Positive electrode active material and application thereof
By arranging a coating layer of polysilotitanoxane and carbon material on the surface of the positive electrode material of the secondary battery, the deficiencies in high temperature and cycle performance of the battery are solved, and higher stability and efficiency are achieved.
Patent Information
- Application Number
- CN202410799711.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-01
AI Technical Summary
Existing secondary batteries have deficiencies in high temperature and cycle performance, which affect their application efficiency and stability.
A cathode active material including a core and a coating layer is used. The core is composed of a material with active ions, and the coating layer is composed of polysilotitanoxane and carbon materials. The coating layer is provided on the surface of the cathode material to improve the performance of the battery. High temperature performance and cycle performance.
It significantly improves the high-temperature performance, cycle performance and rate performance of the battery, reduces the dissolution rate of transition metal ions, and enhances the conductivity and stability of the cathode active material.
Smart Images

Figure BDA0004902997420000141 
Figure BDA0004902997420000151 
Figure BDA0004902997420000171
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary batteries and relates to a positive electrode active material, in particular to a positive electrode active material and an application thereof. Background Art
[0002] Faced with the insufficient supply of fossil energy and the environmental pollution caused by fossil energy, it has become a top priority to actively develop and utilize renewable energy and large-scale power storage technology. Secondary batteries are one of the most developed energy storage devices and are widely used in electric vehicles, home energy storage, start-stop power supplies, portable electronic devices and other fields.
[0003] Existing secondary batteries mainly include lead-acid batteries, nickel-metal hydride batteries, lithium-ion batteries, sodium-ion batteries, potassium-ion batteries, etc. However, in order to meet higher requirements, the cycle performance and high-temperature performance of the battery still need to be further improved, and the positive electrode active material, as one of the key components of the battery, plays a decisive role in the electrochemical performance of the battery.
[0004] Therefore, it is necessary to further optimize the positive electrode active materials in the battery to effectively improve the cycle performance and high temperature performance of the battery. Summary of the invention
[0005] In view of the above-mentioned defects, the present invention provides a positive electrode active material, which can effectively improve the cycle performance and high temperature performance of the battery.
[0006] The present invention provides a positive electrode sheet. Since the positive electrode sheet comprises the positive electrode active material, the high temperature performance and cycle performance of the battery can be effectively improved by using the positive electrode sheet in the battery.
[0007] The present invention provides a secondary battery. Since the secondary battery comprises the positive electrode active material or the positive electrode sheet, the secondary battery has good high temperature performance and cycle performance.
[0008] The present invention provides a positive electrode active material, which comprises a core and a coating layer coated on at least a part of the surface of the core; the core comprises a positive electrode material with active ions, and the coating layer comprises polysilicon titanoxane and a carbon material.
[0009] Furthermore, the absorption amount of the positive electrode active material when placed at a dew point of -10°C for 72 hours is less than 500 ppm.
[0010] Furthermore, the median particle size Dv50 of the positive electrode active material is 0.5 μm to 5 μm.
[0011] Furthermore, the specific surface area of the positive electrode active material is 3m 2 / g~10m 2 / g.
[0012] Furthermore, the mass ratio of the coating layer to the core is (1-4): (96-99);
[0013] And / or, the mass ratio of the polysilicon titanoxane to the carbon material is (6-50):(50-94).
[0014] Further, the carbon material includes at least one of acetylene black, Super P, carbon nanotubes, Ketjen black, and graphene;
[0015] Preferably, the carbon material is carbon nanotube and Super P.
[0016] Furthermore, the diameter of the carbon nanotube is 10nm-25nm, and the particle size of the Super P is 20nm-40nm.
[0017] Furthermore, the positive electrode material having active ions is a Prussian blue positive electrode material;
[0018] The Prussian blue positive electrode material comprises a chemical composition as shown in Formula 1,
[0019] Na m K n (M x Mn 1-x )[Fe(CN)6] y Formula 1
[0020] In Formula 1, 1.5≤m<2, 0≤n≤0.05, 0.1≤x≤0.8, 0.8≤y<1, and M includes at least one of Fe, Mn, Cu, Ni, and Co.
[0021] The present invention provides a positive electrode sheet, which comprises any one of the positive electrode active materials described above.
[0022] The present invention provides a secondary battery, which comprises any one of the above-mentioned positive electrode active materials or the above-mentioned positive electrode sheet.
[0023] The invention effectively improves the high temperature performance and cycle performance of the battery by arranging a coating layer on at least part of the surface of the positive electrode material having active ions, and making the coating layer include polysilicon titanoxane and carbon material. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The first aspect of the present invention provides a positive electrode active material, which includes a core and a coating layer coated on at least a portion of the surface of the core; the core includes a positive electrode material having active ions, and the coating layer includes polysilicon titanoxane and a carbon material.
[0026] The positive electrode material with active ions in the present invention refers to a material that can provide active ions (Li + 、Na + , K + ) Materials that are embedded or embedded in place.
[0027] The present invention does not specifically limit the weight average molecular weight of polysilicon titanoxane.
[0028] The present invention does not specifically limit the mass ratio of polysilicon titanoxane to carbon material and the mass ratio of coating layer to core.
[0029] The present invention does not specifically limit the types of the positive electrode material and the carbon material having active ions.
[0030] The present invention does not specifically limit the sources of the positive electrode material and the carbon material having active ions, and commercially available products or products prepared by conventional preparation methods well known to those skilled in the art may be used.
[0031] The present invention can significantly improve the cycle performance and high temperature performance of the battery by providing a coating layer on at least part of the surface of the positive electrode material having active ions, and making the coating layer include polysilicon titanoxane and carbon material. Based on this phenomenon, the inventor analyzed the positive electrode active material and believed that the reason may be: when the coating layer includes polysilicon titanoxane and carbon material, polysilicon titanoxane and carbon material cooperate with each other. On the one hand, polysilicon titanoxane can produce complexation with transition metal ions during the charge and discharge process, inhibit the dissolution of transition metals, and effectively alleviate lattice distortion; it can also undergo nucleophilic substitution reaction with HF in the electrolyte, effectively eliminate HF in the electrolyte, and reduce the interface side reaction between the positive electrode and the electrolyte; and polysilicon titanoxane has Si-O-Ti bonds, Si-O-Si bonds and Ti -O-Ti bond connected structure, forming a cross-linked skeleton, in which Si-O-Ti bond can slow down the volume strain of the positive electrode active material during the charge and discharge process, ensuring the stability of the interface film; on the other hand, because the coating layer including polysilicon titanium oxane and carbon material has good wettability to the electrolyte, and the Si-O-Si and Ti-O-Ti bonds in polysilicon titanium oxane have a lower active ion diffusion barrier, it can effectively improve the diffusion rate of active ions at the interface between the electrolyte and the positive electrode active material; at the same time, the carbon material can effectively improve the electronic conductivity of the positive electrode active material. This can comprehensively improve the cycle performance and high temperature performance of the positive electrode active material, and also improve the rate performance of the positive electrode active material.
[0032] In addition, since the coating layer including polysilicon titanium oxane and carbon material can reduce the contact area between the positive electrode material with active ions and the electrolyte, the dissolution rate of transition metal ions can be greatly reduced, thereby effectively improving the high-temperature storage and cycle performance of the positive electrode active material.
[0033] The present invention does not specifically limit the preparation method of the positive electrode active material. For example, the positive electrode active material can be prepared by the following steps:
[0034] 1) adding raw materials including a positive electrode material having active ions and a carbon material into deionized water, and uniformly dispersing by ultrasonication. During this process, the carbon material is adsorbed on the surface of the positive electrode material having active ions by weak adsorption, and a first product is obtained after filtering and drying;
[0035] 2) dispersing the first product into an ethanol aqueous solution with an ethanol mass concentration of 98% to 99.5% to obtain a mixed solution; controlling the temperature within the range of 5°C to 30°C, slowly dropping tetraethyl orthosilicate and butyl orthotitanate into the mixed solution, and after the dropping is completed, reacting for 1h to 6h, during which tetraethyl orthosilicate and butyl orthotitanate are hydrolyzed and condensed to form polysilicon titanate, filtering and drying, and then treating in an inert atmosphere at 150°C to 350°C for 2h to 24h to obtain a positive electrode active material.
[0036] In a specific embodiment, the weight average molecular weight of polysilicon titanoxane is 400 to 4000. For example, the weight average molecular weight is 400, 1000, 1600, 2200, 2800, 3400 or 4000. For example, the hydrolysis rate of ethyl orthosilicate and butyl orthotitanate can be further controlled by controlling the mass concentration of ethanol, the dripping rate of ethyl orthosilicate and butyl orthotitanate in the above preparation method, thereby controlling the weight average molecular weight of polysilicon titanoxane to be within the above range. Within this range, the water resistance of the positive electrode active material can be improved, and at the same time, a high electronic conductivity can be ensured.
[0037] In a specific embodiment, the absorption amount of the positive electrode active material is less than 500 ppm when placed at a dew point of -10°C for 72 hours. Within this range, the positive electrode active material has high air stability and is not easy to absorb moisture in the air, which can effectively improve the high temperature performance and cycle performance of the battery.
[0038] The absorption amount of the positive electrode active material at a dew point of -10°C can be obtained by testing using the following method:
[0039] The positive electrode active material is spread flat on the surface of the substrate and placed in an environment with a temperature of 25±1°C, a relative humidity of 8±1%, and a dew point temperature of -10°C for 72 hours. The water content of the positive electrode active material before and after placement is tested using a Karl Fischer titrator. The instrument test cutoff temperature is 200°C, and the absorption amount is the difference between the water content of the positive electrode active material before placement and the water content of the positive electrode active material after placement.
[0040] In a specific embodiment, the thickness of the coating layer is 2nm to 10nm. For example, the thickness of the coating layer is 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm or 10nm. Within this range, the thickness of the coating layer is moderate, which can further improve the electronic conductivity and hydrophobicity of the positive electrode active material particles, thereby effectively improving the diffusion rate of active ions and the transmission rate of electrons, so that the battery has higher rate performance and cycle performance.
[0041] In a specific embodiment, the median particle size Dv50 of the positive electrode active material is 0.5 μm to 5 μm. For example, the median particle size Dv50 of the positive electrode active material is 0.5 μm, 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, 4.5 μm or 5.0 μm. Wherein, Dv50 represents the particle size of 50% volume accumulation. Within this range, the positive electrode active material can have a higher strength, making it less likely to crack during the cycle process, thereby improving the cycle performance of the battery; at the same time, the dispersibility of the positive electrode active material particles in the slurry can be improved.
[0042] Specifically, the median particle size Dv50 of the positive electrode active material can be further adjusted to be between 0.5 μm and 5 μm by adjusting the median particle size Dv50 of the positive electrode material having active ions.
[0043] In one embodiment, the specific surface area of the positive electrode active material is 3 m 2 / g~10m 2 / g. For example, the specific surface area of the positive electrode active material is 3m 2 / g, 4m 2 / g, 5m 2 / g, 6m 2 / g, 7m 2 / g, 8m 2 / g, 9m 2 / g or 10m 2 / g. Within this range, a higher compaction density can be achieved, and it is not easy to crack during the cycle process. While improving the cycle stability of the battery, it can also increase the energy density of the battery.
[0044] Specifically, the specific surface area of the positive electrode material with active ions can be further adjusted to be within 3 m 2 / g~10m 2 / g.
[0045] In a specific embodiment, the mass ratio of the coating layer to the core is (1-4): (96-99). For example, the mass ratio of the coating layer to the core is 1:99, 1.5:98.5, 2:98, 2.5:97.5, 3:97, 3.5:96.5 or 4:96. Within this range, not only can the positive electrode active material have higher cycle performance and high temperature performance, but also the energy density of the positive electrode active material can be improved.
[0046] Specifically, the mass ratio of the coating layer to the core in the present invention can be obtained by testing using the following method:
[0047] First, the chemical composition of the core and the absolute mass content (ppm) of the metal elements in the core material are obtained by ICP-OES testing. Then, the mass content of the core in the positive electrode active material is derived and calculated based on the absolute mass content, thereby calculating the mass ratio of the coating layer to the core material.
[0048] In a specific embodiment, the mass ratio of polysilicon titanoxane to carbon material is (6-50):(50-94). For example, the mass ratio of polysilicon titanoxane to carbon material is 6:94, 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, 45:55 or 50:50. Within this range, polysilicon titanoxane and carbon material can better cooperate to further improve the cycle performance and high temperature performance of the battery.
[0049] Specifically, the mass ratio of polysilicon titanoxane to carbon material in the present invention can be obtained by testing using the following method:
[0050] When the core does not include carbon element, the carbon mass content in the positive electrode active material is first measured by an element analyzer, and then the mass ratio of the coating layer to the core is tested by the above method to obtain the mass of the coating layer, thereby obtaining the mass ratio of polysilicon titanium oxane to the carbon material.
[0051] When the core includes carbon elements, the chemical composition of the core is first obtained by ICP-OES testing, and then the mass proportion of carbon elements in the core is obtained; the total carbon mass content in the positive electrode active material is measured by an elemental analyzer, and the carbon mass content in the coating layer is the difference between the total carbon mass content and the carbon mass content in the core, and then the mass content of polysilicon titanoxane in the coating layer is calculated, thereby obtaining the mass ratio of polysilicon titanoxane to carbon material.
[0052] In a specific embodiment, the carbon material includes at least one of acetylene black, Super P, carbon nanotubes, Ketjen black, and graphene. When the carbon material includes two or more of these materials, the present invention does not specifically limit the ratio between the materials.
[0053] Preferably, the carbon material is carbon nanotube and Super P. Carbon nanotube has a high aspect ratio and is easy to entangle on the particle surface, thus improving the coating effect of the carbon material. Super P can fill in the pores formed by the winding of carbon nanotube, enhance the point-to-point contact, and form a continuous conductive network of point-line contact, which can greatly enhance the conductivity of the positive electrode active material particles, thereby further improving the battery rate performance and increasing the battery capacity.
[0054] In a specific embodiment, the diameter of the carbon nanotube is 10nm to 25nm, and the particle size of Super P is 20nm to 40nm. For example, the diameter of the carbon nanotube is 10nm, 12nm, 14nm, 16nm, 18nm, 20nm, 22nm or 25nm; the particle size of Super P is 20nm, 23nm, 26nm, 29nm, 32nm, 35nm, 38nm or 40nm. Within this range, the carbon nanotube and Super P particles can better cooperate, further improve the conductivity of the positive electrode active material, and enable the battery to have a higher rate performance.
[0055] In a specific embodiment, the positive electrode material having active ions is a Prussian blue positive electrode material; the Prussian blue positive electrode material includes a chemical composition shown in Formula 1,
[0056] Na m K n (M x Mn 1-x )[Fe(CN)6] y Formula 1
[0057] In Formula 1, 1.5≤m<2, 0≤n≤0.05, 0.1≤x≤0.8, 0.8≤y<1, and M includes at least one of Fe, Mn, Cu, Ni, and Co. Among them, K + The doping of Na + The transmission channel can improve the rate performance of the positive electrode active material; the doping of transition metal M can inhibit the Jan-Taylor effect of manganese ions in the charge and discharge process, effectively improve the structural stability of the material, thereby greatly improving the cycle stability of the positive electrode active material; and because the coating layer has good hydrophobicity and electronic conductivity, it can greatly reduce the water absorption rate of Prussian blue positive electrode materials and improve their air stability, thereby ensuring a higher gram capacity Under the premise of improving its high temperature performance, rate performance and cycle stability.
[0058] The present invention does not specifically limit the preparation method of the Prussian blue positive electrode material. For example, it can be prepared by the following steps:
[0059] Na4Fe(CN)6·10H2O and a potassium source are dissolved in deionized water to form a first solution, a transition metal M source, a manganese source and a complexing agent are dissolved in deionized water to form a second solution, the second solution is added dropwise into the first solution to perform a coprecipitation reaction, and after aging, the precipitate is washed, filtered and dried to obtain a Prussian blue cathode material.
[0060] The potassium source in the present invention refers to a raw material that provides potassium element, the M source refers to a raw material that provides M element (Fe, Mn, Cu, Ni, Co), and the manganese source refers to a raw material that provides manganese element. As long as it contains the target element (K, Fe, Mn, Cu, Ni, Co), it falls within the definition of the present invention.
[0061] The present invention does not specifically limit the molar ratio of the Prussian blue cathode material precursor, the potassium source, the M source, and the manganese source. It is only necessary that the chemical formula of the prepared Prussian blue cathode material satisfies Formula 1.
[0062] The second aspect of the present invention provides a positive electrode sheet, which includes the positive electrode active material of the first aspect. Since the positive electrode active material has a special structure and composition, it can not only effectively alleviate lattice distortion, but also reduce the interface side reaction between the positive electrode and the electrolyte, and improve the stability of the interface film; at the same time, it can also improve the diffusion rate of active ions and the transmission rate of electrons. Therefore, the positive electrode sheet including the positive electrode active material can effectively improve the high temperature performance, cycle performance and rate performance of the battery.
[0063] A third aspect of the present invention provides a secondary battery. Since the secondary battery includes the positive electrode active material of the first aspect or the positive electrode sheet of the second aspect, the secondary battery has high cycle performance and high temperature performance.
[0064] Hereinafter, a secondary battery including the positive electrode active material of the present invention will be described in detail through specific examples.
[0065] Example 1
[0066] 1) Prussian blue positive electrode material Na with a mass ratio of 40.42:1 1.82 K 0.04 Fe 0.3 Mn 0.7 (Fe(CN)6) 0.95 and carbon materials (including carbon nanotubes and Super P in a mass ratio of 1:2, the diameter of the carbon nanotubes is 17nm, and the particle size of Super P is 30nm) are added to deionized water and dispersed uniformly by ultrasonication. Among them, the median particle size Dv50 of the Prussian blue positive electrode material is 0.8μm, and the specific surface area is 6m 2 / g; in this process, the carbon material is adsorbed on the surface of the positive electrode material having active ions through weak adsorption, and the first product is obtained after filtering and drying;
[0067] 2) dispersing the first product into an ethanol aqueous solution with a mass concentration of 99% to obtain a mixed solution with a solid content of 10; controlling the temperature within the range of 25°C, slowly adding tetraethyl orthosilicate and butyl orthotitanate to the mixed solution, and reacting for 4 hours after the addition is completed. During this process, tetraethyl orthosilicate and butyl orthotitanate (the mass ratio of tetraethyl orthosilicate to butyl orthotitanate is 1:1, and the mass ratio of tetraethyl orthosilicate and butyl orthotitanate to carbon material is 2:1) are hydrolyzed and condensed to form polysilicon titanate, which is filtered and dried, and then treated at 250°C in an inert atmosphere for 8 hours to obtain the positive electrode active material of this embodiment.
[0068] Example 2
[0069] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that in step 1), the mass ratio of the Prussian blue positive electrode material to the carbon material is adjusted to 102.92:1.
[0070] Example 3
[0071] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that in step 1), the mass ratio of the Prussian blue positive electrode material to the carbon material is adjusted to 30:1.
[0072] Example 4
[0073] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that, in step 1), the mass ratio of the Prussian blue positive electrode material to the carbon material is adjusted to 38.8:1;
[0074] In step 2), the mass ratio of the total mass of tetraethyl orthosilicate and tetrabutyl orthotitanate to the mass ratio of the carbon material is adjusted to 1.7:1.
[0075] Example 5
[0076] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that, in step 1), the mass ratio of the Prussian blue positive electrode material to the carbon material is adjusted to 43.11:1;
[0077] In step 2), the mass ratio of the total mass of tetraethyl orthosilicate and tetrabutyl orthotitanate to the mass ratio of the carbon material is adjusted to 1.5:1.
[0078] Example 6
[0079] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that, in step 1), the mass ratio of the Prussian blue positive electrode material to the carbon material is adjusted to 34.49:1;
[0080] In step 2), the mass ratio of the total mass of tetraethyl orthosilicate and tetrabutyl orthotitanate to the mass ratio of the carbon material is adjusted to 0.5:1.
[0081] Example 7
[0082] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that, in step 1), the mass ratio of the Prussian blue positive electrode material to the carbon material is adjusted to 64.67:1;
[0083] In step 2), the mass ratio of the total mass of tetraethyl orthosilicate and tetrabutyl orthotitanate to the mass ratio of the carbon material is adjusted to 3:1.
[0084] Example 8
[0085] The preparation method of the positive electrode active material in this embodiment is basically the same as that in embodiment 1, except that in step 1), the median particle size Dv50 of the Prussian blue positive electrode material is adjusted to 1 μm, and the specific surface area is adjusted to 5 m 2 / g.
[0086] Example 9
[0087] The preparation method of the positive electrode active material in this embodiment is basically the same as that in embodiment 1, except that in step 1), the median particle size Dv50 of the Prussian blue positive electrode material is adjusted to 0.5 μm, and the specific surface area is adjusted to 10 m 2 / g.
[0088] Example 10
[0089] The preparation method of the positive electrode active material in this embodiment is basically the same as that in embodiment 1, except that in step 1), the median particle size Dv50 of the Prussian blue positive electrode material is adjusted to 3 μm, and the specific surface area is adjusted to 4 m 2 / g.
[0090] Embodiment 11
[0091] The preparation method of the positive electrode active material in this embodiment is basically the same as that in embodiment 1, except that in step 1), the median particle size Dv50 of the Prussian blue positive electrode material is adjusted to 5 μm, and the specific surface area is adjusted to 3 m 2 / g.
[0092] Example 12
[0093] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that in step 1), the diameter of the carbon nanotube is adjusted to 10 nm, and the particle size of Super P is adjusted to 20 nm.
[0094] Embodiment 13
[0095] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that in step 1), the diameter of the carbon nanotubes is adjusted to 25 nm, and the particle size of Super P is adjusted to 40 nm.
[0096] Embodiment 14
[0097] The preparation method of the positive electrode active material in this embodiment is basically the same as that in embodiment 1, except that in step 1), the Prussian blue positive electrode material is replaced by a positive electrode material having a chemical composition of Na 1.82 K 0.04 Fe 0.3 Mn 0.6 Cu 0.1 (Fe(CN)6) 0.95 The positive electrode material has a median particle size Dv50 of 1 μm and a specific surface area of 6 m 2 / g.
[0098] Embodiment 15
[0099] The preparation method of the positive electrode active material in this embodiment is basically the same as that in embodiment 1, except that in step 1), the Prussian blue positive electrode material is replaced by a positive electrode material having a chemical composition of Na 1.82 K 0.04 Fe 0.3 Mn 0.5 Cu 0.1 Co 0.1 (Fe(CN)6) 0.95 The positive electrode material has a median particle size Dv50 of 0.9 μm and a specific surface area of 6 m 2 / g.
[0100] Example 16
[0101] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that in step 1), the mass ratio of the Prussian blue positive electrode material to the carbon material is adjusted to 23.75:1.
[0102] Embodiment 17
[0103] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that in step 1), the mass ratio of the Prussian blue positive electrode material to the carbon material is adjusted to 123.75:1.
[0104] Embodiment 18
[0105] The preparation method of the positive electrode active material in this embodiment is basically the same as that in embodiment 1, except that in step 1), the median particle size Dv50 of the Prussian blue positive electrode material is adjusted to 0.3 μm, and the specific surface area is adjusted to 12 m 2 / g.
[0106] Embodiment 19
[0107] The method for preparing the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that in step 1), the carbon material used is only carbon nanotubes.
[0108] Embodiment 20
[0109] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that in step 1), only Super P is used as the carbon material.
[0110] Embodiment 21
[0111] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that in step 1), the diameter of the carbon nanotube is adjusted to 8 nm, and the particle size of Super P is adjusted to 45 nm.
[0112] Embodiment 22
[0113] The preparation method of the positive electrode active material in this embodiment is basically the same as that in Embodiment 1, except that, in step 1), the mass ratio of the Prussian blue positive electrode material to the carbon material is adjusted to 80.83:1;
[0114] In step 2), the mass ratio of the total mass of tetraethyl orthosilicate and tetrabutyl orthotitanate to the mass ratio of the carbon material is adjusted to 4:1.
[0115] Embodiment 23
[0116] The preparation method of the positive electrode active material in this embodiment is basically the same as that in embodiment 1, except that in step 1), a positive electrode active material having a chemical composition of Na 0.95 Fe 0.33 Ni 0.33 Mn 0.34 The sodium ion transition metal oxide of O2 replaces the Prussian blue positive electrode material. The median particle size Dv50 of the sodium ion transition metal oxide is 6 μm and the specific surface area is 0.8 m 2 / g.
[0117] Embodiment 24
[0118] The preparation method of the positive electrode active material in this embodiment is basically the same as that in embodiment 1, except that in step 1), a positive electrode active material having a chemical composition of Na 2.26 Fe 1.87 The polyanion-shaped compound of (SO4)3 replaces the Prussian blue positive electrode material. The median particle size Dv50 of the polyanion-shaped compound is 3 μm and the specific surface area is 8 m 2 / g.
[0119] Embodiment 25
[0120] The preparation method of the positive electrode active material in this embodiment is basically the same as that in embodiment 1, except that in step 1), a LiNi 0.8 Co 0.1 The nickel cobalt manganese oxide of Mn0.1O2 replaces the Prussian blue positive electrode material. The median particle size Dv50 of the nickel cobalt manganese oxide is 8μm and the specific surface area is 0.5m 2 / g.
[0121] Comparative Example 1
[0122] The positive electrode active material in this comparative example adopts a chemical composition of Na 1.82 K 0.04 Fe 0.3 Mn 0.7 (Fe(CN)6) 0.95 Prussian blue positive electrode material without any coating treatment.
[0123] Comparative Example 2
[0124] The preparation method of the positive electrode active material in this comparative example is basically the same as that in Example 1, except that only the Prussian blue positive electrode material Na 1.82 K 0.04 Fe 0.3 Mn 0.7 (Fe(CN)6) 0.95 Carbon material coating is performed without coating polysilicon titanoxane. The specific steps are as follows:
[0125] The mass ratio of Prussian blue positive electrode material Na 1.82 K 0.04 Fe 0.3 Mn 0.7 (Fe(CN)6) 0.95 and carbon materials (including carbon nanotubes and Super P in a mass ratio of 1:2, the diameter of the carbon nanotubes is 17nm, and the particle size of Super P is 30nm) are added to deionized water and dispersed uniformly by ultrasonication. Among them, the median particle size Dv50 of the Prussian blue positive electrode material is 0.8μm, and the specific surface area is 6m 2 / g; in this process, the carbon material is adsorbed on the surface of the positive electrode material having active ions through weak adsorption, and after filtering and drying, it is treated at 250°C for 8h in an inert atmosphere to obtain the positive electrode active material of this comparative example.
[0126] Comparative Example 3
[0127] The preparation method of the positive electrode active material in this comparative example is basically the same as that in Example 1, except that only the Prussian blue positive electrode material Na 1.82 K0.04 Fe 0.3 Mn 0.7 (Fe(CN)6) 0.95 Polysilicon titanoxane coating is performed without coating carbon material. The specific steps are as follows:
[0128] Prussian blue cathode material Na 1.82 K 0.04 Fe 0.3 Mn 0.7 (Fe(CN)6) 0.95 The obtained mixture was dispersed in an ethanol aqueous solution with a mass concentration of 99% to obtain a mixed solution with a solid content of 10; the temperature was controlled within the range of 25°C, and tetraethyl orthosilicate and butyl orthotitanate were slowly added dropwise to the mixed solution. After the addition was completed, the mixture was reacted for 4 hours. During the reaction, tetraethyl orthosilicate and butyl orthotitanate (the mass ratio of tetraethyl orthosilicate to butyl orthotitanate was 1:1, and the mass ratio of the total mass of tetraethyl orthosilicate and butyl orthotitanate to the mass of the carbon material was 2:1) were hydrolyzed and condensed to form polysilicon titanate. The polysilicon titanate was filtered and dried, and then treated at 250°C in an inert atmosphere for 8 hours to obtain the positive electrode active material of this comparative example.
[0129] Test example
[0130] 1. The mass ratio of polysilicon titanoxane to carbon material, the mass ratio of coating layer to core in the positive electrode active materials prepared in the above embodiments and comparative examples, and the absorption amount, median particle size Dv50 and specific surface area of the positive electrode active materials placed at a dew point of -10°C for 72 hours were tested. The test results are shown in Table 1.
[0131] 1) Water absorption capacity test of samples
[0132] The positive electrode active material is spread flat on the surface of the substrate and placed in an environment with a temperature of 25±1°C, a relative humidity of 8±1%, and a dew point temperature of -10°C for 72 hours. The water content of the positive electrode active material before and after placement is tested using a Karl Fischer titrator. The instrument test cutoff temperature is 200°C, and the absorption amount is the difference between the water content of the positive electrode active material before placement and the water content of the positive electrode active material after placement.
[0133] 2) Particle size test of positive electrode active materials
[0134] Malvern MasterSizer 3000 laser particle size analyzer was used, and the test method was based on GB / T19077-2016 / ISO 13320:2009.
[0135] 3) Specific surface area test of positive electrode active material
[0136] The specific surface area of the positive electrode active material refers to GB / T 19587-2017 "Gas Adsorption BET Method for Testing the Specific Surface Area of Solid Materials" and is tested using a specific surface area tester (such as TriStarⅡ3020).
[0137] 4) Test of the mass ratio of the coating layer to the core
[0138] First, the chemical composition of the core and the absolute mass content (ppm) of the metal elements in the core material are obtained by ICP-OES testing. Then, the mass content of the core in the positive electrode active material is derived and calculated based on the absolute mass content, thereby calculating the mass ratio of the coating layer to the core material.
[0139] 5) Test on the mass ratio of polysilicon titanoxane to carbon material
[0140] When the core does not include carbon element, the carbon mass content in the positive electrode active material is first measured by an element analyzer, and then the mass ratio of the coating layer to the core is tested by the above method to obtain the mass of the coating layer, thereby obtaining the mass ratio of polysilicon titanium oxane to the carbon material.
[0141] When the core includes carbon elements, the chemical composition of the core is first obtained by ICP-OES testing, and then the mass proportion of carbon elements in the core is obtained; the total carbon mass content in the positive electrode active material is measured by an elemental analyzer, and the carbon mass content in the coating layer is the difference between the total carbon mass content and the carbon mass content in the core, and then the mass content of polysilicon titanoxane in the coating layer is calculated, thereby obtaining the mass ratio of polysilicon titanoxane to carbon material.
[0142] The test results are shown in Table 1.
[0143] Table 1
[0144]
[0145]
[0146] 2. The positive electrode active materials prepared in the above-mentioned Examples 1-22 and Comparative Examples 1-3 are made into sodium ion batteries, and the production steps include:
[0147] (1) Preparation of positive electrode sheet: 93 wt % of the above positive electrode active material was mixed with 2.5 wt % of Super P, 1 wt % of carbon nanotubes, 3.5 wt % of binder polyvinylidene fluoride and N-methylpyrrolidone to obtain a positive electrode active layer slurry with a solid content of 45%. The positive electrode active layer slurry was coated on both sides of the functional surface of a 12 μm carbon-coated aluminum foil, and the coating surface density was 9.12 mg / cm 2 After drying at 100°C, the compacted density was 1.5 g / cm3 Positive electrode;
[0148] (2) Preparation of negative electrode sheet: 93 wt% of negative electrode active material hard carbon, 4.8 wt% of conductive agent (4 wt% of conductive carbon black and 0.8 wt% of carbon nanotubes) and 2.2 wt% of binder polyvinylidene fluoride and N-methylpyrrolidone were mixed to obtain negative electrode active layer slurry, which was coated on both sides of the functional surface of the negative electrode current collector 12 μm corona aluminum foil, with a coating surface density of 5.3 mg / cm 2 After drying at 100°C, the compacted density was 0.95 g / cm 3 The negative electrode;
[0149] (3) Battery assembly: The positive electrode sheet, the negative electrode sheet and the PP / ceramic coated separator are stacked to form an electrode group, which is then encapsulated and dried after being filled with an aluminum-plastic film. An electrolyte (1 M NaPF6 / organic solvent (propylene carbonate and ethyl methyl carbonate in a volume ratio of 4:6)) is injected to obtain a sodium ion battery after formation.
[0150] The sodium ion battery prepared above was tested for room temperature cycle performance, high temperature cycle performance, high temperature storage performance, initial DC internal resistance, and transition metal dissolution:
[0151] Room temperature cycle performance: At 25°C, the secondary battery is charged to 3.8V at a constant current of 1C, and then charged at a constant voltage until the current reaches 0.05C. At this time, the secondary battery is fully charged, and the charging capacity at this time is recorded as the charging capacity of the first cycle; after the secondary battery is allowed to stand for 5 minutes, it is discharged to 1.5V at a constant current of 1C. This is a cyclic charge and discharge process, and the discharge capacity at this time is recorded as the discharge capacity of the first cycle C0; the secondary battery is subjected to a cyclic charge and discharge test according to the above process, and the discharge capacity after 600 cycles is recorded as C1. The 600-cycle capacity retention rate is the ratio of C1 to C0. The test results are shown in Table 2.
[0152] High temperature cycle performance: at 45°C, the secondary battery is charged to 3.8V at a constant current of 1C, and then charged at a constant voltage until the current reaches 0.05C. At this time, the secondary battery is fully charged, and the charging capacity at this time is recorded as the charging capacity of the first cycle; after the secondary battery is allowed to stand for 5 minutes, it is discharged to 2.0V at a constant current of 1C. This is a cyclic charge and discharge process, and the discharge capacity at this time is recorded as the discharge capacity of the first cycle C2; the secondary battery is subjected to a cyclic charge and discharge test according to the above process, and the discharge capacity after 600 cycles is recorded as C3. The 600-cycle capacity retention rate is the ratio of C3 to C2. The test results are shown in Table 2.
[0153] High temperature storage performance: Step 1: Under (25±2)℃ environment, discharge the secondary battery at 1C standard constant current to a discharge termination voltage of 1.5V, and leave it for 30min; then charge it to 3.8V at 1C standard constant current and constant voltage, with a cut-off current of 0.05C, and leave it for 30min; discharge it to 1.5V at 1C standard constant current, and obtain the initial capacity C4 of the battery cell; leave it for 30min; measure the DC internal resistance (DCIR) at 50% SOC at (25±2)℃, the test method is to discharge the battery at a rate of 10C for 10S, with every 100ms as the sampling interval point;
[0154] Step 2: Charge to 3.8V with constant current and constant voltage according to the 1C standard charging method, cut off the constant voltage and current at 0.05C, and then leave it in an open circuit at 60℃;
[0155] Step 3: Take out every 7 days, let it stand for 2 hours at (25±2)℃, measure the internal resistance, thickness, remaining capacity, and recovery capacity; adjust to 50% SOC, let it stand for 2 hours, and measure the DC internal resistance (DCIR) at 50% SOC at (25±2)℃. The test method is that the battery is discharged at a rate of 10C for 10S, and every 100ms is the sampling interval point;
[0156] Step 4: Then fully charge the battery at 1C rate to 100% SOC, continue to store, cycle the third and fourth steps until 2 months, and measure the final recovery capacity as C4'; the high temperature recovery performance is C4' / C4;
[0157] Test requirements: All the above tests of capacity, internal resistance, thickness, DCIR, and SOC adjustment are carried out in a (25±2)℃ constant temperature room; when adjusting SOC, adjust it according to the actual recovery capacity under the current state.
[0158] The test results are shown in Table 2.
[0159] Initial DC internal resistance test: At 25°C, charge the secondary battery to 3.8V at 1C constant current, and continue to charge at constant voltage until the current is 0.05C, at which time the secondary battery is fully charged; discharge the secondary battery at 0.5C constant current and adjust the secondary battery to 50% SOC, at which time the voltage of the secondary battery is recorded as U1; discharge the secondary battery at 10C constant current I1 for 10 seconds, use 0.1 second sampling, and the voltage at the end of discharge is recorded as U2. The discharge DC internal resistance of the secondary battery at 50% SOC represents the initial DC internal resistance of the secondary battery, then the initial DC internal resistance of the secondary battery (mΩ) = (U1-U2) / I1, the test results are shown in Table 2.
[0160] Rate performance: At 25°C, the secondary battery is charged to 3.8V at a constant current of 0.5C, and then charged at a constant voltage to a current of 0.05C. At this time, the secondary battery is fully charged; after the secondary battery is allowed to stand for 5 minutes, it is discharged to 1.5V at a constant current of 1C, and the discharge capacity C5 at this time is recorded; the secondary battery is charged to 3.8V at a constant current of 0.5C again, and then charged at a constant voltage to a current of 0.05C. After the secondary battery is allowed to stand for 5 minutes, it is discharged to 1.5V at a constant current of 10C, and the discharge capacity C6 at this time is recorded. The rate performance of the battery is represented by the ratio of C6 to C5. The calculation results are shown in Table 2.
[0161] The test results are shown in Table 2.
[0162] Transition metal dissolution: The full battery with a capacity decay of 80% in the above high temperature cycle test was discharged at a rate of 0.1C to a cut-off voltage of 1.5V. The battery was then disassembled, the negative electrode sheet was taken out, and 30 unit areas (25mm 2 ) was tested by Agilent ICP-OES730 inductively coupled plasma emission spectroscopy (ICP) to obtain the amount of Mn therein, thereby obtaining the amount of Mn dissolved after the cycle. The test standard is based on EPA-6010D-2014, and the test results are shown in Table 2.
[0163] 3. The contact angle and powder resistivity of the positive electrode active materials prepared in the above examples and comparative examples were tested:
[0164] 1) Contact angle test
[0165] The measurement was carried out with reference to GBT 30693-2014. At room temperature, a drop of propylene carbonate solvent was dropped on the surface of the above-mentioned positive electrode sheet. The contact angle of the drop was measured at 60 seconds by a contact angle meter. The test instrument can be an optical contact angle meter. The test results are shown in Table 2.
[0166] 2) Powder resistivity test
[0167] The powder resistivity of the positive electrode active material was tested using the four-probe mode of PRCD3100 (IEST-Yuan Neng Technology). The applied pressure was 20 MPa and the pressure was maintained for 10 seconds. The test results are shown in Table 2.
[0168] Table 2
[0169]
[0170]
[0171] From Table 1 and Table 2, we can see that:
[0172] The water absorption of the positive electrode active materials in Examples 1 to 22 is maintained at a low level, and compared with the positive electrode active materials in Comparative Examples 1 to 3, they have lower powder resistivity, higher room temperature cycle capacity retention rate, high temperature cycle capacity retention rate, high temperature recovery performance and rate performance, as well as lower initial DC internal resistance and Mn dissolution amount; wherein, the contact angle of Example 13 is 20°, and the powder resistivity is 1.2×10 4 Ω·cm, the normal temperature cycle capacity retention rate is 93%, the high temperature cycle capacity retention rate is 88%, the high temperature recovery performance is 87%, the initial DC internal resistance is 17mΩ, the rate performance is 94%, and the Mn dissolution amount is 30ppm; while the powder resistivity in the comparative example is as low as 2.1×10 4 Ω·cm, correspondingly, the normal temperature cycle capacity retention rate is 81%, the high temperature cycle capacity retention rate is 79%, the high temperature recovery performance is 77%, the initial DC internal resistance is 29mΩ, the rate performance is 80%, and the Mn dissolution amount is 234ppm. It can be seen that the positive electrode active material in the present invention has high air stability, as well as good high temperature storage performance and cycle performance, and the dissolution of the transition metal ion Mn is also significantly suppressed.
[0173] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A positive electrode active material, It is characterized in that The positive electrode active material comprises a core and a coating layer coated on at least a part of the surface of the core; the core comprises a positive electrode material having active ions, and the coating layer comprises polysilicon titanoxane and a carbon material.
2. The positive electrode active material according to claim 1, It is characterized in that The absorption amount of the positive electrode active material when placed at a dew point of -10°C for 72 hours is less than 500 ppm.
3. The positive electrode active material according to claim 1 or 2, It is characterized in that The median particle size Dv50 of the positive electrode active material is 0.5 μm to 5 μm.
4. The positive electrode active material according to any one of claims 1 to 3, It is characterized in that The specific surface area of the positive electrode active material is 3 m 2 / g~10m 2 / g.
5. The positive electrode active material according to any one of claims 1 to 4, It is characterized in that The mass ratio of the coating layer to the core is (1-4):(96-99); And / or, the mass ratio of the polysilicon titanoxane to the carbon material is (6-50):(50-94).
6. The positive electrode active material according to any one of claims 1 to 5, It is characterized in that The carbon material includes at least one of acetylene black, Super P, carbon nanotubes, Ketjen black, and graphene; Preferably, the carbon material is carbon nanotube and Super P.
7. The positive electrode active material according to claim 6, It is characterized in that The diameter of the carbon nanotube is 10nm-25nm, and the particle size of the Super P is 20nm-40nm.
8. The positive electrode active material according to any one of claims 1 to 7, It is characterized in that The positive electrode material having active ions is a Prussian blue positive electrode material; The Prussian blue positive electrode material comprises a chemical composition as shown in Formula 1, Na m K n (M x Mn 1-x )[Fe(CN) 6 y Formula 1 In Formula 1, 1.5≤m<2, 0≤n≤0.05, 0.1≤x≤0.8, 0.8≤y<1, and M includes at least one of Fe, Mn, Cu, Ni, and Co.
9. A positive electrode sheet, It is characterized in that The positive electrode sheet comprises the positive electrode active material according to any one of claims 1 to 8.
10. A secondary battery, It is characterized in that The secondary battery comprises the positive electrode active material according to any one of claims 1 to 8, or the positive electrode sheet according to claim 9.