Ternary positive electrode material and preparation method thereof, positive electrode plate and battery
By adopting a double-layer coating structure of polycrystalline particles and single-crystal particles, combined with the adjustment of specific elements, the problem of microcrack formation in the ternary cathode material during the cycle charge and discharge process is solved, and the cycle performance and thermal stability of the material are improved. , reducing the growth of DC internal resistance.
Patent Information
- Application Number
- CN202410808364.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-01
AI Technical Summary
During the cycle charge and discharge process of the ternary cathode material, due to the presence of oxygen precipitation and heterogeneous phases, thermal stress accumulates and micro-cracks are formed, which in turn affects its cycle performance, especially when the molar ratio of nickel element is high.
It adopts a combined structure of polycrystalline particles and single crystal particles. The polycrystalline particles include an inner core and a double-layer cladding layer. The inner core contains Li1.1Ni0.9Co0.05Mn0.03Al0.001Nb0.002Sr0.001O. 2. The first coating layer contains Co, and the second coating layer contains B and Al, which are formed through sintering. The single crystal particles also adopt a double-layer coating structure, combining lithium, aluminum, niobium, magnesium, and strontium elements to adjust the structure and Ion channels improve the stability and cycling performance of materials.
It effectively inhibits the formation and expansion of micro-cracks, improves the diffusion capacity of lithium ions, enhances the cycle performance and thermal stability of the material, and reduces the growth of DC internal resistance.
Smart Images

Figure CN118738331A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a ternary positive electrode material and a preparation method thereof, a positive electrode sheet and a battery. Background Art
[0002] Lithium-ion batteries are currently the most widely used electrochemical power source. Since the positive electrode material has a crucial influence on the performance of lithium-ion batteries, many researchers are committed to studying positive electrode materials with high capacity and long cycle life.
[0003] Although increasing the molar ratio of nickel in non-lithium metal elements in ternary cathode materials can improve the specific capacity of lithium-ion batteries to a certain extent, during the cyclic charge and discharge process, due to oxygen precipitation and the existence of heterogeneous phases, the internal thermal stress of the ternary cathode material gradually accumulates, which easily promotes the formation of microcracks. At the same time, with the increase in the number of charge and discharge cycles under the conditions, the lattice of the material changes, and the generation and expansion of microcracks are accelerated along with the expansion of the volume. The microcracks will expand along the reaction area between the material and the electrolyte, and accelerate the pulverization of active particles and the decomposition of electrolyte materials, deteriorating the cycle performance of the ternary cathode material. This trend is particularly obvious when the molar ratio of nickel is ≥90%. Summary of the invention
[0004] Based on this, it is necessary to provide a ternary positive electrode material and a preparation method thereof, a positive electrode plate and a battery to improve the cycle performance of the ternary positive electrode material.
[0005] In a first aspect of the present application, a ternary positive electrode material is provided, comprising a polycrystalline particle, wherein the polycrystalline particle comprises a core C1, a first coating layer D1 covering at least a portion of the surface of the core C1, and a second coating layer E1 covering at least a portion of the surface of the first coating layer D1, wherein the core C1 comprises a chemical formula of Li i1 Ni a1 Co b1 Mn c1 Al d1 Nb e1 Mg f1 Sr g1 O2 material, wherein 1≤i1≤1.1, 0.9≤a1<1, 0.01≤b1≤0.06, 0.01≤c1≤0.04, 0<d1≤0.003, 0<e1≤0.003, 0<f1≤0.003, 0<g1≤0.003, a1+b1+c1+d1+e1+f1+g1=1, the first coating layer D1 contains Co element, and the second coating layer E1 contains B element and Al element.
[0006] In some embodiments, the first coating layer D1 includes LiCoO2, and the second coating layer E1 includes Li2O—LiBO2 and Li2O—LiAlO2—LiBO2.
[0007] In some embodiments, the mass content of the Co element in the first coating layer D1 in the polycrystalline particles is 10000 ppm to 30000 ppm.
[0008] In some embodiments, the mass content of the B element in the second coating layer E1 in the polycrystalline particles is 500 ppm to 2000 ppm.
[0009] In some embodiments, the molar ratio of the Co element in the first coating layer D1 to the B element in the second coating layer E1 is 5:1 to 30:1.
[0010] In some embodiments, a molar ratio of the B element in the second coating layer E1 to the Al element in the second coating layer E1 is 1:4 to 4:1.
[0011] In some embodiments, the primary particles of the polycrystalline particles are arranged radially along the center of the core C1.
[0012] In some embodiments, the polycrystalline particles have a particle size distribution with a span >1.
[0013] In some embodiments, the volume average particle size Dv50 of the polycrystalline particles is 8 μm to 20 μm.
[0014] In some embodiments, the powder compaction density of the ternary cathode material at 258 MPa is ≥ 3.65 g / cm 3 .
[0015] In some embodiments, the ternary cathode material further comprises a single crystal particle, wherein the single crystal particle comprises a core C2, a first coating layer D2 covering at least a portion of the surface of the core C2, and a second coating layer E2 covering at least a portion of the surface of the first coating layer D2, wherein the core C2 comprises a chemical formula of Li i2 Ni a2 Co b2 Mn c2 Al d2 Nb e2 Mg f2 Sr g2O2 material, wherein 1≤i2≤1.1, 0.9≤a2<1, 0.01≤b2≤0.06, 0.01≤c2≤0.04, 0<d2≤0.003, 0<e2≤0.003, 0<f2≤0.003, 0<g2≤0.003, a2+b2+c2+d2+e2+f2+g2=1, the first coating layer D2 contains Co element, and the second coating layer E2 contains B element and Al element.
[0016] In some embodiments, the first coating layer D2 comprises LiCoO2, and the second coating layer E2 comprises Li2O-LiBO2 and Li6Al2B4O 12 .
[0017] In some embodiments, the mass content of the Co element in the first coating layer D2 in the single crystal particle is 10000ppm~30000ppm.
[0018] In some embodiments, the mass content of the B element in the second coating layer E2 in the single crystal particle is 500ppm-2000ppm.
[0019] In some embodiments, the molar ratio of the Co element in the first coating layer D2 to the B element in the second coating layer E2 is 5:1 to 30:1.
[0020] In some embodiments, the molar ratio of the B element in the second coating layer E2 to the Al element in the second coating layer E2 is 1:4 to 4:1.
[0021] In some embodiments, the span of the particle size distribution of the single crystal particles is >1.
[0022] In some embodiments, the volume average particle size Dv50 of the single crystal particles is 1 μm to 5 μm.
[0023] In some embodiments, the mass ratio of the single crystal particles to the polycrystalline particles is 1:9 to 4:6.
[0024] In a second aspect of the present application, a method for preparing a ternary positive electrode material is provided, the preparation method comprising the steps of preparing polycrystalline particles;
[0025] The step of preparing polycrystalline particles comprises:
[0026] The polycrystalline particle precursor, the first lithium source, the first aluminum source, the first niobium source, the first magnesium source and the first strontium source are mixed, and subjected to a first sintering treatment to obtain a core C1 of the polycrystalline particle;
[0027] The core C1 and the first cobalt source are mixed, and subjected to a second sintering treatment to form a first coating layer D1 on at least a portion of the surface of the core C1, thereby obtaining a first intermediate;
[0028] The first intermediate, the first boron source and the second aluminum source are mixed, and subjected to a third sintering process to form a second coating layer E1 on at least a portion of the surface of the first coating layer D1, thereby obtaining the polycrystalline particles;
[0029] The core C1 comprises a chemical formula of Li i1 Ni a1 Co b1 Mn c1 Al d1 Nb e1 Mg f1 Sr g1 O2 material, wherein 1≤i1≤1.1, 0.9≤a1<1, 0.01≤b1≤0.06, 0.01≤c1≤0.04, 0<d1≤0.003, 0<e1≤0.003, 0<f1≤0.003, 0<g1≤0.003, a1+b1+c1+d1+e1+f1+g1=1, the first coating layer D1 contains Co element, and the second coating layer E1 contains B element and Al element.
[0030] In some embodiments, the preparation method further comprises the step of preparing single crystal particles;
[0031] The step of preparing single crystal particles comprises:
[0032] The single crystal particle precursor, the second lithium source, the third aluminum source, the second niobium source, the second magnesium source and the second strontium source are mixed, and subjected to a fourth sintering treatment to obtain a core C2 of the single crystal particle;
[0033] The core C2 and the second cobalt source are mixed and subjected to a fifth sintering process to form a first coating layer D2 on at least a portion of the surface of the core C2 to obtain a second intermediate;
[0034] The second intermediate, the second boron source and the fourth aluminum source are mixed, and subjected to a sixth sintering process to form a second coating layer E2 on at least a portion of the surface of the first coating layer D2, thereby obtaining the single crystal particle;
[0035] The core C2 contains a chemical formula of Li i2 Ni a2 Co b2 Mn c2 Al d2 Nb e2 Mg f2 Sr g2O2 material, wherein 1≤i2≤1.1, 0.9≤a2<1, 0.01≤b2≤0.06, 0.01≤c2≤0.04, 0<d2≤0.003, 0<e2≤0.003, 0<f2≤0.003, 0<g2≤0.003, a2+b2+c2+d2+e2+f2+g2=1, the first coating layer D2 contains Co element, and the second coating layer E2 contains B element and Al element.
[0036] In some embodiments, the polycrystalline particle precursor comprises a chemical formula of Ni x1 Co y1 Mn z1 (OH)2 material, wherein 0.9≤x1<1, 0.01≤y1≤0.06, 0.01≤z1≤0.04, x1+y1+z1=1.
[0037] In some embodiments, the single crystal particle precursor comprises a chemical formula of Ni x2 Co y2 Mn z2 (OH)2 material, wherein 0.9≤x2<1, 0.01≤y2≤0.06, 0.01≤z2≤0.04, x2+y2+z2=1.
[0038] In some embodiments, the first lithium source and the second lithium source each independently include one or more of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxide, lithium oxalate, and lithium peroxide.
[0039] In some embodiments, the first aluminum source, the second aluminum source, the third aluminum source, and the fourth aluminum source each independently include an inorganic compound containing the aluminum element, and the inorganic compound containing the aluminum element includes one or more of aluminum oxide, aluminum sulfate, aluminum nitrate, aluminum silicate, and aluminum sulfide.
[0040] In some embodiments, the first niobium source and the second niobium source each independently include one or more of niobium oxide, niobium oxalate, niobium nitrate, and niobium acetate.
[0041] In some embodiments, the first magnesium source and the second magnesium source each independently include an inorganic compound containing the magnesium element, and the inorganic compound containing the magnesium element includes one or more of magnesium sulfate and magnesium nitrate.
[0042] In some embodiments, the first strontium source and the second strontium source each independently include an inorganic compound containing strontium element, and the inorganic compound containing strontium element includes one or more of strontium carbonate, strontium sulfate and strontium nitrate.
[0043] In some embodiments, the first cobalt source and the second cobalt source each independently include one or more of cobalt oxyhydroxide, cobalt hydroxide, cobalt oxide, and cobalt fluoride.
[0044] In some embodiments, the first boron source and the second boron source each independently include one or more of boron oxide, boric acid, and borate.
[0045] In some embodiments, the first sintering process, the second sintering process, the third sintering process, the fourth sintering process, the fifth sintering process, and the sixth sintering process are each independently performed in an oxygen-containing atmosphere.
[0046] In some embodiments, the process conditions of the first sintering treatment and the fourth sintering treatment independently include: a sintering temperature of 750° C. to 920° C., and a sintering time of 13 h to 17 h.
[0047] In some embodiments, the process conditions of the second sintering treatment and the fifth sintering treatment independently include: a sintering temperature of 620° C. to 690° C., and a sintering time of 5 h to 8 h.
[0048] In some embodiments, the process conditions of the third sintering treatment and the sixth sintering treatment independently include: a sintering temperature of 260° C. to 320° C., and a sintering time of 6 h to 10 h.
[0049] The third aspect of the present application provides a positive electrode plate, comprising at least one of the ternary positive electrode material described in the first aspect of the present application and the ternary positive electrode material prepared by the preparation method described in the second aspect of the present application.
[0050] The fourth aspect of the present application provides a battery, comprising the positive electrode sheet described in the third aspect of the present application.
[0051] The fifth aspect of the present application provides an electrical device, comprising the battery described in the fourth aspect of the present application.
[0052] Compared with the traditional technology, the above-mentioned ternary positive electrode material and its preparation method, positive electrode sheet and battery have at least the following advantages:
[0053] The aluminum element in the core C1 of the above-mentioned ternary positive electrode material can refine the grains, strengthen the radial arrangement of primary particles, and effectively inhibit the formation and expansion of microcracks in polycrystalline particles. The niobium element can adjust the textured microstructure of the core C1 to stabilize the lattice structure, refine the grains, reduce stress accumulation, and limit the generation of microcracks. The magnesium element can expand the interlayer spacing of the core C1 material and reduce the degree of disorder inside the core C1 material. At the same time, it can effectively reduce the risk of material structure collapse and further limit the generation of microcracks. The strontium element has a larger ion radius, which can effectively expand the lithium ion channel, improve the diffusion capacity of lithium ions, and increase the ion migration rate.
[0054] The first coating layer D1 and the second coating layer E1 of the above-mentioned ternary positive electrode material can improve the interface stability, reduce the electrolyte erosion of the core C1, and reduce the side reactions of the core C1. The Co element, B element and Al element therein can maintain the relative stability of the crystal structure during the charging and discharging process, inhibit the lattice distortion of the material and the migration of metal ions, and reduce the irreversible transformation in the crystal structure; therefore, the coordinated use of the above-mentioned core C1, the first coating layer D1 and the second coating layer E1 can synergistically improve the cycle performance of the ternary positive electrode material while reducing the DCR (direct current internal resistance) growth. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is the SEM image of the ternary positive electrode material prepared in Example 1 of the present application.
[0056] Figure 2 This is a SEM image of the cross section of the polycrystalline particles prepared in Example 1 of the present application.
[0057] Figure 3 This is a powder compaction density diagram of the ternary positive electrode material prepared in Example 1 of the present application.
[0058] Figure 4 This is a comparison chart of the room temperature cycle capacity retention rate of the batteries prepared in Example 1 of the present application and Comparative Example 1. DETAILED DESCRIPTION
[0059] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0060] In this application, "first aspect", "second aspect", "third aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0061] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0062] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0063] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0064] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by technicians in the technical field of this application. The terms used in this application and in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more related listed items. The term "multiple" in this application means at least two, such as two, three, etc., unless otherwise clearly and specifically limited.
[0065] In one embodiment of the present application, a ternary positive electrode material is provided, including a polycrystalline particle, wherein the polycrystalline particle includes a core C1, a first coating layer D1 covering at least a portion of the surface of the core C1, and a second coating layer E1 covering at least a portion of the surface of the first coating layer D1, wherein the core C1 includes a chemical formula of Li i1 Ni a1 Co b1 Mn c1 Al d1 Nb e1 Mg f1 Sr g1O2 material, wherein 1≤i1≤1.1, 0.9≤a1<1, 0.01≤b1≤0.06, 0.01≤c1≤0.04, 0<d1≤0.003, 0<e1≤0.003, 0<f1≤0.003, 0<g1≤0.003, a1+b1+c1+d1+e1+f1+g1=1, the first coating layer D1 contains Co element, and the second coating layer E1 contains B element and Al element.
[0066] In the above-mentioned embodiment, the aluminum element in the core C1 can refine the grains, strengthen the radial arrangement of the primary particles, and effectively inhibit the formation and expansion of microcracks in the polycrystalline particles. The niobium element can adjust the textured microstructure of the core C1 to stabilize the lattice structure, refine the grains, reduce stress accumulation, and limit the generation of microcracks. The magnesium element can expand the interlayer spacing of the material of the core C1, reduce the degree of disorder inside the material of the core C1, and effectively reduce the risk of material structure collapse, which can further limit the generation of microcracks. The strontium element has a larger ion radius, which can effectively expand the lithium ion channel and increase the lithium ion diffusion capacity and increase the ion migration rate; the first coating layer D1 and the second coating layer E1 can improve the interface stability, reduce the electrolyte erosion of the core C1, and reduce the side reactions of the core C1. The Co element, B element and Al element therein can maintain the relative stability of the crystal structure during the charge and discharge process, inhibit the lattice distortion of the material and the migration of metal ions, and reduce the irreversible transformation in the crystal structure; therefore, the combined use of the above-mentioned core C1, the first coating layer D1 and the second coating layer E1 can synergistically improve the cycle performance of the ternary positive electrode material and reduce the growth of DCR (direct current internal resistance).
[0067] It can be understood that i1 includes but is not limited to: 1, 1.02, 1.04, 1.06, 1.08, 1.1; a1 includes but is not limited to: 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99; b1 includes but is not limited to: 0.01, 0.02, 0.03, 0.04, 0.05, 0.06; c1 includes but is not limited to: 0.01, 0.015, 0.02, 0.025, 03, 0 .035, 0.04; d1 includes but is not limited to: 0.001, 0.0015, 0.002, 0.0025, 0.003; e1 includes but is not limited to: 0.001, 0.0015, 0.002, 0.0025, 0.003; f1 includes but is not limited to: 0.001, 0.0015, 0.002, 0.0025, 0.003; g1 includes but is not limited to: 0.001, 0.0015, 0.002, 0.0025, 0.003.
[0068] In some embodiments, the first coating layer D1 includes LiCoO2, and the second coating layer E1 includes Li2O-LiBO2 and Li2O-LiAlO2-LiBO2. Thus, the thermal stability and cycle performance of the ternary cathode material can be further improved, while further reducing the DCR growth.
[0069] In some embodiments, the mass content of the Co element in the first coating layer D1 in the polycrystalline particles is 10000ppm~30000ppm. Thus, the cycle performance of the ternary positive electrode material can be further improved, while further reducing the DCR growth. It is understood that the above mass content includes but is not limited to: 10000ppm, 12000ppm, 14000ppm, 16000ppm, 18000ppm, 20000ppm, 23000ppm, 25000ppm, 27000ppm, 30000ppm.
[0070] In some embodiments, the mass content of the B element in the second coating layer E1 in the polycrystalline particles is 500ppm~2000ppm. Thus, the cycle performance of the ternary positive electrode material can be further improved, while further reducing the DCR growth. It is understood that the above mass content includes but is not limited to: 500ppm, 700ppm, 900ppm, 1000ppm, 1200ppm, 1400ppm, 1600ppm, 1800ppm, 2000ppm.
[0071] In some embodiments, the molar ratio of the Co element in the first coating layer D1 to the B element in the second coating layer E1 is 5:1 to 30:1. Thus, the cycle performance of the ternary positive electrode material can be further improved, while further reducing the DCR growth. It is understood that the above molar ratio includes but is not limited to: 5:1, 10:1, 15:1, 20:1, 25:1, 30:1. Further, the molar ratio of the Co element in the first coating layer D1 to the B element in the second coating layer E1 is 5:1 to 20:1.
[0072] In some embodiments, the molar ratio of the B element in the second coating layer E1 to the Al element in the second coating layer E1 is 1:4 to 4:1. Thus, the cycle performance of the ternary positive electrode material can be further improved, while further reducing the DCR growth. It is understood that the above molar ratio includes but is not limited to: 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1. Further, the molar ratio of the B element in the second coating layer E1 to the Al element in the second coating layer E1 is 1:4 to 1:1.
[0073] In some embodiments, the primary particles of the polycrystalline particles are arranged radially along the center of the core C1, thereby relieving the stress inside the polycrystalline particles during the charge-discharge cycle, thereby further improving the cycle performance of the ternary positive electrode material.
[0074] In some embodiments, the span of the particle size distribution of the polycrystalline particles is greater than 1. Such a design is conducive to improving the compaction density of the powder of the ternary positive electrode material and the compaction density of the positive electrode sheet containing the ternary positive electrode material. It is understood that the span of the particle size distribution of the polycrystalline particles includes but is not limited to: 1.01, 1.03, 1.05, 1.08, 1.1, 1.13, 1.15, 1.18, 1.2, 1.3, 1.4.
[0075] In this application, the span of the particle size distribution can be calculated by (Dv90-Dv10) / Dv50. In the volume cumulative distribution curve, the particle sizes corresponding to the cumulative particle size distribution numbers of the particles reaching 10%, 50%, and 90% are Dv10, Dv50, and Dv90, respectively.
[0076] In some embodiments, the volume average particle size Dv50 of the polycrystalline particles is 8 μm to 20 μm. Thus, the powder compaction density of the ternary positive electrode material and the compaction density of the positive electrode sheet can be further improved. It is understood that the above Dv50 includes but is not limited to: 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm.
[0077] In some embodiments, the specific surface area of the polycrystalline particles is 0.5 m 2 / g~1m 2 / g.
[0078] In some embodiments, the powder compaction density of the ternary cathode material at 258 MPa is ≥ 3.65 g / cm 3 .
[0079] In some embodiments, the ternary cathode material further comprises a single crystal particle, the single crystal particle comprising a core C2, a first coating layer D2 covering at least a portion of the surface of the core C2, and a second coating layer E2 covering at least a portion of the surface of the first coating layer D2, the core C2 comprising a chemical formula of Li i2 Ni a2 Co b2 Mn c2 Al d2 Nb e2 Mg f2 Sr g2O2 materials, wherein 1≤i2≤1.1, 0.9≤a2<1, 0.01≤b2≤0.06, 0.01≤c2≤0.04, 0<d2≤0.003, 0<e2≤0.003, 0<f2≤0.003, 0<g2≤0.003, a2+b2+c2+d2+e2+f2+g2=1, the first coating layer D2 contains Co element, and the second coating layer E2 contains B element and Al element. The use of single crystal particles with polycrystalline particles can reduce the risk of polycrystalline particles breaking during the rolling of the pole piece and the charging and discharging process, thereby further improving the compaction density of the positive pole piece and the cycle performance of the ternary positive electrode material.
[0080] It can be understood that i2 includes but is not limited to: 1, 1.02, 1.04, 1.06, 1.08, 1.1; a2 includes but is not limited to: 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99; b2 includes but is not limited to: 0.01, 0.02, 0.03, 0.04, 0.05, 0.06; c2 includes but is not limited to: 0.01, 0.015, 0.02, 0.025, 03, 0 .035, 0.04; d2 includes but is not limited to: 0.001, 0.0015, 0.002, 0.0025, 0.003; e2 includes but is not limited to: 0.001, 0.0015, 0.002, 0.0025, 0.003; f2 includes but is not limited to: 0.001, 0.0015, 0.002, 0.0025, 0.003; g2 includes but is not limited to: 0.001, 0.0015, 0.002, 0.0025, 0.003.
[0081] In some embodiments, the first coating layer D2 comprises LiCoO2, and the second coating layer E2 comprises Li2O-LiBO2 and Li2O-LiAlO2-LiBO2. Thus, the thermal stability and cycle performance of the ternary cathode material can be further improved, while further reducing the DCR growth.
[0082] In some embodiments, the mass content of the Co element in the first coating layer D2 in the single crystal particles is 10000ppm~30000ppm. Thus, the cycle performance of the ternary positive electrode material can be further improved, while further reducing the DCR growth. It is understood that the above mass content includes but is not limited to: 10000ppm, 12000ppm, 14000ppm, 16000ppm, 18000ppm, 20000ppm, 23000ppm, 25000ppm, 27000ppm, 30000ppm.
[0083] In some embodiments, the mass content of the B element in the second coating layer E2 in the single crystal particles is 500ppm~2000ppm. Thus, the cycle performance of the ternary positive electrode material can be further improved, while further reducing the DCR growth. It is understood that the above mass content includes but is not limited to: 500ppm, 700ppm, 900ppm, 1000ppm, 1200ppm, 1400ppm, 1600ppm, 1800ppm, 2000ppm.
[0084] In some embodiments, the molar ratio of the Co element in the first coating layer D2 to the B element in the second coating layer E2 is 5: 1 to 30: 1. Thus, the cycle performance of the ternary positive electrode material can be further improved, while further reducing the DCR growth.
[0085] In some embodiments, the molar ratio of the B element in the second coating layer E2 to the Al element in the second coating layer E2 is 1:4 to 4:1. Thus, the cycle performance of the ternary positive electrode material can be further improved, while further reducing the DCR growth.
[0086] In some embodiments, the span of the particle size distribution of the single crystal particles is greater than 1. With such a design, the single crystal particles can play a buffering role when the positive electrode sheet is rolled, which is conducive to further improving the compaction density of the positive electrode sheet. It is understood that the span of the particle size distribution of the single crystal particles includes but is not limited to: 1.01, 1.03, 1.05, 1.08, 1.1, 1.13, 1.15, 1.18, 1.2, 1.3, 1.4.
[0087] In some embodiments, the volume average particle size Dv50 of the single crystal particles is 1 μm to 5 μm. With such a design, the single crystal particles can play a buffering role when the positive electrode sheet is rolled, reducing the proportion of polycrystalline particles cracking, thereby further improving the cycle performance of the ternary positive electrode material. It is understood that the above Dv50 includes but is not limited to: 1 μm, 2 μm, 3 μm, 4 μm, 5 μm.
[0088] In some embodiments, the single crystal particle has a specific surface area of 1 m 2 / g~2m 2 / g.
[0089] In some embodiments, the mass ratio of single crystal particles to polycrystalline particles is 1:9 to 4:6. With such a design, single crystal particles can have a good buffering effect on polycrystalline particles, which is conducive to further improving the cycle performance.
[0090] Another embodiment of the present application provides a method for preparing a ternary positive electrode material, the preparation method comprising the steps of preparing polycrystalline particles;
[0091] The steps of preparing polycrystalline particles include:
[0092] The polycrystalline particle precursor, the first lithium source, the first aluminum source, the first niobium source, the first magnesium source and the first strontium source are mixed, and subjected to a first sintering treatment to obtain a core C1 of the polycrystalline particle;
[0093] The core C1 and the first cobalt source are mixed, and subjected to a second sintering treatment to form a first coating layer D1 on at least a portion of the surface of the core C1 to obtain a first intermediate;
[0094] The first intermediate, the first boron source and the second aluminum source are mixed, and subjected to a third sintering process to form a second coating layer E1 on at least a portion of the surface of the first coating layer D1 to obtain polycrystalline particles;
[0095] The core C1 contains the chemical formula Li i1 Ni a1 Co b1 Mn c1 Al d1 Nb e1 Mg f1 Sr g1 O2 material, wherein 1≤i1≤1.1, 0.9≤a1<1, 0.01≤b1≤0.06, 0.01≤c1≤0.04, 0<d1≤0.003, 0<e1≤0.003, 0<f1≤0.003, 0<g1≤0.003, a1+b1+c1+d1+e1+f1+g1=1, the first coating layer D1 contains Co element, and the second coating layer E1 contains B element and Al element.
[0096] The above preparation method is relatively simple and is conducive to the mass production of ternary positive electrode materials. In addition, the use of the core C1, the first coating layer D1 and the second coating layer E1 can synergistically improve the cycle performance of the ternary positive electrode material and reduce the DCR (direct current internal resistance) growth.
[0097] In some embodiments, the method for preparing the ternary cathode material further comprises the step of preparing single crystal particles;
[0098] The steps of preparing single crystal particles include:
[0099] The single crystal particle precursor, the second lithium source, the third aluminum source, the second niobium source, the second magnesium source and the second strontium source are mixed, and subjected to a fourth sintering treatment to obtain a core C2 of the single crystal particle;
[0100] The core C2 and the second cobalt source are mixed and subjected to a fifth sintering process to form a first coating layer D2 on at least a portion of the surface of the core C2 to obtain a second intermediate;
[0101] The second intermediate, the second boron source and the fourth aluminum source are mixed, and subjected to a sixth sintering process to form a second coating layer E2 on at least a portion of the surface of the first coating layer D2, thereby obtaining a single crystal particle;
[0102] The core C2 contains the chemical formula Li i2 Ni a2 Co b2 Mn c2 Al d2 Nb e2 Mg f2 Sr g2 O2 material, wherein 1≤i2≤1.1, 0.9≤a2<1, 0.01≤b2≤0.06, 0.01≤c2≤0.04, 0<d2≤0.003, 0<e2≤0.003, 0<f2≤0.003, 0<g2≤0.003, a2+b2+c2+d2+e2+f2+g2=1, the first coating layer D2 contains Co element, and the second coating layer E2 contains B element and Al element.
[0103] The use of the above-mentioned single crystal particles in combination with the above-mentioned polycrystalline particles can reduce the risk of polycrystalline particles breaking during electrode sheet rolling and charging and discharging, thereby further improving the compaction density of the positive electrode sheet and the cycle performance of the ternary positive electrode material.
[0104] In some embodiments, the polycrystalline particle precursor comprises a Ni x1 Co y1 Mn z1 (OH)2 material, wherein 0.9≤x1<1, 0.01≤y1≤0.06, 0.01≤z1≤0.04, x1+y1+z1=1. It is understood that x1 includes but is not limited to: 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99; y1 includes but is not limited to: 0.01, 0.02, 0.03, 0.04, 0.05, 0.06; z1 includes but is not limited to: 0.01, 0.015, 0.02, 0.025, 0.03, 0.035, 0.04.
[0105] In some embodiments, the single crystal particle precursor comprises a Ni x2 Co y2 Mn z2(OH)2 materials, wherein 0.9≤x2<1, 0.01≤y2≤0.06, 0.01≤z2≤0.04, x2+y2+z2=1. x2 includes but is not limited to: 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99; y1 includes but is not limited to: 0.01, 0.02, 0.03, 0.04, 0.05, 0.06; z1 includes but is not limited to: 0.01, 0.015, 0.02, 0.025, 0.03, 0.035, 0.04.
[0106] In some embodiments, the first lithium source and the second lithium source each independently include one or more of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxide, lithium oxalate, and lithium peroxide.
[0107] In some embodiments, the first aluminum source, the second aluminum source, the third aluminum source, and the fourth aluminum source each independently include an inorganic compound containing the aluminum element, and the inorganic compound containing the aluminum element includes one or more of aluminum oxide, aluminum sulfate, aluminum nitrate, aluminum silicate, and aluminum sulfide.
[0108] In some embodiments, the first niobium source and the second niobium source each independently include one or more of niobium oxide, niobium oxalate, niobium nitrate, and niobium acetate.
[0109] In some embodiments, the first magnesium source and the second magnesium source each independently include an inorganic compound containing the magnesium element, and the inorganic compound containing the magnesium element includes one or more of magnesium sulfate and magnesium nitrate.
[0110] In some embodiments, the first strontium source and the second strontium source each independently include an inorganic compound containing strontium element, and the inorganic compound containing strontium element includes one or more of strontium carbonate, strontium sulfate, and strontium nitrate.
[0111] In some embodiments, the first cobalt source and the second cobalt source each independently include one or more of cobalt oxyhydroxide, cobalt hydroxide, cobalt oxide, and cobalt fluoride.
[0112] In some embodiments, the first boron source and the second boron source each independently include one or more of boron oxide, boric acid, and a borate salt.
[0113] In some embodiments, the first sintering process, the second sintering process, the third sintering process, the fourth sintering process, the fifth sintering process, and the sixth sintering process are each independently performed in an oxygen-containing atmosphere.
[0114] In some embodiments, the process conditions of the first sintering treatment and the fourth sintering treatment independently include: a sintering temperature of 750°C to 920°C, and a sintering time of 13h to 17h. It is understood that the sintering temperatures of the first sintering treatment and the fourth sintering treatment independently include but are not limited to: 750°C, 770°C, 800°C, 820°C, 850°C, 870°C, 900°C, 920°C, and the sintering times of the first sintering treatment and the fourth sintering treatment include but are not limited to: 13h, 14h, 15h, 16h, 17h.
[0115] In some embodiments, the process conditions of the second sintering treatment and the fifth sintering treatment independently include: a sintering temperature of 620°C to 690°C, and a sintering time of 5h to 8h. The sintering temperatures of the second sintering treatment and the fifth sintering treatment independently include, but are not limited to, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, and 690°C, and the sintering times of the second sintering treatment and the fifth sintering treatment independently include, but are not limited to, 5h, 6h, 7h, and 8h.
[0116] In some embodiments, the process conditions of the third sintering treatment and the sixth sintering treatment independently include: a sintering temperature of 260°C to 320°C, and a sintering time of 6h to 10h. The sintering temperatures of the third sintering treatment and the sixth sintering treatment independently include, but are not limited to, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, and 320°C, and the sintering times of the third sintering treatment and the sixth sintering treatment independently include, but are not limited to, 6h, 7h, 8h, 9h, and 10h.
[0117] By adjusting the process parameters or process conditions in the above-mentioned preparation method, the ternary positive electrode material provided in one embodiment of the present application can be obtained.
[0118] Another embodiment of the present application provides a positive electrode plate, comprising at least one of the above-mentioned ternary positive electrode material of the present application and the ternary positive electrode material prepared by the above-mentioned preparation method of the present application.
[0119] The positive electrode sheet may include a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material, a conductive agent, and a binder. The positive electrode active material includes at least one of the ternary positive electrode materials described above in the present application or the ternary positive electrode materials prepared by the preparation method described above in the present application, and the conductive agent and the binder may be conductive agents and binders commonly used in the technical field.
[0120] Furthermore, another embodiment of the present application also provides a battery, including the above-mentioned positive electrode plate of the present application.
[0121] The above-mentioned battery may, for example, include the above-mentioned positive electrode sheet, negative electrode sheet, electrolyte and diaphragm of the present application. The diaphragm is arranged between the positive electrode sheet and the negative electrode sheet, and mainly plays the role of preventing the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte plays the role of conducting active ions between the positive electrode sheet and the negative electrode sheet. During the battery charging and discharging process, the active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The present application has no special restrictions on the negative electrode sheet, electrolyte and diaphragm, and the negative electrode sheet, electrolyte and diaphragm prepared by the preparation method commonly used in the technical field, or the negative electrode sheet, electrolyte and diaphragm commonly used in the art can be used. Optionally, the above-mentioned battery includes a lithium-ion battery.
[0122] Furthermore, another embodiment of the present application also provides an electrical device, including the above-mentioned battery of the present application.
[0123] The above-mentioned electrical devices may include any equipment or devices that use batteries as driving sources, such as mobile phones, laptop computers, electric vehicles, ships, satellites, energy storage devices, smart home appliances, etc., but are not limited thereto.
[0124] In order to further illustrate the present application, the technical scheme of the present application is described in detail below in conjunction with specific examples. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in the field or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0125] Example 1
[0126] The preparation method of the ternary positive electrode material is as follows:
[0127] (1) Preparation of polycrystalline particles
[0128] (1.1) The polycrystalline particle precursor (Ni 0.92 Co 0.05 Mn 0.03 (OH)2) and lithium source (LiOH) are mixed in a molar ratio of Li / Me=1.05, and then 0.05% of aluminum source Al2O3, 0.2% of niobium source Nb2O5, 0.1% of magnesium source MgSO4 and 0.1% of strontium source SrCO3 are added in a mass ratio of the polycrystalline particle precursor, and dry mixed in a mixer, and mixed thoroughly to obtain a mixed material;
[0129] (1.2) The mixed material is transferred to an atmosphere furnace, sintered in an oxygen atmosphere, calcined at 800°C for 15 hours, cooled in the furnace, and the obtained material is crushed and sieved in turn to obtain a core C1 of a polycrystalline particle, which contains a chemical formula of Li 1.05 Ni 0.9155 Co 0.05 Mn0.03 Al 0.0005 Nb 0.002 Sr 0.001 Mg 0.001 O2 materials;
[0130] (1.3) the core C1 is fully mixed with 1.5% by mass of a cobalt source CoOOH, and then sintered at 650° C. for 6 h to obtain an intermediate; the first coating layer D1 in the intermediate is coated on a portion of the surface of the core C1, and the first coating layer D1 contains LiCoO2;
[0131] (1.4) The intermediate is mixed with distilled water in a certain proportion, stirred at 180 rpm for 90 seconds, placed in a 150° C. vibration dryer for 1.5 hours, and taken out after drying. The dried intermediate is dry-mixed with 0.1% by mass of aluminum source Al2O3 and 0.1% by mass of boron source H2BO3, so that the aluminum source and the boron source are uniformly attached to the surface of the dried intermediate. After sintering at 280° C. in an oxygen atmosphere for 8 hours, the intermediate is cooled and sieved to obtain polycrystalline particles with a volume average particle size Dv50 of 15 μm, and the span of the particle size distribution of the polycrystalline particles is greater than 1;
[0132] The polycrystalline particles include a core C1, a first coating layer D1 and a second coating layer E1, the second coating layer E1 contains Li2O-LiBO2 and Li2O-LiAlO2-LiBO2, the mass content of the Co element in the first coating layer D1 in the polycrystalline particles is 15000ppm, the mass content of the B element in the second coating layer E1 in the polycrystalline particles is 1000ppm, the molar ratio of the Co element in the first coating layer D1 to the B element in the second coating layer E1 is 15:1, and the molar ratio of the B element in the second coating layer E1 to the Al element in the second coating layer E1 is 1:1.
[0133] (2) Preparation of single crystal particles
[0134] (2.1) The single crystal particle precursor (Ni 0.94 Co 0.04 Mn 0.02 (OH)2) and lithium source (LiOH) are mixed in a molar ratio of Li / Me=1.05, and then 0.1% of aluminum source Al2O3, 0.25% of niobium source Nb2O5, 0.1% of magnesium source MgSO4 and 0.05% of strontium source SrCO3 are added in a mass ratio of the single crystal particle precursor, and dry mixed in a mixer, and mixed thoroughly to obtain a mixed material;
[0135] (2.2) The mixed material is transferred to an atmosphere furnace and sintered in an oxygen atmosphere at 900°C for 15 hours. The obtained material is then cooled in the furnace and crushed to obtain a core C2 of a single crystal particle. The core C2 contains a chemical formula of Li 1.05 Ni 0.915 Co 0.05 Mn 0.03 Al 0.001 Nb 0.0025 Sr 0.0005 Mg 0.001 O2 materials;
[0136] (2.3) the core C2 is fully mixed with 2% by mass of the cobalt source CoOOH, and then sintered at 670° C. for 6 h to obtain an intermediate; the first coating layer D2 in the intermediate is coated on a portion of the surface of the core C2, and the first coating layer D2 contains LiCoO2;
[0137] (2.4) mixing the intermediate with 0.1% by mass of an aluminum source Al2O3 and 0.05% by mass of a boron source H2BO3, so that the aluminum source and the boron source are uniformly attached to the surface of the intermediate, sintering at 300°C in an oxygen atmosphere for 6 hours, cooling and sieving to obtain single crystal particles with a volume average particle size Dv50 of 4 μm, and a span of the particle size distribution of the single crystal particles greater than 1;
[0138] The single crystal particle includes a core C2, a first coating layer D2 and a second coating layer E2, the second coating layer E2 contains Li2O-LiBO2 and Li2O-LiAlO2-LiBO2, the mass content of the Co element in the first coating layer D2 in the single crystal particle is 20000ppm, the mass content of the B element in the second coating layer E2 in the single crystal particle is 1000ppm, the molar ratio of the Co element in the first coating layer D2 to the B element in the second coating layer E2 is 20:1, and the molar ratio of the B element in the second coating layer E2 to the Al element in the second coating layer E2 is 1:1.
[0139] (3) Preparation of ternary cathode materials
[0140] The polycrystalline particles and the single crystal particles are uniformly mixed in a mass ratio of 8:2 to obtain a ternary positive electrode material.
[0141] Example 2
[0142] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that: the amount of the cobalt source added in step (1.3) is changed, and in step (1.3), the core C1 is fully mixed with the cobalt source accounting for 1% of its mass ratio;
[0143] The obtained polycrystalline particles include a core C1, a first coating layer D1 and a second coating layer E1, the second coating layer E1 contains Li2O-LiBO2 and Li2O-LiAlO2-LiBO2, the mass content of the Co element in the first coating layer D1 in the polycrystalline particles is 10000ppm, the mass content of the B element in the second coating layer E1 in the polycrystalline particles is 1000ppm, the molar ratio of the Co element in the first coating layer D1 to the B element in the second coating layer E1 is 10:1, and the molar ratio of the B element in the second coating layer E1 to the Al element in the second coating layer E1 is 1:1.
[0144] Example 3
[0145] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that: the amount of the boron source added in step (1.4) is changed, and in step (1.4), the dried intermediate and 0.1% by mass of the aluminum source and 0.15% by mass of the boron source are dry mixed;
[0146] The obtained polycrystalline particles include a core C1, a first coating layer D1 and a second coating layer E1, the second coating layer E1 contains Li2O-LiBO2 and Li2O-LiAlO2-LiBO2, the mass content of the Co element in the first coating layer D1 in the polycrystalline particles is 15000ppm, the mass content of the B element in the second coating layer E1 in the polycrystalline particles is 1500ppm, the molar ratio of the Co element in the first coating layer D1 to the B element in the second coating layer E1 is 10:1, and the molar ratio of the B element in the second coating layer E1 to the Al element in the second coating layer E1 is 1.5:1.
[0147] Example 4
[0148] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that: the amount of the boron source added in step (1.4) is changed, and in step (1.4), the dried intermediate and 0.1% by mass of the aluminum source and 0.05% by mass of the boron source are dry mixed;
[0149] The obtained polycrystalline particles include a core C1, a first coating layer D1 and a second coating layer E1, the second coating layer E1 contains Li2O-LiBO2 and Li2O-LiAlO2-LiBO2, the mass content of the Co element in the first coating layer D1 in the polycrystalline particles is 15000ppm, the mass content of the B element in the second coating layer E1 in the polycrystalline particles is 500ppm, the molar ratio of the Co element in the first coating layer D1 to the B element in the second coating layer E1 is 30:1, and the molar ratio of the B element in the second coating layer E1 to the Al element in the second coating layer E1 is 1:2.
[0150] Comparative Example 1
[0151] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that: no strontium source is added in step (1.1), and the core C1 obtained in step (1.2) contains a chemical formula of Li 1.05 Ni 0.9165 Co 0.05 Mn 0.03 Al 0.0005 Nb 0.002 Mg 0.001 O2 material.
[0152] Comparative Example 2
[0153] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that: no magnesium source is added in step (1.1), and the core C1 obtained in step (1.2) contains a chemical formula of Li 1.05 Ni 0.9165 Co 0.05 Mn 0.03 Al 0.0005 Nb 0.002 Sr 0.001 O2 material.
[0154] Comparative Example 3
[0155] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that: no niobium source is added in step (1.1), and the core C1 obtained in step (1.2) contains a chemical formula of Li 1.05 Ni 0.9175 Co 0.05 Mn 0.03 Al 0.0005 Sr 0.001 Mg 0.001 O2 material.
[0156] Comparative Example 4
[0157] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that: no aluminum source is added in step (1.1), and the core C1 obtained in step (1.2) contains a chemical formula of Li 1.05 Ni 0.916 Co 0.05 Mn 0.03 Nb 0.002 Sr 0.001 Mg 0.001 O2 material.
[0158] Comparative Example 5
[0159] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that the niobium source in step (1.1) is replaced by an antimony source Sb2O3, and the core C1 obtained in step (1.2) contains a chemical formula of Li1.05 Ni 0.9155 Co 0.05 Mn 0.03 Al 0.0005 Sb 0.002 Sr 0.001 Mg 0.001 O2 material.
[0160] Comparative Example 6
[0161] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that: step (1.3) is omitted, and in step (1.4), the core C1 is mixed with distilled water in a certain proportion;
[0162] The obtained polycrystalline particles do not have the first coating layer D1, and the second coating layer E1 coats part of the surface of the core C1. The mass content of the B element in the second coating layer E1 in the polycrystalline particles is 1000ppm, and the molar ratio of the B element in the second coating layer E1 to the Al element in the second coating layer E1 is 1:1.
[0163] Comparative Example 7
[0164] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that: no boron source is added in step (1.4), and the amount of aluminum source added accounts for 0.2% of the mass ratio of the dried intermediate;
[0165] The obtained polycrystalline particle includes a core C1, a first coating layer D1 and a second coating layer E1, wherein the second coating layer E1 includes Li2O—LiAlO2.
[0166] Comparative Example 8
[0167] The preparation method of the ternary positive electrode material is basically the same as that of Example 1, except that: in step (1.4), no aluminum source is added, and the amount of the boron source added accounts for 0.2% of the mass ratio of the dried intermediate;
[0168] The obtained polycrystalline particle includes a core C1, a first coating layer D1 and a second coating layer E1, wherein the second coating layer E1 includes Li2O—LiBO2.
[0169] The components of the ternary positive electrode materials prepared in each embodiment and each comparative example were measured using an ICP-AES (inductively coupled plasma atomic emission spectrometry) tester.
[0170] The volume average particle size Dv50 and the span of the particle size distribution of the ternary positive electrode materials prepared in each embodiment and each comparative example are measured using a particle size tester.
[0171] The ternary positive electrode materials prepared in each embodiment and each comparative example were tested using a SEM (scanning electron microscope).
[0172] Test method for powder compaction density of ternary cathode materials:
[0173] Weigh 3.00050±0.00010g of the sample with weighing paper, put all the weighed samples into the sample slot, place the mold on the tablet press, turn the screw to the top of the mold and leave a little gap, tighten the nut in front, apply pressure to the required value, hold the pressure for one minute, then loosen the nut in front, release the pressure, measure the height H1 under the required pressure, record the data, place it under the tablet press again to test the next pressure, and so on. The powder compaction density of the ternary positive electrode material PD=m*10 / [(H1-H0)*S]. In the above formula, m: sample weight, g; H0: original height, mm; H1: height after pressing, mm; S: area, 1.766.cm 2 .
[0174] Electrochemical performance test
[0175] (1) Assembling the battery
[0176] The ternary positive electrode material, acetylene black and polyvinylidene fluoride were mixed in a mass ratio of 90:5:5, and an appropriate amount of N-methylpyrrolidone was added as a dispersant. The slurry was then evenly coated on aluminum foil and vacuum dried at 120°C for 12 hours. The dried positive electrode sheet was rolled with a roller machine, and the aluminum foil was cut with a slicer into circular sheets with a diameter of 1.3 cm. The loading amount of active material was controlled at 12 g / cm 2 About, and then assembled the half-cell in an argon atmosphere glove box, controlling the water partial pressure ≤0.1pm, the oxygen partial pressure ≤0.1pm, using metallic lithium as the negative electrode, 1M LiPF6 solution as the electrolyte, and the solvent being FEC, DEC and DMC in a volume ratio of 1:1:1. The assembly specification is CR2032 button cell.
[0177] (2) Cyclic performance test and DC resistance (DCR) growth test
[0178] At 25°C, the battery was charged and discharged for 100 cycles at a current density of 1.0C, and the capacity retention rate of the battery after the 100th cycle was tested with a voltage range of 2.5V~4.25V.
[0179] 100-week capacity retention rate (%) = discharge specific capacity at the 100th week / discharge specific capacity at the 1st week × 100%.
[0180] DCR= (discharge voltage - static voltage) / current*1000;
[0181] DCR growth = DCR in the 100th week / DCR in the first week * 100%.
[0182] Table 1
[0183]
[0184] Figure 1 This is the SEM image of the ternary cathode material prepared in Example 1. Figure 1 It can be seen that the ternary positive electrode material prepared in Example 1 contains polycrystalline particles and single crystal particles. Figure 2 This is a SEM image of the cross section of the polycrystalline particles prepared in Example 1. Figure 2 It can be seen that the primary particles of the polycrystalline particles prepared in Example 1 are arranged radially along the center of the inner core.
[0185] Figure 3 The powder compaction density diagram of the ternary positive electrode material prepared in Example 1 is shown in FIG. Figure 3 It can be seen from the data in Table 1 that the powder compaction density of the ternary positive electrode material of Example 1 at 258 MPa is higher than that of Comparative Example 1. In addition, the powder compaction density of the ternary positive electrode materials of Examples 1 to 4 under this condition remains higher or equivalent to that of the ternary positive electrode materials of Comparative Examples 1 to 8. Figure 4 The comparison chart of the room temperature cycle capacity retention rate of the batteries prepared in Example 1 and Comparative Example 1 is shown in FIG. Figure 4 It can be seen from the data in Table 1 that, compared with Comparative Examples 1 to 8, the 100-week capacity retention rate of the battery of Example 1 is relatively high, and the DCR growth of the battery of Example 1 is significantly smaller, indicating that the application can synergistically improve the cycle performance of the ternary positive electrode material and reduce the DCR growth through the coordinated use of the core, the first coating layer D1 and the second coating layer E1.
[0186] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0187] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.
Claims
1. A ternary positive electrode material, characterized in that: The polycrystalline particles include a core C1, a first coating layer D1 covering at least a portion of the surface of the core C1, and a second coating layer E1 covering at least a portion of the surface of the first coating layer D1. The core C1 contains a chemical formula of Li i1 Ni a1 Co b1 Mn c1 Al d1 Nb e1 Mg f1 Sr g1 O2 material, wherein 1≤i1≤1.1, 0.9≤a1<1, 0.01≤b1≤0.06, 0.01≤c1≤0.04, 0<d1≤0.003, 0<e1≤0.003, 0<f1≤0.003, 0<g1≤0.003, a1+b1+c1+d1+e1+f1+g1=1, the first coating layer D1 contains Co element, and the second coating layer E1 contains B element and Al element.
2. The ternary cathode material according to claim 1, characterized in that: The first coating layer D1 includes LiCoO2, and the second coating layer E1 includes Li2O—LiBO2 and Li2O—LiAlO2—LiBO2.
3. The ternary cathode material according to claim 1, characterized in that: The ternary positive electrode material has at least one of the following characteristics (1) to (8): (1) The mass content of the Co element in the first coating layer D1 in the polycrystalline particles is 10000ppm to 30000ppm; (2) The mass content of the B element in the second coating layer E1 in the polycrystalline particles is 500ppm to 2000ppm; (3) The molar ratio of the Co element in the first coating layer D1 to the B element in the second coating layer E1 is 5:1 to 30:1; (4) the molar ratio of the B element in the second coating layer E1 to the Al element in the second coating layer E1 is 1:4 to 4:1; (5) the primary particles of the polycrystalline particles are arranged radially along the center of the core C1; (6) The span of the particle size distribution of the polycrystalline particles is greater than 1; (7) The volume average particle size Dv50 of the polycrystalline particles is 8 μm to 20 μm; (8) The powder compaction density of the ternary positive electrode material at 258 MPa is ≥ 3.65 g / cm 3 .
4. The ternary positive electrode material according to any one of claims 1 to 3, characterized in that: The ternary positive electrode material also includes a single crystal particle, the single crystal particle includes a core C2, a first coating layer D2 covering at least a portion of the surface of the core C2, and a second coating layer E2 covering at least a portion of the surface of the first coating layer D2, the core C2 contains a chemical formula of Li i2 Ni a2 Co b2 Mn c2 Al d2 Nb e2 Mg f2 Sr g2 O2 material, wherein 1≤i2≤1.1, 0.9≤a2<1, 0.01≤b2≤0.06, 0.01≤c2≤0.04, 0<d2≤0.003, 0<e2≤0.003, 0<f2≤0.003, 0<g2≤0.003, a2+b2+c2+d2+e2+f2+g2=1, the first coating layer D2 contains Co element, and the second coating layer E2 contains B element and Al element; Optionally, the first coating layer D2 contains LiCoO2, and the second coating layer E2 contains Li2O-LiBO2 and Li2O-LiAlO2-LiBO2.
5. The ternary cathode material according to claim 4, characterized in that: The ternary positive electrode material has at least one of the following characteristics (1) to (7): (1) The mass content of the Co element in the first coating layer D2 in the single crystal particle is 10000ppm to 30000ppm; (2) The mass content of the B element in the second coating layer E2 in the single crystal particle is 500ppm to 2000ppm; (3) The molar ratio of the Co element in the first coating layer D2 to the B element in the second coating layer E2 is 5:1 to 30:1; (4) the molar ratio of the B element in the second coating layer E2 to the Al element in the second coating layer E2 is 1:4 to 4:1; (5) The span of the particle size distribution of the single crystal particles is greater than 1; (6) The volume average particle size Dv50 of the single crystal particles is 1 μm to 5 μm; (7) The mass ratio of the single crystal particles to the polycrystalline particles is 1:9 to 4:
6.
6. A method for preparing a ternary positive electrode material, characterized in that: The preparation method comprises the steps of preparing polycrystalline particles; The step of preparing polycrystalline particles comprises: The polycrystalline particle precursor, the first lithium source, the first aluminum source, the first niobium source, the first magnesium source and the first strontium source are mixed, and subjected to a first sintering treatment to obtain a core C1 of the polycrystalline particle; The core C1 and the first cobalt source are mixed, and subjected to a second sintering treatment to form a first coating layer D1 on at least a portion of the surface of the core C1, thereby obtaining a first intermediate; The first intermediate, the first boron source and the second aluminum source are mixed, and subjected to a third sintering process to form a second coating layer E1 on at least a portion of the surface of the first coating layer D1, thereby obtaining the polycrystalline particles; The core C1 comprises a chemical formula of Li i1 Ni a1 Co b1 Mn c1 Al d1 Nb e1 Mg f1 Sr g1 O2 material, wherein 1≤i1≤1.1, 0.9≤a1<1, 0.01≤b1≤0.06, 0.01≤c1≤0.04, 0<d1≤0.003, 0<e1≤0.003, 0<f1≤0.003, 0<g1≤0.003, a1+b1+c1+d1+e1+f1+g1=1, the first coating layer D1 contains Co element, and the second coating layer E1 contains B element and Al element.
7. The preparation method according to claim 6, characterized in that: The preparation method further comprises the step of preparing single crystal particles; The step of preparing single crystal particles comprises: The single crystal particle precursor, the second lithium source, the third aluminum source, the second niobium source, the second magnesium source and the second strontium source are mixed, and subjected to a fourth sintering treatment to obtain a core C2 of the single crystal particle; The core C2 and the second cobalt source are mixed and subjected to a fifth sintering process to form a first coating layer D2 on at least a portion of the surface of the core C2 to obtain a second intermediate; The second intermediate, the second boron source and the fourth aluminum source are mixed, and subjected to a sixth sintering process to form a second coating layer E2 on at least a portion of the surface of the first coating layer D2, thereby obtaining the single crystal particle; The core C2 contains a chemical formula of Li i2 Ni a2 Co b2 Mn c2 Al d2 Nb e2 Mg f2 Sr g2 O2 material, wherein 1≤i2≤1.1, 0.9≤a2<1, 0.01≤b2≤0.06, 0.01≤c2≤0.04, 0<d2≤0.003, 0<e2≤0.003, 0<f2≤0.003, 0<g2≤0.003, a2+b2+c2+d2+e2+f2+g2=1, the first coating layer D2 contains Co element, and the second coating layer E2 contains B element and Al element.
8. The preparation method according to claim 7, characterized in that: The preparation method satisfies at least one of the following conditions (1) to (13): (1) The polycrystalline particle precursor comprises a chemical formula of Ni x1 Co y1 Mn z1 (OH)2 materials, wherein 0.9≤x1<1, 0.01≤y1≤0.06, 0.01≤z1≤0.04, x1+y1+z1=1; (2) The single crystal particle precursor includes a chemical formula of Ni x2 Co y2 Mn z2 (OH)2 materials, wherein 0.9≤x2<1, 0.01≤y2≤0.06, 0.01≤z2≤0.04, x2+y2+z2=1; (3) The first lithium source and the second lithium source each independently include one or more of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxide, lithium oxalate and lithium peroxide; (4) the first aluminum source, the second aluminum source, the third aluminum source and the fourth aluminum source each independently include an inorganic compound containing aluminum, and the inorganic compound containing aluminum includes one or more of aluminum oxide, aluminum sulfate, aluminum nitrate, aluminum silicate and aluminum sulfide; (5) The first niobium source and the second niobium source each independently include one or more of niobium oxide, niobium oxalate, niobium nitrate and niobium acetate; (6) The first magnesium source and the second magnesium source each independently include an inorganic compound containing magnesium, and the inorganic compound containing magnesium includes one or more of magnesium sulfate and magnesium nitrate; (7) The first strontium source and the second strontium source each independently include an inorganic compound containing strontium, and the inorganic compound containing strontium includes one or more of strontium carbonate, strontium sulfate and strontium nitrate; (8) The first cobalt source and the second cobalt source each independently include one or more of cobalt oxyhydroxide, cobalt hydroxide, cobalt oxide and cobalt fluoride; (9) The first boron source and the second boron source each independently include one or more of boron oxide, boric acid and borate; (10) the first sintering process, the second sintering process, the third sintering process, the fourth sintering process, the fifth sintering process and the sixth sintering process are each independently performed in an oxygen-containing atmosphere; (11) The process conditions of the first sintering treatment and the fourth sintering treatment independently include: a sintering temperature of 750° C. to 920° C. and a sintering time of 13 h to 17 h; (12) The process conditions of the second sintering treatment and the fifth sintering treatment independently include: a sintering temperature of 620° C. to 690° C. and a sintering time of 5 h to 8 h; (13) The process conditions of the third sintering treatment and the sixth sintering treatment independently include: a sintering temperature of 260° C. to 320° C., and a sintering time of 6 h to 10 h.
9. A positive electrode sheet, characterized in that: It comprises at least one of the ternary positive electrode materials described in any one of claims 1 to 5 and the ternary positive electrode materials prepared by the preparation method described in any one of claims 6 to 8.
10. A battery, characterized in that: Including the positive electrode sheet as described in claim 9.