Positive electrode material with spinel coating layer, preparation method and battery
By adopting the core-shell protection structure of the spinel coating in the cathode material of the sodium-ion battery, the problems of structural instability and poor sodium ion permeability of the layered transition metal oxide cathode material are solved, and the sodium ion permeability is significantly improved. Battery gram capacity and cycle stability.
Patent Information
- Application Number
- CN202410762760.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-01
AI Technical Summary
Due to structural instability and poor sodium ion permeability, existing layered transition metal oxide cathode materials for sodium-ion batteries have insufficient cycle performance and cannot fully exert their high gram capacity and rate performance.
The sodium transition metal oxide cathode material with a spinel coating is used to form a typical shell-core protective structure through a one-step coating method of high-temperature calcination. The ion exchange between lithium or potassium and sodium is used to form a lithium-sodium or potassium-sodium blend tip. The spar protective layer enhances material stability and improves the entry and exit performance of sodium ions.
It significantly improves the gram capacity and cycle stability of sodium-ion batteries, simplifies the material production process, avoids the complexity of traditional secondary coating and island-like coating problems, and enhances the long cycle performance of the material.
Smart Images

Figure CN118738274A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of sodium ion batteries, and in particular to a sodium transition metal oxide positive electrode material with a spinel coating layer, a preparation method and a sodium ion battery. Background Art
[0002] Layered transition metal oxide cathode materials for sodium ion batteries are considered to be the most valuable cathode materials for sodium ion batteries due to their high gram capacity, wide range of raw material sources, good rate performance, and simple and mature processing and preparation schemes. At present, this type of material has begun to be gradually mass-produced.
[0003] According to the environment of Na+, layered materials can be divided into two categories: P-type and O-type (the most widely studied are P2, P3 and O3). However, as a layered structure of transition metal oxide cathode materials for sodium ion batteries, due to the instability of the layered structure (collapse of the layered structure during charging and discharging, migration of transition metals and electrolyte erosion on the surface, etc.), compared with other sodium ion battery cathode materials, such as polyanion series sodium ion battery materials (NFS or NFPP, etc.), the cycle performance they exhibit still has a lot of room for improvement.
[0004] In addition to the structural design of the material itself, the modification of the positive electrode material of the sodium ion battery, such as coating, morphology modification, composite performance, etc., will also change the capacity characterization and long cycle performance of the sodium ion battery. Therefore, in order to achieve high specific energy and high stability electrode materials and further improve the comprehensive performance of existing sodium ion batteries, the research on morphology and coating processes is of great significance. Summary of the invention
[0005] The present application provides a sodium transition metal oxide positive electrode material with a spinel coating layer, a preparation method and a sodium ion battery. The positive electrode material has a typical core-shell protection structure, with a layered transition metal oxide as the core (P2, P3 phase or mixed phase) and a spinel shell coated on the surface as a protective layer. While having a high gram capacity, the material stability is enhanced. In addition, during the synthesis process, the material in the present application adopts a high-temperature calcination one-step coating method. Based on the combined action of kinetics and thermodynamics, part of the lithium or potassium and sodium are ion-exchanged to form a lithium-sodium or potassium-sodium blended spinel protective layer, which protects the core positive electrode material from decomposition while allowing sodium ions to pass through, thereby improving the entry, exit and deintercalation performance of sodium ions. The gram capacity and cycle stability of the prepared sodium ion battery are greatly improved.
[0006] In a first aspect, the present application provides a sodium transition metal oxide positive electrode material having a spinel coating layer, wherein the general formula of the sodium transition metal oxide having a spinel coating layer of the positive electrode material is Na x Nia Mn b M c O2 0.1(L x Mn 2- c M c O4); wherein, 0.7≤x≤1.0, a>0, b>0, c>0, a+b+c=1, M is selected from one of Mg, Al, Fe, Cu, Ti, Co, La, Zn or Zr, and L is one of Li and K.
[0007] In a second aspect, the present application provides a method for preparing a sodium transition metal oxide positive electrode material having a spinel coating layer, comprising the following steps:
[0008] According to the stoichiometric ratio, nickel salt, manganese salt and M salt are used to prepare a first mixed solution containing nickel ions, manganese ions and M ions, and a second mixed solution containing manganese ions and M ions. The first mixed solution is first subjected to titration precipitation by a step-by-step titration co-precipitation method. After the reaction is complete, the second mixed solution is added to further perform titration precipitation. During the process, the pH value is controlled and the grains are slowly grown so that the particle size of the obtained co-precipitation precursor is 6-10 um. After spray drying, a first transition metal carbonate or hydroxide precipitation precursor is obtained.
[0009] According to the stoichiometric ratio, the sodium-containing compound, the L-containing compound and the first transition metal carbonate or hydroxide precipitation precursor are mixed and sintered to obtain the sodium transition metal oxide positive electrode material with a spinel coating layer.
[0010] In a third aspect, the present application provides a method for preparing a sodium transition metal oxide positive electrode material having a spinel coating layer, comprising the following steps:
[0011] According to the stoichiometric ratio, nickel salt and manganese salt are used to prepare a third mixed solution containing nickel ions and manganese ions, and a fourth mixed solution containing manganese ions. The third mixed solution is first subjected to titration precipitation by a step-by-step titration co-precipitation method. After the reaction is complete, the fourth mixed solution is added and further titration precipitation is performed. During the process, the pH value is controlled and the grain growth is performed slowly, so that the particle size of the obtained co-precipitation precursor is 6-10 um. After spray drying, a second transition metal carbonate or hydroxide precipitation precursor is obtained.
[0012] According to the stoichiometric ratio, the sodium-containing compound, the second transition metal carbonate or hydroxide precipitation precursor, the L-containing compound, and the M-containing compound are mixed and sintered to obtain the sodium transition metal oxide positive electrode material with a spinel coating layer.
[0013] In a fourth aspect, the present application provides a sodium ion battery comprising a positive electrode material, wherein the positive electrode material comprises the sodium transition metal oxide positive electrode material having a spinel coating layer as described in the first aspect above, or comprises the sodium transition metal oxide positive electrode material having a spinel coating layer prepared by the preparation method described in the second aspect or the third aspect above.
[0014] The technical effects of this application are:
[0015] Compared with the prior art, the sodium transition metal oxide positive electrode material with a spinel coating layer provided in the embodiment of the present application is designed based on the traditional layered transition metal oxide layered coating method. The traditional layered transition metal oxide coating process generally adopts the method of external oxide coating (such as aluminum oxide Al2O3, zirconium oxide ZrO2 or titanium oxide TiO2, etc.), and this type of coating method is divided into dry and wet methods, and is a more complex secondary coating. Among them, the dry coating cannot completely coat the core positive electrode material (generally in an island shape), so the obtained positive electrode material has poor cycle performance; and although the wet coating can completely coat the material, the coating pretreatment required by the wet method is more complicated, and because the coating is complete, the isolation effect of the coating layer prevents sodium ions from passing smoothly, and the rate performance and gram capacity of the material are all reduced.
[0016] The material in this application adopts a high-temperature calcination and one-step coating method. The prepared material has a typical core-shell protection structure, with a layered transition metal oxide as the core (P2, P3 phase or mixed phase) and a spinel shell coated on the surface as a protective layer. While having a higher gram capacity, the material stability is enhanced; the gram capacity and cycle stability of the prepared sodium ion battery are greatly improved.
[0017] On the one hand, the material in the present application optimizes and improves the formulation process, uses a specific stoichiometric ratio as the formula, introduces elements such as Li and K that are easy to form a spinel structure, and uses a larger precursor core as the core and smaller additive materials (such as iron oxide, titanium oxide, magnesium oxide, etc.) as attachments. A high-temperature calcination and one-step coating method is used to prepare a spinel protective layer with a core-shell structure; at the same time, the secondary coating step is also omitted, making the material production process simpler and more efficient.
[0018] Secondly, since some of the formula materials (sodium carbonate, lithium carbonate, etc.) adhere and melt at high temperature, the molten environment provided makes the prepared spinel protective layer a completely coated protective layer without island coating or incomplete coating, eliminating the possibility of rapid attenuation of the material during charging and discharging.
[0019] Thirdly, due to the presence of the sodium ion-coated spinel protective layer, the synthetic stability of the core positive electrode material at high temperature is effectively protected. Further, the possibility of preparing high-sodium P2 phase, P3 phase (or mixed phase) positive electrode materials (Na≥0.8) is also improved, greatly enhancing the characterization gram capacity of the material of this application.
[0020] Fourthly, due to the effect of the high temperature environment, the material of the present application can quickly complete the difficult lithium-sodium or potassium-sodium ion replacement process under the joint action of high temperature dynamics and thermodynamics. The formed spinel protective layer is a lithium-sodium or potassium-sodium blended spinel protective layer, which protects the core positive electrode material from decomposition while allowing sodium ions to pass through, thereby improving the entry and exit and deintercalation performance of sodium ions, and increasing the gram capacity and long cycle performance of the material.
[0021] The method for preparing a sodium transition metal oxide positive electrode material with a spinel coating layer provided in an embodiment of the present application is prepared by a simple method of co-precipitation combined with calcination, and has the characteristics of cheap and readily available raw materials and a simple preparation process. The obtained sodium transition metal oxide positive electrode material with a spinel coating layer has a complete crystal form and high purity.
[0022] The sodium ion battery provided in the embodiment of the present application uses a sodium transition metal oxide positive electrode material with a spinel coating layer as the positive electrode material. The material has a typical core-shell protection structure, with a layered transition metal oxide as the core (P2, P3 phase or mixed phase) and a spinel shell coated on the surface as a protective layer. While having a higher gram capacity, the material stability is enhanced; the gram capacity and cycle stability of the manufactured sodium ion battery are greatly improved.
[0023] For the general modification treatment method of the positive electrode material of the sodium ion battery, the common dry mixing or high temperature processing in the related technology can only sinter the spinel layer to the gap between the grains or the crystal interface, and cannot achieve the effect of completely and evenly covering the entire tiny grain ball with the spinel layer. In addition, if the spinel coating layer is formed by using only a sodium source as a raw material, the obtained spinel layer does not have a very good structure and uniformity, and the final coating effect is poor (because the spinel structure is still based on LiMn2O4, and the structure and consistency of the formed NaMn2O4 are poor). If the spinel coating layer is obtained on a large scale using a lithium source as a raw material, the spinel structure is easily separated from the core body, which eventually leads to the large-scale formation of a phase separation dominated by the LiMn2O4 structure (forming a second core of LiMn2O4), thereby causing the failure of the spinel outer layer coating structure.
[0024] The technical solution adopted in this application is:
[0025] 1. Core layer Na x Ni a Mnb M c O2 and coating layer L x Mn 2-c M c O4 is expanded according to the molar ratio of 10:1, which can ensure the core layer Na x Ni a Mn b M c O2 structure, and try to avoid phase separation and the formation of L x Mn 2-c M c O4 second core.
[0026] 2. The precursor is treated by forming a gradient difference precursor with NiMn and Mn source, so that spinel L is easily formed. x Mn 2-c M c The raw materials of the O4 structure are in the outer layer of the structure, and the formation of the spinel protective layer on the grain boundary is avoided as much as possible, so as to obtain a spinel structure protective layer uniformly covering the surface.
[0027] 3. With high temperature sintering as the final driving force, sodium source and lithium source or potassium source are added at the same time. Under the promotion of high temperature kinetics and thermodynamics, the sodium source and lithium source or potassium source are moved to the lowest energy state position respectively, and finally a stable core layer Na x Ni a Mn b M c O2 and uniform coating layer L x Mn 2-c M c O4 structure.
[0028] This gradient distribution and the dual-source driving effect (sodium source and lithium source, or sodium source and potassium source) can effectively avoid the formation of L x Mn 2-c M c O4 second core phase separation, finally obtaining a sodium ion battery positive electrode material that is uniformly and completely covered with a spinel layer.
[0029] In order to more clearly demonstrate the technical means of the present application and ensure the smooth implementation of the contents of the specification, some typical embodiments of the present application are listed below together with drawings and detailed descriptions. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 XRD patterns of the sodium transition metal oxides with spinel coating layers prepared in Examples 1 to 14 of the present application;
[0031] Figure 2 This is a TEM display of the sodium transition metal oxide with a spinel coating layer prepared in Example 1 of the present application;
[0032] Figure 3 The AC-TEM spherical aberration test was performed on the surface of the sphere of the sodium transition metal oxide with a spinel coating layer prepared in Example 1 of the present application, and the FFT conversion diagram was made;
[0033] Figure 4 A schematic diagram of the first cycle charge and discharge curve of a sodium ion half-cell assembled with the positive electrode material of Example 1 of the present application at 2.0-4.1V and 0.1C;
[0034] Figure 5 Schematic diagram of the long cycle of a sodium ion half-cell assembled with the positive electrode material of Example 1 of the present application and the positive electrode material of Comparative Example 1 at 2.0-4.1V and 0.5C. DETAILED DESCRIPTION
[0035] In order to make the invention purpose and technical solution of the present application clearer and easier to understand, the content of the present application is further described in detail below in conjunction with the accompanying drawings and examples. However, it should be clear that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application. Without departing from the spirit and substance of the present application, modifications and replacements made to the method, preparation steps or conditions of the present application are within the scope of the present application.
[0036] The present invention provides a sodium transition metal oxide positive electrode material having a spinel coating layer. The sodium transition metal oxide having a spinel coating layer has the general formula shown below:
[0037] Na x Ni a Mn b M c O2 0.1(L x Mn 2-c M c O4); where 0.7≤x≤1.0, a>0, b>0, c>0,
[0038] a+b+c=1, M is selected from one of Mg, Al, Fe, Cu, Ti, Co, La, Zn or Zr, and L is one of Li and K. For example, x is 0.7, 0.8, 0.9, 1.0, etc.; a is 0.1, 0.2, 0.3, 0.4, 0.5, etc.; b is 0.1, 0.2, 0.3, 0.4, 0.5, and c is 0.1, 0.2, etc.
[0039] In some embodiments, 0.4≥a≥0.3, 0.6≥b≥0.4, 0.2≥c≥0.1. For example, a is 0.3, 0.4, etc.; b is 0.4, 0.5, 0.6, etc.; c is 0.1, 0.2, etc.
[0040] In some embodiments, the sodium transition metal oxide having a spinel coating layer may be
[0041] Na 1.0 Ni 0.4 Mn 0.5 Ti 0.1 O2·0.1(Li 1.0 Mn 1.9 Ti 0.1 O4)
[0042] Na 1.0 Ni 0.4 Mn 0.5 Mg 0.1 O2·0.1(Li 1.0 Mn 1.9 Mg 0.1 O4)
[0043] Na 1.0 Ni 0.4 Mn 0.5 Zr 0.1 O2·0.1(Li 1.0 Mn 1.9 Zr 0.1 O4)
[0044] Na 1.0 Ni 0.4 Mn 0.5 Al 0.1 O2·0.1(Li 1.0 Mn 1.9 Al 0.1 O4)、Na 1.0 Ni 0.4 Mn 0.5 Cu 0.1 O2·0.1(Li 1.0 Mn 1.9 Cu 0.1 O4)、Na 0.9 Ni 0.4 Mn 0.5 La 0.1 O2·0.1(Li 0.9 Mn 1.9 La 0.1 O4)、Na 0.9 Ni 0.4 Mn 0.4 Fe 0.2 O2·0.1(Li 0.9 Mn 1.8 Fe 0.2 O4)、Na 0.8 Ni 0.3 Mn 0.6Zinc 0.1 O2 0.1(Li 0.8 Mn 1.9 Zinc 0.1 O4), Na 0.7 Ni 0.3 Mn 0.6 Co 0.1 O2 0.1(Li 0.7 Mn 1.9 Co 0.1 O4), Na 1.0 Ni 0.4 Mn 0.5 Ti 0.1 O2 0.1(K 1.0 Mn 1.9 Ti 0.1 O4), Na 1.0 Ni 0.4 Mn 0.5 Mg 0.1 O2 0.1(K 1.0 Mn 1.9 Mg 0.1 O4), Na 1.0 Ni 0.4 Mn 0.5 Fe 0.1 O2 0.1(K 1.0 Mn 1.9 Fe 0.1 O4), Na 1.0 Ni 0.4 Mn 0.5 Al 0.1 O2 0.1(K .1.0 Mn 1.9 Al 0.1 O4), Na 1.0 Ni 0.4 Mn 0.5 Cu 0.1 O2·0.1(K 1.0 Mn 1.9 Cu 0.1 O4) Very little in the middle.
[0045] Like Figure 1 indication, Figure 1 This is the reason
[0046] Na 1.0 Ni 0.4 Mn 0.5 Ti 0.1 O2 0.1(Li 1.0 Mn 1.9 Ti 0.1 O4), Na 1.0 Ni 0.4 Mn0.5 Mg 0.1 O2·0.1(Li 1.0 Mr 1.9 Mg 0.1 O4)、Na 1.0 Ni 0.4 Mr 0.5 Zr 0.1 O2·0.1(Li 1.0 Mr 1.9 Zr 0.1 O4)、Na 1.0 Ni 0.4 Mr 0.5 Al 0.1 O2·0.1(Li 1.0 Mr 1.9 Al 0.1 O4)、Na 1.0 Ni 0.4 Mr 0.5 Cu 0.1 O2·0.1(Li 1.0 Mr 1.9 Cu 0.1 O4)、Na 0.9 Ni 0.4 Mr 0.5 Day 0.1 O2·0.1(Li 0.9 Mr 1.9 Day 0.1 O4)、Na 0.9 Ni 0.4 Mr 0.4 Feb 0.2 O2·0.1(Li 0.9 Mr 1.8 Feb 0.2 O4)、Na 0.8 Ni 0.3 Mr 0.6 Zn 0.1 O2·0.1(Li 0.8 Mr 1.9 Zn 0.1 O4)、Na 0.7 Ni 0.3 Mr 0.6 Co 0.1 O2·0.1(Li 0.7 Mr 1.9 Co 0.1 O4)、Na 1.0 Ni 0.4 Mr 0.5 Tea 0.1 O2·0.1(K 1.0 Mr 1.9 Tea0.1 O4)、Na 1.0 Ni 0.4 Mn 0.5 Mg 0.1 O2·0.1(K 1.0 Mn 1.9 Mg 0.1 O4)、Na 1.0 Ni 0.4 Mn 0.5 Fe 0.1 O2·0.1(K 1.0 Mn 1.9 Fe 0.1 O4)、Na 1.0 Ni 0.4 Mn 0.5 Al 0.1 O2·0.1(K .1.0 Mn 1.9 Al 0.1 O4)、Na 1.0 Ni 0.4 Mn 0.5 Cu 0.1 O2·0.1(K 1.0 Mn 1.9 Cu 0.1 O4)
[0047] Taking the XRD (X-ray diffraction) spectrum as an example, the horizontal axis is twice the incident angle of the x-ray (θ) (2θ, the unit is degree), and the vertical axis is the intensity after diffraction (intensity, au in the figure is the abbreviation of absorbance unit); according to Figure 1 It can be seen that this type of sodium transition metal oxide with a spinel coating has a core crystal form of a pure phase P2 structure or a mixed phase structure of P2 and P3. While maintaining a higher capacity, it can provide better material stability and has a smoother sodium ion deintercalation capability.
[0048] The present application embodiment provides a method for preparing the above-mentioned sodium transition metal oxide positive electrode material with a spinel coating layer, which comprises the following steps:
[0049] According to the stoichiometric ratio, nickel salt, manganese salt and M salt are used to prepare a first mixed solution containing nickel ions, manganese ions and M ions, and a second mixed solution containing manganese ions and M ions. The first mixed solution is first subjected to titration precipitation by a step-by-step titration co-precipitation method. After the reaction is complete, the second mixed solution is added to further perform titration precipitation. During the process, the pH value is controlled and the grains are slowly grown so that the particle size of the obtained co-precipitation precursor is 6-10 um. After spray drying, a first transition metal carbonate or hydroxide precipitation precursor is obtained.
[0050] According to the stoichiometric ratio, the sodium-containing compound, the L-containing compound and the first transition metal carbonate or hydroxide precipitation precursor are mixed and sintered to obtain the sodium transition metal oxide positive electrode material with a spinel coating layer.
[0051] The present application provides another method for preparing the above-mentioned sodium transition metal oxide positive electrode material with a spinel coating layer, which comprises the following steps:
[0052] According to the stoichiometric ratio, nickel salt and manganese salt are used to prepare a third mixed solution containing nickel and manganese ions, and a fourth mixed solution containing manganese ions. The third mixed solution is first subjected to titration precipitation by a step-by-step titration co-precipitation method. After the reaction is complete, the fourth mixed solution is added and further titration precipitation is performed. During the process, the pH value is controlled and the grains are slowly grown so that the particle size of the obtained co-precipitation precursor is 6-10 um. After spray drying, a second transition metal carbonate or hydroxide precipitation precursor is obtained.
[0053] According to the stoichiometric ratio, the sodium-containing compound, the second transition metal carbonate or hydroxide precipitation precursor, the L-containing compound, and the M-containing compound are mixed and sintered to obtain the sodium transition metal oxide positive electrode material with a spinel coating layer.
[0054] The preparation method is explained in detail below.
[0055] The nickel salt involved in the raw material can be at least one of nickel sulfate, nickel acetate, and nickel nitrate; the manganese salt is selected from at least one of manganese sulfate, manganese acetate, and manganese nitrate; and the M salt can be at least one of sulfate M salt, acetate M salt, nitrate M salt, and acetate M salt, where M represents one of Mg, Al, Fe, Cu, Ti, Co, La, Zn, or Zr, and L represents one of Li and K. Before the coprecipitation reaction, it is necessary to prepare the nickel salt, manganese salt, and M salt into corresponding aqueous solutions to improve the reaction efficiency of the coprecipitation reaction.
[0056] In some embodiments, when nickel salt, manganese salt and M salt are mixed and dissolved in water, the total feed ratio of the nickel salt, manganese salt and M salt for co-precipitation reaction is (0.5-1):1:(0-0.5) according to the molar ratio.
[0057] In some embodiments, when performing a co-precipitation reaction, a precipitant needs to be added to the solution. The precipitant adjusts the pH value of the reaction system and controls the slow growth of the grains to 6-10 um.
[0058] In some embodiments, the precipitant used in the embodiments of the present application can be a mixed solution of sodium carbonate and ammonia water or a sodium hydroxide solution.
[0059] In some embodiments, when a sodium-containing compound, an L-containing compound and a first transition metal carbonate or hydroxide precipitation precursor are mixed, the molar ratio of sodium in the sodium-containing compound: first transition metal carbonate or hydroxide precipitation precursor: L in the L-containing compound is (0.7-1):1:(0.07-0.1).
[0060] In some embodiments, the sodium-containing compound is at least one of sodium carbonate, sodium acetate, and sodium hydroxide.
[0061] In some embodiments, the L-containing compound is at least one of an L-containing carbonate and an L-containing hydroxide.
[0062] In some embodiments, the nickel salt and manganese salt are first subjected to a coprecipitation reaction according to a molar ratio, and the total feed ratio is (0.5-1):1 to prepare a second transition metal carbonate or hydroxide precipitation precursor. Then, the sodium-containing compound, the second transition metal carbonate or hydroxide precipitation precursor, the L-containing compound, and the M-containing compound are mixed and sintered, and according to the molar ratio, the sodium in the sodium-containing compound: the second transition metal carbonate or hydroxide precipitation precursor: the M in the M-containing compound: the L in the L-containing compound = (0.7-1):1:(0.11-0.22):(0.07-0.1).
[0063] In some embodiments, the sodium-containing compound is at least one of sodium carbonate, sodium acetate, and sodium hydroxide.
[0064] In some embodiments, the L-containing compound is at least one of an L-containing carbonate and an L-containing hydroxide; the M-containing compound is at least one of an M-containing metal oxide, an M-containing oxide, an M-containing carbonate, and an M-containing hydroxide.
[0065] In some embodiments, when the sodium-containing compound, the L-containing compound and the first transition metal carbonate or hydroxide precipitation precursor are mixed, or when the sodium-containing compound, the second transition metal carbonate or hydroxide precipitation precursor and the L-containing compound, the M-containing compound are mixed, mechanical grinding can be adopted, or the two can be made into a solution, mixed and ultrasonically shaken to form a slurry, and then dried, ball milled, etc. The purpose of mixing is to make the sodium-containing compound, the L-containing compound and the first transition metal carbonate or hydroxide precipitation precursor mixed evenly, or to make the sodium-containing compound, the second transition metal carbonate or hydroxide precipitation precursor and the L-containing compound, the M-containing compound mixed evenly, so as to facilitate sintering into a sodium transition metal oxide positive electrode material with a spinel coating layer.
[0066] In some embodiments, the sintering conditions are to first sinter at a constant temperature of 300-500°C for 1-5 hours, then quickly heat up to 900-1050°C to melt the lithium-containing compound and the sodium-containing compound at the same time, and sinter at a constant temperature for 12-24 hours. The sintering atmosphere is oxygen or air or a mixture of oxygen and air.
[0067] The method for preparing the sodium transition metal oxide positive electrode material with a spinel coating layer in the embodiment of the present application can be obtained by co-precipitation combined with calcination, and has the characteristics of cheap and readily available raw materials and a simple preparation process. The obtained sodium transition metal oxide positive electrode material with a spinel coating layer has a complete crystal form and high purity.
[0068] Since the sodium transition metal oxide positive electrode material with a spinel coating layer is used as the active material of the positive electrode, the positive electrode material has a typical core-shell protection structure, with a layered transition metal oxide as the core (P2, P3 phase or mixed phase) and a spinel shell coated on the surface as a protective layer, while having a higher gram capacity, the material stability is enhanced; the prepared sodium ion battery has been greatly improved in terms of gram capacity, cycle stability, etc. Therefore, the embodiment of the present application also provides a positive electrode sheet and a sodium ion battery of the sodium transition metal oxide positive electrode material with a spinel coating layer as described above.
[0069] Among them, the positive electrode sheet uses a sodium transition metal oxide positive electrode material with a spinel coating layer as the positive electrode active material, and also contains a conductive agent and a binder.
[0070] Specifically, the sodium transition metal oxide positive electrode material with a spinel coating layer is mixed with a conductive agent, a binder and a solvent to form a positive electrode slurry, which is coated on the surface of the positive electrode current collector, and then dried, rolled and cut into pieces to form a positive electrode sheet. The mass ratio of the sodium transition metal oxide positive electrode material with a spinel coating layer, the conductive agent and the binder in the positive electrode sheet is 8:1:1. When preparing the positive electrode slurry, the solvent can be N-methylpyrrolidone (NMP).
[0071] The sodium ion battery includes the above-mentioned positive electrode sheet, or the positive electrode material contains the sodium transition metal oxide positive electrode material with a spinel coating layer according to the embodiment of the present application.
[0072] In some embodiments, the positive electrode material of the sodium ion battery of the embodiment of the present application, the core portion of the sodium transition metal oxide positive electrode material having a spinel coating layer may contain at least one of a P2 phase transition metal oxide, a P3 phase transition metal oxide, and an O3 phase transition metal oxide.
[0073] In some embodiments, the sodium ion battery provided in the embodiments of the present application uses metallic sodium as the negative electrode material, and the electrolyte is any one of 1M NaPF6 / (EC:DMC=1:1) electrolyte, 1M NaPF6 / PC electrolyte, and 1M NaClO4 / (EC:PC=1:1) electrolyte, wherein EC represents ethylene carbonate, DMC represents dimethyl carbonate, PC represents propylene carbonate, EC:DMC=1:1 represents a solvent formed by ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1, and EC:PC represents a solvent formed by ethylene carbonate and propylene carbonate in a volume ratio of 1:1.
[0074] In some embodiments, the sodium ion battery provided in the embodiments of the present application uses a diaphragm that is a polyolefin microporous membrane such as polyethylene, polypropylene, etc., such as a Celgard diaphragm.
[0075] Example 1
[0076] A method for preparing a sodium transition metal oxide positive electrode material having a spinel coating layer comprises the following steps:
[0077] (a) mixing and dissolving nickel sulfate and manganese sulfate in water at a molar ratio of 0.4:0.5 to prepare a first mixed solution with a total transition metal ion concentration of 0.9 mol / L; and dissolving manganese sulfate alone in water to prepare a second mixed solution with a total transition metal ion concentration of 0.19 mol / L;
[0078] In the first stage of the reaction, 100 mL of the first mixed solution is added, and a mixed aqueous solution of 1.0 mol / L sodium carbonate and 0.10 mol / L ammonia water is used as a precipitant, and the pH value is controlled to allow a precipitation reaction to proceed; after the precipitation reaction in the first stage is completed, 100 mL of the second mixed solution is added in the second stage, and the precipitant is continuously added dropwise to allow the grains to further grow slowly. In the two-step reaction, the total molar ratio of nickel sulfate to manganese sulfate is controlled to be 0.4:(0.5+0.19) to prepare a nickel-manganese gradient distribution carbonate precursor, and the obtained precursor is spray-dried to obtain a powder.
[0079] (b) Sodium carbonate, the carbonate precursor powder obtained in step (a), lithium carbonate and titanium oxide are mixed in a molar ratio of 0.5:1.09:0.05:0.11 and added into a ball mill together with grinding beads of the same weight, and ball milled at a speed of 200 r / min for 2 h. The mixed powder is taken out and mixed evenly in a mortar.
[0080] (c) The powder mixed in step (b) was pressed into a disc with a diameter of 20 mm on a cold press at a pressure of 100 MPa for 5 min.
[0081] (d) The pressed flake mixture in step (c) was placed in a tubular furnace, heated to 500°C in a mixed atmosphere of oxygen and air (mixing ratio 1:5) and sintered at a constant temperature for 4 hours, then heated to 1000°C and sintered at a constant temperature for 20 hours, and naturally cooled to room temperature to obtain sample 1. Its molecular formula is Na 1.0 Ni 0.4 Mn 0.5 Ti 0.1 O2·0.1(Li 1.0 Mn 1.9 Ti 0.1 O4), the particle size is 8 to 15 μm. The obtained sample 1 was subjected to XRD and TEM (Transmission Electron Microscope, transmission electron microscope) tests, and the surface of the sphere was subjected to AC-TEM spherical aberration test (Spherical Aberration Corrected Transmission Electron Microscope, spherical aberration correction transmission electron microscope), and the spherical aberration data of the obtained surface coating layer was converted by FFT and plotted. The specific test results are detailed in Figure 1 and Figure 2 , the long cycle performance is shown in Table 1.
[0082] Example 2
[0083] Referring to Example 1, nickel sulfate and manganese sulfate were prepared in a total molar ratio of 0.4: (0.5 + 0.19) to prepare a carbonate precursor, magnesium oxide was used to replace the titanium oxide in Example 1, sodium carbonate, the prepared carbonate precursor, lithium carbonate, and magnesium oxide were mixed in a molar ratio of 0.5: 1.09: 0.05: 0.11, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high temperature ion replacement. 1.0 Ni 0.4 Mn 0.5 Mg 0.1 O2·0.1(Li 1.0 Mn 1.9 Mg 0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0084] Example 3
[0085] Referring to Example 1, nickel sulfate and manganese sulfate were prepared in a total molar ratio of 0.4: (0.5 + 0.19) to prepare a carbonate precursor, zirconium oxide was used to replace the titanium oxide in Example 1, sodium carbonate, the prepared carbonate precursor, lithium carbonate, and zirconium oxide were mixed in a molar ratio of 0.5: 1.09: 0.05: 0.11, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high temperature ion replacement. 1.0 Ni 0.4 Mn 0.5 Zr 0.1 O2·0.1(Li 1.0 Mn 1.9 Zr 0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0086] Example 4
[0087] Referring to Example 1, a carbonate precursor was prepared by using nickel sulfate and manganese sulfate in a total molar ratio of 0.4:(0.5+0.19), and aluminum oxide was used to replace the titanium oxide in Example 1. Sodium carbonate, the prepared carbonate precursor, lithium carbonate, and aluminum oxide were mixed in a molar ratio of 0.5:1.09:0.05:0.055, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high-temperature ion replacement. 1.0 Ni 0.4 Mn 0.5 Al 0.1 O2·0.1(Li 1.0 Mn 1.9 Al 0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0088] Example 5
[0089] Referring to Example 1, nickel sulfate and manganese sulfate were prepared in a total molar ratio of 0.4: (0.5 + 0.19) to prepare a carbonate precursor, copper oxide was used to replace the titanium oxide in Example 1, sodium carbonate, the prepared carbonate precursor, lithium carbonate, and copper oxide were mixed in a molar ratio of 0.5: 1.09: 0.05: 0.11, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high temperature ion replacement. 1.0 Ni 0.4 Mn 0.5 Cu 0.1 O2·0.1(Li 1.0 Mn 1.9 Cu0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0090] Example 6
[0091] Referring to Example 1, nickel sulfate and manganese sulfate were prepared in a total molar ratio of 0.4: (0.5 + 0.19) to prepare a carbonate precursor, lanthanum oxide was used to replace the titanium oxide in Example 1, sodium carbonate, the prepared carbonate precursor, lithium carbonate, and lanthanum oxide were mixed in a molar ratio of 0.45: 1.09: 0.045: 0.055, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high temperature ion replacement. 0.9 Ni 0.4 Mn 0.5 La 0.1 O2·0.1(Li 0.9 Mn 1.9 La 0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0092] Example 7
[0093] Referring to Example 1, a carbonate precursor was prepared by using nickel sulfate and manganese sulfate in a total molar ratio of 0.4:(0.4+0.18), ferrous oxide was used to replace the titanium oxide in Example 1, and sodium carbonate, the prepared carbonate precursor, lithium carbonate, and ferrous oxide were mixed in a molar ratio of 0.45:0.98:0.045:0.22, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high-temperature ion replacement. 0.9 Ni 0.4 Mn 0.4 Fe 0.2 O2·0.1(Li 0.9 Mn 1.8 Fe 0.2 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0094] Example 8
[0095] Referring to Example 1, nickel sulfate and manganese sulfate were prepared in a total molar ratio of 0.3: (0.6 + 0.19) to prepare a carbonate precursor, zinc oxide was used to replace the titanium oxide in Example 1, sodium carbonate, the prepared carbonate precursor, lithium carbonate, and zinc oxide were mixed in a molar ratio of 0.4: 1.09: 0.04: 0.11, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high temperature ion replacement. 0.8 Ni 0.3 Mn 0.6 Zn 0.1 O2·0.1(Li 0.8 Mn 1.9 Zn 0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0096] Example 9
[0097] Referring to Example 1, nickel sulfate and manganese sulfate were prepared in a total molar ratio of 0.3: (0.6 + 0.19) to prepare a carbonate precursor, cobalt trioxide was used to replace the titanium oxide in Example 1, sodium carbonate, the prepared carbonate precursor, lithium carbonate, and cobalt trioxide were mixed in a molar ratio of 0.35: 1.09: 0.035: 0.055, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high temperature ion replacement. 0.7 Ni 0.3 Mn 0.6 Co 0.1 O2·0.1(Li 0.7 Mn 1.9 Co 0.1 O -4 ), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0098] Example 10
[0099] Referring to Example 1, nickel sulfate and manganese sulfate were prepared in a total molar ratio of 0.4: (0.5 + 0.19) to prepare a carbonate precursor, potassium carbonate was used to replace the lithium carbonate in Example 1, sodium carbonate, the prepared carbonate precursor, potassium carbonate, and titanium oxide were mixed in a molar ratio of 0.5: 1.09: 0.05: 0.11, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high temperature ion replacement. 1.0 Ni 0.4 Mn 0.5 Ti 0.1 O2·0.1(K 1.0 Mn1.9 Ti 0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0100] Embodiment 11
[0101] Referring to Example 1, nickel sulfate and manganese sulfate were used in a total molar ratio of 0.4: (0.5 + 0.19) to prepare a carbonate precursor, potassium carbonate was used to replace the lithium carbonate in Example 1, and magnesium oxide was used to replace the titanium oxide in Example 1. Sodium carbonate, the prepared carbonate precursor, potassium carbonate, and magnesium oxide were mixed in a molar ratio of 0.5: 1.09: 0.05: 0.11, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high-temperature ion replacement. 1.0 Ni 0.4 Mn 0.5 Mg 0.1 O2·0.1(K 1.0 Mn 1.9 Mg 0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0102] Example 12
[0103] Referring to Example 1, nickel sulfate and manganese sulfate were used in a total molar ratio of 0.4: (0.5 + 0.19) to prepare a carbonate precursor, potassium carbonate was used to replace the lithium carbonate in Example 1, and ferrous oxide was used to replace the titanium oxide in Example 1. Sodium carbonate, the prepared carbonate precursor, potassium carbonate, and ferrous oxide were mixed in a molar ratio of 0.5: 1.09: 0.05: 0.11, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high-temperature ion replacement. 1.0 Ni 0.4 Mn 0.5 Fe 0.1 O2·0.1(K 1.0 Mn 1.9 Fe 0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0104] Example 13
[0105] Referring to Example 1, nickel sulfate and manganese sulfate were prepared in a total molar ratio of 0.4: (0.5 + 0.19) to prepare a carbonate precursor, potassium carbonate was used to replace the lithium carbonate in Example 1, and aluminum oxide was used to replace the titanium oxide in Example 1. Sodium carbonate, the prepared carbonate precursor, potassium carbonate, and aluminum oxide were mixed in a molar ratio of 0.5: 1.09: 0.05: 0.055, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high-temperature ion replacement. 1.0 Ni 0.4 Mn 0.5 Al 0.1 O2·0.1(K .1.0 Mn 1.9 Al 0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0106] Embodiment 14
[0107] Referring to Example 1, nickel sulfate and manganese sulfate were used in a total molar ratio of 0.4: (0.5 + 0.19) to prepare a carbonate precursor, potassium carbonate was used to replace the lithium carbonate in Example 1, and copper oxide was used to replace the titanium oxide in Example 1. Sodium carbonate, the prepared carbonate precursor, potassium carbonate, and copper oxide were mixed in a molar ratio of 0.5: 1.09: 0.05: 0.11, and then the treatment method in Example 1 was used to obtain a sodium ion battery positive electrode material Na with a surface spinel coating layer formed by high-temperature ion replacement. 1.0 Ni 0.4 Mn 0.5 Cu 0.1 O2·0.1(K 1.0 Mn 1.9 Cu 0.1 O4), its XRD spectrum is as follows Figure 1 The long cycle performance is shown in Table 1.
[0108] Comparative Example 1
[0109] A sodium transition metal oxide positive electrode material without ion replacement to form a surface spinel coating layer:
[0110] (a) nickel sulfate and manganese sulfate are mixed and dissolved in water at a molar ratio of 0.4:0.5 to prepare a mixed transition metal salt solution of nickel sulfate and manganese sulfate with a total transition metal ion concentration of 1.0 mol / L, and a mixed aqueous solution of 1.0 mol / L sodium carbonate and 0.10 mol / L ammonia water is used as a precipitant, and the pH value is controlled to prepare a nickel manganese carbonate precursor by coprecipitation.
[0111] (b) sodium carbonate, the carbonate precursor obtained in step (a) and titanium oxide in a molar ratio of 0.5:0.9:
[0112] 0.1 ratio and add into the spherical ink tank and ball milling balls, and ball mill at a speed of 200r / min for 2h.
[0113] Take out the mixed powder and mix well in a mortar.
[0114] (c) The uniformly mixed precursor powders were pressed into discs with a diameter of 20 mm on a cold press at a pressure of 100 MPa for 5 min.
[0115] (d) The pressed flake mixture in step (c) was placed in a tubular furnace, heated to 500° C. and sintered at a constant temperature for 4 h in a mixed atmosphere of oxygen and air (mixing ratio 1:5), then heated to 1000° C. and sintered at a constant temperature for 20 h, and naturally cooled to room temperature to obtain a comparative example sample Na 1.0 Ni 0.4 Mn 0.5 Ti 0.1 O2, its XRD spectrum is as follows Figure 2 shown.
[0116] Application Example 1
[0117] A sodium ion battery, the preparation method of which comprises the following steps:
[0118] (1) The sample obtained in Example 1 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0119] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0120] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0121] Application Example 2
[0122] A sodium ion battery, the preparation method of which comprises the following steps:
[0123] (1) The sample obtained in Example 2 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0124] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0125] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0126] Application Example 3
[0127] A sodium ion battery, the preparation method of which comprises the following steps:
[0128] (1) The sample obtained in Example 3 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0129] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0130] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0131] Application Example 4
[0132] A sodium ion battery, the preparation method of which comprises the following steps:
[0133] (1) The sample obtained in Example 4 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0134] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0135] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0136] Application Example 5
[0137] A sodium ion battery, the preparation method of which comprises the following steps:
[0138] (1) The sample obtained in Example 5 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0139] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0140] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0141] Application Example 6
[0142] A sodium ion battery, the preparation method of which comprises the following steps:
[0143] (1) The sample obtained in Example 6 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0144] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0145] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0146] Application Example 7
[0147] A sodium ion battery, the preparation method of which comprises the following steps:
[0148] (1) The sample obtained in Example 7 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0149] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0150] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0151] Application Example 8
[0152] A sodium ion battery, the preparation method of which comprises the following steps:
[0153] (1) The sample obtained in Example 8 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0154] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0155] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0156] Application Example 9
[0157] A sodium ion battery, the preparation method of which comprises the following steps:
[0158] (1) The sample obtained in Example 9 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0159] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0160] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0161] Application Example 10
[0162] A sodium ion battery, the preparation method of which comprises the following steps:
[0163] (1) The sample obtained in Example 10 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0164] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0165] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0166] Application Example 11
[0167] A sodium ion battery, the preparation method of which comprises the following steps:
[0168] (1) The sample obtained in Example 11 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0169] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0170] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0171] Application Example 12
[0172] A sodium ion battery, the preparation method of which comprises the following steps:
[0173] (1) The sample obtained in Example 12 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0174] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0175] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0176] Application Example 13
[0177] A sodium ion battery, the preparation method of which comprises the following steps:
[0178] (1) The sample obtained in Example 13 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0179] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0180] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0181] Application Example 14
[0182] A sodium ion battery, the preparation method of which comprises the following steps:
[0183] (1) The sample obtained in Example 14 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0184] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0185] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0186] Application Example 15
[0187] A sodium ion battery, the preparation method of which comprises the following steps:
[0188] (1) The sample obtained in Comparative Example 1 was used as a positive electrode active material, mixed with conductive carbon black and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1, dissolved in N-methylpyrrolidone (NMP) solvent to prepare a positive electrode slurry, and coated on an aluminum foil, dried, and cut to obtain a positive electrode sheet.
[0189] (2) The positive electrode obtained in step (1) was assembled with metal sodium and Celgard separator into a sodium ion battery, wherein the electrolyte of the sodium ion battery was a mixture of 1M NaPF6 / (EC:DMC=1:1) (according to the volume ratio of EC:DMC=1:1). After assembly, the battery was allowed to stand for 24 hours, and then subjected to charge and discharge activation test.
[0190] Specifically, the test method is: charge and discharge three times at a current density of 0.1C (1C = 100 mA / g) within a voltage range of 2.0-4.1V; and then perform a cycle performance test at 0.5C (1C = 100 mA / g). The results are shown in Table 1.
[0191] Figure 1 The diffraction peaks of all samples from Example 1 to Example 14 show the P2 structure or P3 structure of sodium transition metal oxide (or a mixed phase of P2 and P3), and there are fewer impurity peaks, which proves that the main material obtained is a sodium-containing transition metal oxide positive electrode material, namely Na x Ni a Mnb M c O2 part. However, the spinel structure as the coating layer is difficult to directly observe in the XRD diffraction peak due to its low content, so the positive electrode material of the embodiment of the present application uses a more precise TEM (transmission electron microscope) and AC-TEM (spherical aberration corrected transmission electron microscope) to further analyze the obtained positive electrode material.
[0192] from Figure 2 It can be seen from the TEM (transmission electron microscope) that sample 1 of Example 1 has a spherical structure, and the crystals in the core part are distributed periodically, and the structure contains two phases (P2 phase and P3 phase) with a clear boundary line. Please note that Figure 2 The dimension in the lower left corner is 50 nm.
[0193] Figure 3 In this application, the material sphere of Example 1 was subjected to AC-TEM spherical aberration test (spherical aberration corrected transmission electron microscope), and the obtained surface coating layer spherical aberration data was FFT converted and plotted to obtain the accurate surface coating material lattice (unit cell) shape. Figure 3 It can be seen that under extremely microscopic conditions, the crystal structure unit cell shows a spinel structure (rhombohedral structure), proving that the surface coating structure of the material of the present application is a spinel coating layer (Li x Mn 2-c M c O4).
[0194] Of course, during the reaction, due to the effects of high temperature kinetics and thermodynamics, Li or K and Na undergo heat exchange (high temperature ion replacement), so the core part can also be shown as Na x Li y Ni a Mn b M c O2 structure or Na x K y Ni a Mn b M c O2 structure, and the surface-coated spinel structure can also be (Li x Na y Mn 2-c M c O4) or (K x Na y Mn 2-c M c O4), but the above ion replacement does not affect its crystal structure, that is, it does not affect the XRD, TEM, and AC-TEM test results.
[0195] The sodium transition metal oxide positive electrode material Na with a spinel coating layer obtained in Example 1 1.0 Ni 0.4 Mn 0.5 Ti 0.1 O2·0.1(Li 1.0 Mn 1.9 Ti 0.1 O4) was used as the positive electrode material and sodium metal negative electrode to assemble sodium ion batteries and conduct electrochemical performance tests. Figure 4 As shown, in the voltage range of 2.0 to 4.1 V, the first charge capacity is about 120 mAh / g and the discharge capacity is about 115 mAh / g when cycled at a current density of 0.1 C (10 mA / g).
[0196] like Figure 5 As shown, the material obtained in Example 1 still has a reversible capacity of about 105 mAh / g when cycled at 0.5C (50 mA / g), and the capacity retention rate after 100 cycles is about 98%, while the material in Comparative Example 1, due to the absence of an external spinel protective layer, has a capacity retention rate of only 80% after 100 cycles; this indicates that the structural changes of the material in Example 1 are highly reversible during the electrochemical cycle, and because of the protection of the external spinel layer, the core of the material is completely undamaged during the charge and discharge process, and the stability is extremely high. Therefore, the sodium transition metal oxide positive electrode material with a spinel coating layer in the embodiment of the present application has extremely stable long-cycle capabilities based on the design of the core-shell structure and the protection of the external spinel layer, and has great potential for use in energy storage and related equipment.
[0197] Table 1
[0198]
[0199] It should be understood that the terms used in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application.
[0200] It should also be understood that the term “and / or” used in the specification and appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0201] The above is only a specific embodiment of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A sodium transition metal oxide positive electrode material having a spinel coating layer, characterized in that: The sodium transition metal oxide with a spinel coating layer of the positive electrode material has the following general formula: So x Ni a Mr b M c O2·0.1(L x Mr 2-c M c O4); Among them, 0.7≤x≤1.0, a>0, b>0, c>0, a+b+c=1, M is selected from one of Mg, Al, Fe, Cu, Ti, Co, La, Zn or Zr, and L is one of Li and K.
2. The positive electrode material according to claim 1, characterized in that 0.4≥a≥0.3, 0.6≥b≥0.4, 0.2≥c≥0.
1.
3. The positive electrode material according to claim 1, characterized in that The positive electrode material presents a core-shell structure, wherein the shell is a spinel structure, and the core can be at least one of a P2 phase transition metal oxide, a P3 phase transition metal oxide or an O3 phase transition metal oxide.
4. The positive electrode material according to claim 2, characterized in that The sodium transition metal oxide having a spinel coating layer is Na 1.0 Ni 0.4 Mn 0.5 Ti 0.1 O2·0.1(Li 1.0 Mn 1.9 Ti 0.1 O4) So 1.0 Ni 0.4 Mr 0.5 Mg 0.1 O2·0.1(Li 1.0 Mr 1.9 Mg 0.1 O4) Na 1.0 Ni 0.4 Mn 0.5 Zr 0.1 O2·0.1(Li 1.0 Mn 1.9 Zr 0.1 O4)、 <h2 style=";text-align:left;direction:ltr">Na<h2 style=";text-align:left;direction:ltr"> 1.0 <h2 style=";text-align:left;direction:ltr"> Ni<h2 style=";text-align:left;direction:ltr"> 0.4 <h2 style=";text-align:left;direction:ltr"> Mn<h2 style=";text-align:left;direction:ltr"> 0.5 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.1 <h2 style=";text-align:left;direction:ltr"> O2·0.1(Li<h2 style=";text-align:left;direction:ltr"> 1.0 <h2 style=";text-align:left;direction:ltr"> Mn<h2 style=";text-align:left;direction:ltr"> 1.9 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.1 <h2 style=";text-align:left;direction:ltr"> O4) So 1.0 Ni 0.4 Mr 0.5 Cu 0.1 O2·0.1(Li 1.0 Mr 1.9 Cu 0.1 O4) So 0.9 Ni 0.4 Mr 0.5 Day 0.1 O2·0.1(Li 0.9 Mr 1.9 Day 0.1 O4) So 0.9 Ni 0.4 Mr 0.4 Feb 0.2 O2·0.1(Li 0.9 Mr 1.8 Feb 0.2 O4) So 0.8 Ni 0.3 Mr 0.6 Zn 0.1 O2·0.1(Li 0.8 Mr 1.9 Zn 0.1 O4) So 0.7 Ni 0.3 Mr 0.6 Co 0.1 O2·0.1(Li 0.7 Mr 1.9 Co 0.1 O4) Na 1.0 Ni 0.4 Mn 0.5 You 0.1 O2·0.1(K 1.0 Mn 1.9 You 0.1 O4)、 That 1.0 By 0.4 Mn 0.5 Mg 0.1 O2·0.1(K 1.0 Mn 1.9 Mg 0.1 O4)、 So 1.0 Ni 0.4 Mr 0.5 Feb 0.1 O2·0.1(K 1.0 Mr 1.9 Feb 0.1 O4) <h2 style=";text-align:left;direction:ltr">Na<h2 style=";text-align:left;direction:ltr"> 1.0 <h2 style=";text-align:left;direction:ltr"> Ni<h2 style=";text-align:left;direction:ltr"> 0.4 <h2 style=";text-align:left;direction:ltr"> Mn<h2 style=";text-align:left;direction:ltr"> 0.5 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.1 <h2 style=";text-align:left;direction:ltr"> O2·0.1(K<h2 style=";text-align:left;direction:ltr"> .1.0 <h2 style=";text-align:left;direction:ltr"> Mn<h2 style=";text-align:left;direction:ltr"> 1.9 <h2 style=";text-align:left;direction:ltr"> Al<h2 style=";text-align:left;direction:ltr"> 0.1 <h2 style=";text-align:left;direction:ltr"> O4) Na 1.0 Ni 0.4 Mn 0.5 Cu 0.1 O2·0.1(K 1.0 Mn 1.9 Cu 0.1 O4) at least one.
5. A method for preparing a sodium transition metal oxide positive electrode material having a spinel coating layer as claimed in any one of claims 1 to 4, characterized in that: The preparation method comprises: According to the stoichiometric ratio, a nickel salt, a manganese salt, and an M salt are mixed and dissolved in water respectively to prepare a first mixed solution containing nickel ions, manganese ions, and M ions, and a second mixed solution containing manganese ions and M ions, and a step-by-step titration co-precipitation method is used to first titrate and precipitate the first mixed solution, and after the reaction is complete, the second mixed solution is added to further titrate and precipitate, during which the pH value is controlled and the grain growth is slowly performed, so that the particle size of the obtained co-precipitation precursor is 6-10 um, and the first transition metal carbonate or hydroxide precipitation precursor is obtained after spray drying; According to the stoichiometric ratio, the sodium-containing compound, the L-containing compound and the first transition metal carbonate or hydroxide precipitation precursor are mixed and sintered to obtain the sodium transition metal oxide positive electrode material with a spinel coating layer.
6. The preparation method according to claim 5, characterized in that: According to the molar ratio, the total feed ratio of the nickel salt, manganese salt and M salt for the coprecipitation reaction is (0.5-1):1:(0-0.5); The sodium-containing compound is at least one of sodium carbonate, sodium acetate, and sodium hydroxide; the L-containing compound is at least one of L-containing carbonate and L-containing hydroxide; According to the molar ratio, the sodium in the sodium-containing compound: the first transition metal carbonate or hydroxide precipitation precursor: the L in the L-containing compound = (0.7-1): 1: (0.07-0.1); The sintering conditions are: first sinter at a constant temperature of 300-500°C for 1-5 hours, then quickly heat up to 900-1050°C to melt the L-containing compound and the sodium-containing compound at the same time, and sinter at a constant temperature for 12-24 hours. The sintering atmosphere is oxygen or air or a mixture of oxygen and air.
7. A method for preparing a sodium transition metal oxide positive electrode material having a spinel coating layer as claimed in any one of claims 1 to 4, characterized in that: The preparation method comprises: According to the stoichiometric ratio, a nickel salt and a manganese salt are mixed and dissolved in water to prepare a third mixed solution containing nickel ions and manganese ions, and a fourth mixed solution containing manganese ions. The third mixed solution is first subjected to titration precipitation by a step-by-step titration coprecipitation method. After the reaction is complete, the fourth mixed solution is added to further perform titration precipitation. During the process, the pH value is controlled and the grains are slowly grown so that the particle size of the obtained coprecipitation precursor is 6-10 um. After spray drying, a second transition metal carbonate or hydroxide precipitation precursor is obtained. According to the stoichiometric ratio, the sodium-containing compound, the second transition metal carbonate or hydroxide precipitation precursor, the L-containing compound, and the M-containing compound are mixed and sintered to obtain the sodium transition metal oxide positive electrode material with a spinel coating layer.
8. The preparation method according to claim 7, characterized in that: According to the molar ratio, the total feed ratio of the nickel salt and the manganese salt for the coprecipitation reaction is (0.5-1):1; The sodium-containing compound is at least one of sodium carbonate, sodium acetate, and sodium hydroxide; the L-containing compound is at least one of L-containing carbonate and L-containing hydroxide; the M-containing compound is at least one of M-containing metal oxide, M-containing oxide, M-containing carbonate, and M-containing hydroxide; According to the molar ratio, the sodium in the sodium-containing compound: the second transition metal carbonate or hydroxide precipitation precursor: the M in the M-containing compound: the L in the L-containing compound = (0.7-1): 1: (0.11-0.22): (0.07-0.1). The sintering conditions are: first sinter at a constant temperature of 300-500°C for 1-5 hours, then quickly heat up to 900-1050°C to melt the lithium-containing compound and the sodium-containing compound at the same time, and sinter at a constant temperature for 12-24 hours. The sintering atmosphere is oxygen or air or a mixture of oxygen and air.
9. A sodium ion battery comprising a positive electrode material, characterized in that: The positive electrode material comprises the sodium transition metal oxide positive electrode material with a spinel coating layer as described in any one of claims 1 to 4, or comprises the sodium transition metal oxide positive electrode material with a spinel coating layer prepared by the preparation method as described in any one of claims 5 to 8.
10. The sodium ion battery according to claim 9, characterized in that: The core part of the positive electrode material may be at least one of a P2 phase transition metal oxide, a P3 phase transition metal oxide, and an O3 phase transition metal oxide.
Citation Information
Cited By
Sodium ferric phosphate pyrophosphate material of high-voltage platform, positive pole piece, battery cell and preparation method of sodium ferric phosphate pyrophosphate material
CN120600794A
The invention relates to a spinel phase coated P2 / P3 / O3 / Oapos and a preparation method thereof. 3 composite layered oxide material, preparation method and application
CN120933363A
A spinel-coated p2 / p3 / o3 / o'3 composite layered oxide material, a preparation method and applications
CN120933363B