ti, V, Cr, Fe, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La and Ce; preferably, M element includes at least one of Ti, V, Cr, Fe, Co, Mn, Ni, Cu and Zn. The crystal structure of sodium-containing layered oxide is similar to that of ternary positive electrode materials, and sodium-containing layered oxide has higher energy density, higher compaction density and better cycle performance. In addition, the metals contained in the layered oxide, such as copper, manganese and iron, are more abundant and relatively cheap, which can further reduce the manufacturing cost of the battery.

[0043] According to some embodiments of the present application, the type of positive electrode active material is not particularly limited. For example, the positive electrode active material may include a polyanionic compound, and the cationic element of the polyanionic compound may include at least one of Ni, V, Co, Fe, Mn and Cu. Preferably, the cation of the polyanionic compound may include Ni 2+ 、Ni 3+ 、Co 2+ 、Co 3+ , Fe 2 + , Fe 3+ , Mn 3+ 、V 3+ and Cu 2+ At least one of; the anion of the polyanionic compound includes F - PO4 3- 、P2O7 4- and (PO4)2P2O7 10 -at least one; preferably, the anion of the polyanionic compound includes F-. The crystal structure of the polyanionic compound is mainly an olivine structure. The polyanionic compound has a better cycle life, a higher output voltage and a better structural stability. The polyanionic compound has a small volume change and a small phase change during the insertion and extraction of sodium ions, and has a good long-term cycle stability.

[0044] According to some embodiments of the present application, the anion of the polyanionic compound is not particularly limited. For example, when the anion of the polyanionic compound includes PO4 3- and P2O7 4- When P2O7 4- With PO4 3- The molar ratio of P2O7 can be 0.1-5; preferably, the polyanionic compound has 4- With PO4 3- The molar ratio of P2O7 can be 0.1-3.4- With PO4 3- When the molar ratio is between 0.1 and 5, the polyanionic compound has a higher specific capacity and better cycle performance.

[0045] According to some embodiments of the present application, the positive electrode active material layer may further include a sodium supplement additive, the mass fraction of the positive electrode active material in the positive electrode active material layer may be 50wt%-98wt%, and the mass fraction of the sodium supplement additive in the positive electrode active material layer may be 2wt%-50wt%. In the present application, the sodium supplement agent can make up for the loss of active sodium caused by the formation of SEI during the first charge and discharge process of the battery, so that the battery has enough reversible active sodium in subsequent cycles, thereby improving the energy density of the battery; the sodium supplement additive can also be used to make up for the sodium consumption during the cycle process, thereby improving the cycle performance of the battery. According to other embodiments of the present application, the content of the sodium supplement additive in the positive electrode active material layer is not particularly limited. For example, when a sodium-free positive electrode active material and / or a low-sodium positive electrode active material is selected, the content of the sodium supplement additive can be appropriately increased so that the energy density of the positive electrode sheet meets the battery design requirements; when a conventional sodium-containing positive electrode active material is used, the content of the sodium supplement additive can be appropriately reduced so that the energy density of the positive electrode sheet meets the battery design requirements. Those skilled in the art can make a selection according to actual conditions.

[0046] According to some embodiments of the present application, by selecting a volatile sodium supplement additive, gas can be generated during the formation process of the battery and escaped from the positive electrode active material layer, thereby further providing a pore structure for the positive electrode active material layer to increase the porosity of the positive electrode active material layer. The type of sodium supplement additive is not particularly limited. For example, the sodium supplement additive may include at least one of Na2S, NaN3, Na2NiO2, NaC6H5O7, Na2O, Na2O2, Na6CoO4, Na5FeO4, Na2C2O4, Na2C4O4, Na2C3O5, Na2C4O6, and Na2C6O6.

[0047] According to some embodiments of the present application, the thickness of the positive electrode sheet is not particularly limited. For example, the thickness of the positive electrode current collector is 5 μm-60 μm, and the thickness of the positive electrode active material layer is 50 μm-350 μm. When the thickness of the positive electrode current collector and the positive electrode active material layer is within the above range, and the porosity of the positive electrode active material layer is 25%-50%, the thickness change of the positive electrode sheet during the charge and discharge process can meet D max / D min It is 104.5%-300%.

[0048] According to some embodiments of the present application, the positive electrode active material layer on the positive electrode sheet in the present application can be compressed and rebounded, so that when the thickness of the negative electrode sheet increases during charging, the thickness of the positive electrode sheet can be adaptively reduced; when the thickness of the negative electrode sheet decreases during discharging, the thickness of the positive electrode sheet can be adaptively increased, so that the internal stress of the battery is always in a relatively stable state during the charging and discharging process. When the thickness of the positive electrode sheet meets D max / D min When the volume of the negative electrode sheet is 104.5%-300%, some space has been reserved in the structural design of the battery shell, and the reserved space can be used to relieve the stress caused by the volume expansion of the battery during the charge and discharge process. Specifically, in the initial stage of the expansion of the negative electrode sheet, the reserved space of the battery shell can be used to relieve the relatively slight volume expansion of the negative electrode sheet. As the volume of the negative electrode sheet further expands, the positive electrode sheet can shrink in volume accordingly after receiving pressure from the negative electrode sheet side, thereby further relieving the pressure caused by the volume expansion of the negative electrode sheet. The reserved space of the battery shell and the compressible and resilient positive electrode sheet can work together to relieve the stress generated by the negative electrode sheet with a large volume change rate during the charge and discharge process. For example, it can be used to relieve the thickness that meets d max / d min The expansion and contraction changes of the negative electrode sheet during the charge and discharge process (d max is the thickness of the negative electrode sheet when the battery is at 100% SOC, d min is the thickness of the negative electrode sheet when the battery is at 0% SOC). Preferably, the thickness of the negative electrode sheet satisfies d max / d min It can be 120%-400%.

[0049] According to some embodiments of the present application, the thickness of the negative electrode sheet is not particularly limited. For example, the thickness of the negative electrode current collector may be 5 μm-600 μm, and the thickness of the sodium metal layer on the surface of the negative electrode current collector may be 0 μm-200 μm. When the thickness of the negative electrode current collector and the sodium metal layer is within the above range, the thickness change of the negative electrode sheet during the charge and discharge process may satisfy d max / d min It is 100%-700%.

[0050] It should be noted that for a "negative electrode-free" metal battery, when the battery is at 100% SOC, a metal layer is deposited on the surface of the negative electrode current collector. When the battery is at 0% SOC, the metal layer on the surface of the negative electrode current collector should theoretically disappear completely. However, in actual situations, when the battery is in a low SOC state, such as 0% SOC, there may still be a small amount of irregularly deposited metal on the negative electrode current collector. The thickness of the residual deposited metal is relatively thin, and the effect on the thickness of the negative electrode plate can be ignored.

[0051] According to some embodiments of the present application, for a negative electrode sheet in which a negative electrode active material is added during the production process and a negative electrode active material layer is provided on the surface of the negative electrode current collector, taking a sodium ion battery as an example, during the charge and discharge process, the negative electrode sheet will expand and shrink in volume due to the generation of sodium dendrites on the surface of the negative electrode active material layer, the intercalation reaction of sodium ions in the negative electrode active material layer, the alloy reaction involving sodium ions, the expansion of the silicon-containing negative electrode active material in the negative electrode active material layer, etc. The positive electrode sheet in the present application is also applicable to batteries containing the above-mentioned negative electrode sheet, and can effectively alleviate the stress changes caused by the volume changes of the negative electrode sheet.

[0052] It is understandable that the positive electrode plate in the present application is also applicable to the lithium-ion battery system. Those skilled in the art can make corresponding adjustments to the type of positive electrode active material, negative electrode current collector, etc. according to actual conditions, which will not be repeated here.

[0053] In another aspect of the present application, the present application proposes a method for preparing the aforementioned positive electrode sheet, comprising: providing a positive electrode current collector; providing a positive electrode slurry, and coating the positive electrode slurry on at least one side of the positive electrode current collector to form a positive electrode active material layer. Therefore, the method has all the features and advantages of the aforementioned positive electrode sheet, which will not be described in detail here.

[0054] According to some embodiments of the present application, the method for obtaining a positive electrode active material layer having a pore structure is not particularly limited. For example, a positive electrode sheet that meets the aforementioned porosity requirements can be obtained by a chemical method. Specifically, providing a positive electrode slurry may include: uniformly mixing the positive electrode active material and the sodium supplement additive in a solvent; after forming the positive electrode active material layer, it may further include: assembling the positive electrode sheet and the negative electrode sheet into a battery and performing a formation treatment. In this step, a non-residual volatile or semi-residual sodium supplement additive is uniformly mixed with the positive electrode active material. When the battery is subjected to a formation treatment, the sodium supplement additive will react to form a gas and be discharged, thereby leaving a pore structure on the positive electrode active material layer to further increase the porosity of the positive electrode active material layer. When a sodium-free positive electrode active material and / or a low-sodium positive electrode active material is selected, the content of the sodium supplement additive can be appropriately increased so that the energy density of the positive electrode sheet meets the battery design requirements; when a conventional sodium-containing positive electrode active material is used, the content of the sodium supplement additive can be appropriately reduced so that the energy density of the positive electrode sheet meets the battery design requirements. Those skilled in the art can make a choice according to actual conditions.

[0055] It should be noted that the material types and related parameters of the above-mentioned positive electrode active materials and sodium supplement additives can refer to part or all of the technical features in the aforementioned embodiments. For the parts not described in this embodiment, reference can also be made to the aforementioned embodiments and related drawings, which will not be repeated here.

[0056] According to some embodiments of the present application, before coating the positive electrode slurry on at least one side of the positive electrode current collector, the method further includes: arranging a sodium foil on the surface of the positive electrode current collector for coating the positive electrode slurry. Thus, the sodium foil can be arranged to further improve the sodium supplement effect for the positive electrode sheet.

[0057] According to some embodiments of the present application, the method for obtaining a positive electrode active material layer with a pore structure is not particularly limited. For example, a positive electrode sheet that meets the aforementioned porosity requirements can be obtained by a physical method. Specifically, the positive electrode sheet is placed under a pressing roller for cold pressing treatment, and then the cold pressed positive electrode sheet is stripped for a second time and then rolled by a pore-making roller before being wound into sheets. By arranging pore-making nails of different lengths on the pore-making roller, the porosity of the positive electrode active material layer can be controlled, thereby improving the porosity of the positive electrode active material layer and reducing the cost of battery manufacturing. According to some embodiments of the present application, the pore-forming roller may include a roller body, and pore-forming pins distributed on the surface of the roller body, the pore-forming pins including at least one column of first pore-forming pins and at least one column of second pore-forming pins; each column of first pore-forming pins is adjacent to each column of second pore-forming pins; the length of the first pore-forming pins is greater than the length of the second pore-forming pins, the length of the first pore-forming pins is 80-90% of the thickness of the active material layer, the length of the second pore-forming pins is 40%-60% of the thickness of the active material layer, the arrangement density of the second pore-forming pins is 100%-200% of the arrangement density of the first pore-forming pins, the diameter of the pore-forming pins is 100μm-800μm, and the spacing between two adjacent columns of first pore-forming pins is 1-2 times the length of the first pore-forming pins. Specifically, a row of first pore-forming nails is arranged between two adjacent rows of second pore-forming nails, the spacing between two adjacent rows of first pore-forming nails is 1.5 times the length of the first pore-forming nails, the spacing between two adjacent rows of second pore-forming nails is 1.5 times the length of the first pore-forming nails, the length of the first pore-forming nails is 85% of the thickness of the positive electrode active material layer, and the diameter is 550 μm; the length of the second pore-forming nails is 50% of the thickness of the positive electrode active material layer, the diameter is 550 μm, and the arrangement density of the second pore-forming nails is 150% of the arrangement density of the first pore-forming nails. Thus, a positive electrode active material layer with a porosity within the aforementioned range can be obtained.

[0058] In another aspect of the present application, the present application proposes a battery, comprising: a positive electrode sheet, a negative electrode sheet, and a separator between the positive electrode sheet and the negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet mentioned above, and / or the positive electrode sheet prepared by the above method, the negative electrode sheet includes a negative electrode collector, and the thickness of the negative electrode sheet satisfies d max / d min 100%-700%, where d max is the thickness of the negative electrode sheet when the battery is at 100% SOC, d min is the thickness of the negative electrode sheet when the battery is at 0% SOC. Preferably, the thickness of the negative electrode sheet satisfies dmax / d min The volume change rate of the battery during the charge and discharge process is good, and the structural stability is high.

[0059] According to some embodiments of the present application, there is no particular limitation on the shape of the battery, which may be cylindrical, square, or any other shape. Figure 4 The square structure battery 5 is used as an example. Figure 5 , the outer package may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0060] According to some embodiments of the present application, the battery may include an outer package for packaging a positive electrode sheet, a negative electrode sheet, and an electrolyte.

[0061] According to some embodiments of the present application, the outer packaging may include a shell and a cover plate. Among them, the shell may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell has an opening connected to the receiving cavity, and the cover plate can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly through a winding process or a lamination process. The electrode assembly is encapsulated in the receiving cavity. The electrolyte can be an electrolyte, and the electrolyte is infiltrated in the electrode assembly. The number of electrode assemblies contained in the battery can be one or more, which can be adjusted according to demand.

[0062] According to some embodiments of the present application, the outer packaging of the battery may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0063] According to some embodiments of the present application, the batteries can be assembled into a battery module, and the number of batteries contained in the battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module. Figure 6In the battery module 4, the multiple batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. The multiple batteries 5 may further be fixed by fasteners. The battery module 4 may also include a housing having a storage space, in which the multiple batteries 5 are stored. The battery module 4 may also include a housing having a storage space, in which the multiple secondary batteries 5 are stored. In some embodiments, the above-mentioned battery modules may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0064] According to some embodiments of the present application, the above-mentioned battery modules can also be assembled into a battery pack. The number of battery modules contained in the battery pack can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery pack. Figure 7 and Figure 8 1 is a battery pack 1 as an example. Figure 7 and Figure 8 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0065] In another aspect of the present application, the present application proposes an electrical device, which includes the aforementioned positive electrode plate, and / or the positive electrode plate prepared by the aforementioned method, and / or the aforementioned battery, and the battery is used to provide electrical energy. Specifically, the battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited to these. The electrical device can select batteries, battery modules or battery packs according to its usage requirements.

[0066] According to some embodiments of the present application, Fig. 9 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the battery, a battery pack or a battery module can be used.

[0067] According to some embodiments of the present application, the power-consuming device may also be a mobile phone, a tablet computer, a laptop computer, etc. The device is usually required to be light and thin, and a battery may be used as a power source.

[0068] In this application, all the numbers disclosed herein are approximate values, regardless of whether the words "about" or "approximately" are used. The value of each number may vary by less than 10% or a reasonable difference considered by those skilled in the art, such as 1%, 2%, 3%, 4% or 5%.

[0069] In the description of the present application, it should be understood that the terms "thickness", "upper", etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.

[0070] The scheme of the present application is described below by specific examples. It should be noted that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this area or the product instructions are used. The reagents or instruments used are not specified by the manufacturer, and are all conventional products that can be obtained commercially.

[0071] Embodiment 1:

[0072] Positive electrode preparation:

[0073] The positive electrode active material Na3V2(PO4)3, the sodium supplement agent Na2C2O4, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are dissolved in a solvent N-methylpyrrolidone (NMP) at a weight ratio of X1:X2:5%:2%, and the mixture is fully stirred and mixed to prepare a positive electrode slurry. The solvent ratio is adjusted to control the viscosity of the positive electrode slurry to 2000mPa·S-5000mPa·S;

[0074] The positive electrode slurry is evenly coated on a positive electrode current collector aluminum foil with a thickness of 60 μm, and then dried, cold pressed, and cut to obtain a positive electrode sheet. The coating surface density is controlled according to the following corresponding embodiment.

[0075] Preparation of negative electrode sheet:

[0076] The conductive carbon tube dispersion (conductive carbon content 2wt%) and the thickener carbon methyl cellulose sodium (CMC) are fully stirred and mixed in a proper amount of deionized water solvent system at a weight ratio of 95%:5%, and the viscosity of the negative electrode slurry is controlled to be 2000mPa·S-8000mPa·S. The slurry is coated on a 60μm copper foil and dried to obtain a negative electrode sheet with a functional coating on both sides of the negative electrode current collector.

[0077] Battery preparation:

[0078] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrodes to play an isolating role. The electrode assembly is wound and placed in a designed battery casing. The electrolyte is added to the battery casing. The battery is formed after the battery cell is allowed to stand for 12 hours. Negative pressure exhaust is performed during the formation process, and the battery is obtained after packaging.

[0079] Examples 2-12 and Comparative Examples 1-5 are consistent with Example 1, and the differences are specifically shown in Table 1.

[0080] The following performance tests were performed on the batteries in Examples 1-12 and Comparative Examples 1-5, and the test methods were as follows:

[0081] 1. Porosity of the positive electrode active material layer: refer to GB / T 24586-2009 and determine it by the following steps: immerse the positive electrode sheet in ethyl methyl carbonate (EMC) for cleaning, and use AccuPycⅡ1340 equipment to measure it by gas displacement method. The calculation formula is as follows: Porosity ρ of the positive electrode sheet 总 =(V-V0) / V 总 × 100%, where V0 is the true volume, V is the apparent volume, and the porosity of the positive electrode active material layer is ρ = ρ 总 ×V / (VV 集流体 ) Among them, V 集流体 The test results are shown in Table 1.

[0082] 2. Thickness of positive electrode: D max The test includes: when the battery is at 0% SOC, the battery is disassembled and the thickness of the positive electrode is tested with a micrometer; min The test includes: when the battery is 100% SOC, the battery is disassembled and the thickness of the positive electrode plate is tested with a micrometer. 100% SOC means that the battery is charged to 4.3V at 1C at 2.5V-4.3V under a constant temperature environment of 25°C, and then charged at a constant voltage at 4.3V to a current of less than or equal to 0.05mA. At this time, the battery is 100% SOC; 0% SOC means that the battery is discharged to 0% SOC as much as possible at 1C, and further discharged to the target voltage using 0.04C. After disassembling the battery cell, the metal deposition area on the surface of the negative electrode current collector accounts for no more than 5% of the total area of ​​the disassembled negative electrode current collector. At this time, the battery is 0% SOC. See Table 2 for the test results.

[0083] 3. Thickness of negative electrode sheet: d max The test includes: when the battery is at 100% SOC, the battery is disassembled and the thickness of the negative electrode plate is tested using a micrometer; d minThe test includes: when the battery is at 0% SOC, the battery is disassembled and the thickness of the negative electrode plate is tested using a micrometer. The test results are shown in Table 2.

[0084] 4. Battery cycle life: At a constant temperature of 25°C, charge the battery at 1C to 4.3V at 1.5-3.6V, and then charge at a constant voltage at 4.3V until the current is less than or equal to 0.05mA. Let it stand for 5 minutes, then discharge it at 1C to 2.5V, and record the discharge capacity at this time as D0. Repeat the above charge and discharge cycle until the discharge capacity is reduced to 80% of D0. Record the number of cycles the battery has gone through at this time, which is the cycle life of 80% SOH (State Of Health). See Table 2 for the test results.

[0085] 5. Cyclic expansion pressure of the battery: Place the test cell in the test fixture, which consists of three plates, which can be steel plates or aluminum plates. The three plates, the cell and the sensor form a "plate / cell / plate sensor / plate" placement state. Adjust the distance between the plates to adjust the appropriate initial fixture force (the surface pressure is calculated by the cell force area, P = F / S). During the cycle, the sensor transmits the specific corresponding expansion force data, and records the maximum expansion force during each cycle. By calculating the pressure, the corresponding number of cycles under 1MPa is obtained as the cutoff condition. The test results are shown in Table 2.

[0086] 6. Compacted density of positive electrode sheet: By measuring the mass of positive electrode sheet per unit area (g / cm 2 ) and the thickness of the positive electrode sheet (cm) (the number of collection points is greater than 14). Among them, the compaction density = the mass of the positive electrode sheet per unit area (g / cm 2 ) / thickness of positive electrode sheet (cm). The test results are shown in Table 1.

[0087] Table 1

[0088]

[0089] Table 2

[0090]

[0091]

[0092] The test results show that the thickness of the positive electrode sheet in Examples 1-13 meets D max / D min The 80% SOH cycle number of the batteries in Examples 1-13 is higher than that of the batteries in Comparative Examples 1-4, indicating that the thickness is selected to meet the D max / D minThe battery assembled with 104.5%-300% positive electrode sheets can achieve the effect of increasing and decreasing the thickness of the positive electrode sheets and the negative electrode sheets, thereby effectively alleviating the volume change of the negative electrode sheets during the charging and discharging process, thereby effectively improving the cycle life of the battery.

[0093] The thickness of the positive electrode sheet in Examples 1-13 satisfies D max / D min The corresponding cycle numbers of the batteries in Examples 1-13 when the expansion pressure is ≥1MPa are all higher, and are better than the corresponding cycle numbers of the batteries in Comparative Examples 1-4 when the expansion pressure is ≥1MPa. This shows that by selecting the thickness to meet D max / D min The battery assembled with 104.5%-300% positive electrode sheets has a high surface flatness, so that the internal stress of the battery is always in a relatively stable state during the charging and discharging process, thereby significantly improving the structural stability of the battery.

[0094] Among them, the positive electrode active materials in Examples 11 and 12 use sulfide positive electrode active materials, which effectively improves the volume change rate of the positive electrode plate, thereby effectively improving the expansion tolerance of the battery; the porosity of the positive electrode active material layer in Comparative Example 3 is too large, which makes the structural stability of the positive electrode plate poor, thereby making the structural stability of the battery poor and the cycle performance significantly reduced.

[0095] In the description of the present application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for examples and may be any technical feature connected by "and / or" in the present application.

[0096] Unless otherwise specified, all scientific and technological terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. All patents and publications related to this application are incorporated herein by reference in their entirety. The term "comprising" or "including" is an open expression, i.e., including the content specified in this application, but does not exclude the content of other aspects.

[0097] In the description of this specification, the description with reference to the terms "one embodiment", "another embodiment", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory. In addition, it should be noted that in this specification, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated.

[0098] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A positive electrode sheet, characterized in that: include: Positive electrode current collector; A positive electrode active material layer, the positive electrode active material layer is disposed on at least one side surface of the positive electrode current collector, the positive electrode active material layer comprises a positive electrode active material, and the positive electrode active material comprises a positive electrode active material containing sodium, The thickness of the positive electrode sheet satisfies D max / D min 104.5%-300%, wherein after the positive electrode sheet and the negative electrode sheet are assembled into a battery, the thickness of the positive electrode sheet when the battery is at 0% SOC is D max When the battery is at 100% SOC, the thickness of the positive electrode sheet is D min , Wherein, the negative electrode plate includes a negative electrode current collector, and when the battery is at 100% SOC, at least one side surface of the negative electrode current collector has a sodium metal layer.

2. The positive electrode sheet according to claim 1, characterized in that: The porosity of the positive electrode active material layer is 25%-50%.

3. The positive electrode sheet according to claim 1, characterized in that: The positive electrode active material includes a layered oxide, the layered oxide satisfying the chemical formula Na x M y O2, wherein 0<x≤4.5, 0<y≤1, and the M element includes at least one of Ti, V, Cr, Fe, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La and Ce; preferably, the M element includes at least one of Ti, V, Cr, Fe, Co, Mn, Ni, Cu and Zn.

4. The positive electrode sheet according to claim 1, characterized in that: The positive electrode active material includes a polyanionic compound, wherein the cation element of the polyanionic compound includes at least one of Ni, V, Co, Fe, Mn and Cu, and the anion of the polyanionic compound includes F - PO4 3- 、P2O7 4- and (PO4)2P2O7 10- At least one of; Preferably, the anion of the polyanionic compound includes F - .

5. The positive electrode sheet according to claim 4, characterized in that: The anions of the polyanionic compound include PO4 3- and P2O7 4- , the P2O7 in the polyanionic compound 4- With the PO4 3- The molar ratio of P2O7 is 0.1-5; preferably, the P2O7 4- With the PO4 3- The molar ratio is 0.1-3.

6. The positive electrode sheet according to claim 1, characterized in that: The positive electrode active material layer further includes a sodium supplement additive, the mass fraction of the positive electrode active material in the positive electrode active material layer is 50wt%-98wt%, and the mass fraction of the sodium supplement additive in the positive electrode active material layer is 2wt%-50wt%.

7. The positive electrode sheet according to claim 6, characterized in that: The sodium supplement additive includes at least one of Na2S, NaN3, Na2NiO2, NaC6H5O7, Na2O, Na2O2, Na6CoO4, Na5FeO4, Na2C2O4, Na2C4O4, Na2C3O5, Na2C4O6 and Na2C6O6.

8. The positive electrode sheet according to claim 1, characterized in that: The thickness of the negative electrode sheet satisfies d max / d min is 100%-700%, wherein the d max is the thickness of the negative electrode sheet when the battery is at 100% SOC, and the d min is the thickness of the negative electrode plate when the battery is at 0% SOC.

9. A method for preparing a positive electrode sheet according to any one of claims 1 to 8, characterized in that: include: providing a positive electrode current collector; A positive electrode slurry is provided, and the positive electrode slurry is coated on at least one side surface of the positive electrode collector to form a positive electrode active material layer.

10. The method according to claim 9, characterized in that The providing of positive electrode slurry comprises: uniformly mixing positive electrode active material and sodium supplement additive in a solvent; after forming the positive electrode active material layer, the further step comprises: assembling the positive electrode plate and the negative electrode plate into a battery, and performing a formation treatment.

11. The method according to claim 9, characterized in that Before coating the positive electrode slurry on at least one side of the surface of the positive electrode collector, the method further comprises: arranging a sodium foil on the surface of the positive electrode collector for coating the positive electrode slurry.

12. A battery, characterized in that: include: A positive electrode sheet, a negative electrode sheet, and a separator between the positive electrode sheet and the negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet according to any one of claims 1 to 8, and / or the positive electrode sheet prepared by the method according to any one of claims 9 to 11, The negative electrode sheet includes a negative electrode current collector, and the thickness of the negative electrode sheet satisfies d max / d min is 100%-700%, wherein the d max is the thickness of the negative electrode sheet when the battery is at 100% SOC, and the d min is the thickness of the negative electrode plate when the battery is at 0% SOC.

13. An electrical device, characterized in that: include: The positive electrode sheet according to any one of claims 1 to 8, and / or the positive electrode sheet prepared by the method according to any one of claims 9 to 11, and / or the battery according to claim 12.